A Prussian blue cathode material for sodium-ion batteries and its preparation method
By employing a two-step progressive dehydration process combining liquid nitrogen quick-freezing and a high thermal conductivity carrier with cryogenic quick-freezing and low-temperature heat treatment, the structural damage and agglomeration problems of Prussian blue materials during the removal of crystal water were solved, resulting in the preparation of high-performance sodium-ion battery cathode materials.
Patent Information
- Application Number
- CN202611226902.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-13
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies struggle to remove the water of crystallization from Prussian blue materials while simultaneously preventing damage to the crystal framework and particle agglomeration caused by ice crystals, and ensuring excellent electrochemical performance, especially the complete removal of coordination water.
The material is subjected to cryogenic freezing using liquid nitrogen combined with a high thermal conductivity metal carrier. After deep cryogenic freezing and drying, it is heat-treated under low temperature vacuum. Through a two-step progressive dehydration process, the structural integrity and porosity of the material are ensured.
A method was developed to completely remove water of crystallization under mild conditions, avoiding damage to the framework and particle agglomeration caused by ice crystals, and producing sodium-ion battery cathode materials with high specific capacity, high initial coulombic efficiency and excellent cycle stability.
Smart Images

Figure CN123105675A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of new energy materials technology, and in particular to a method for preparing a sodium-ion battery cathode material. Background Technology
[0002] Prussian blue and its analogues (PBAs) have attracted much attention as cathode materials for sodium-ion batteries due to their three-dimensional open framework, abundant raw materials, and high theoretical capacity. However, during their conventional aqueous synthesis, a large amount of coordinated water and free water (collectively referred to as water of crystallization) is inevitably introduced into the lattice channels of the material. The presence of this water of crystallization severely degrades the electrochemical performance of the material: water molecules occupy sodium ion storage sites, reducing reversible capacity; under the battery's operating voltage, the water of crystallization reacts with the organic electrolyte, consuming the active sodium source, generating gas, and causing the battery to swell or even fail; water desorption and re-intercalation cause repeated expansion and contraction of the crystal structure, accelerating material pulverization and leading to a sharp decline in cycle life.
[0003] In existing technologies, the main methods for reducing the water of crystallization content of Prussian blue materials include high-temperature vacuum heat treatment and freeze-drying. While high-temperature heat treatment can remove adsorbed water and some interstitial water to a certain extent, the temperature usually needs to be above 150℃, which can easily lead to local collapse or phase transformation of the Prussian blue framework. Simultaneously, due to capillary forces and surface tension, irreversible hard agglomeration easily occurs between particles, forming dense masses and reducing the material's electrochemical active area and ion transport rate. Furthermore, for bound water that is strongly coordinated with metal ions, heating alone is insufficient to completely remove it before structural damage occurs.
[0004] To address the aforementioned issues, Chinese patent application CN116375054A proposes a preparation method that uses freeze-drying technology to reduce the water of crystallization content. This method involves first freezing the Prussian blue precipitate obtained after co-precipitation synthesis and filtration at -20°C for 2 hours, then transferring it to a freeze dryer cold trap under vacuum, and gradually heating it from -50°C to 50°C for drying at a rate of 10°C / h. This two-stage freeze-thaw drying process effectively reduces the water of crystallization content to a certain extent, and the resulting material exhibits good rate performance.
[0005] However, the technical solution in CN116375054A still has the following significant shortcomings: First, its freezing stage uses a regular refrigerator for slow freezing at -20℃, resulting in an extremely low freezing rate. This causes the moisture in the material to form large ice crystals during the freezing process. These large ice crystals can expand and even puncture the nanoscale three-dimensional framework structure of Prussian blue, causing irreversible crystal damage. Second, in the freeze-drying stage, it uses a process of gradually increasing the temperature from -50℃ to 50℃. During the drying process, the material temperature eventually rises above zero degrees Celsius. The ice crystals melt at the end of sublimation, and the resulting liquid water causes particle aggregation due to surface tension. Furthermore, the presence of liquid water accelerates the dissolution of metal ions in the Prussian blue framework and structural degradation. Third, it cannot guarantee the full sublimation of ice crystals inside the material. In particular, for coordinated water with strong binding forces to metal ions, this solution does not provide an effective removal method, therefore the dehydration effect still needs to be improved.
[0006] Therefore, how to efficiently remove various types of water of crystallization, including coordination water, from Prussian blue materials while avoiding damage to the crystal framework by ice crystals and preventing particle agglomeration, so as to obtain Prussian blue cathode materials with complete structure, loose and porous structure and excellent electrochemical performance, remains a technical problem that urgently needs to be solved in this field. Summary of the Invention
[0007] This invention provides a Prussian blue cathode material for sodium-ion batteries and its preparation method, thereby solving the technical problems mentioned in the background art.
[0008] To solve the above-mentioned technical problems, the technical solution proposed by this invention is as follows:
[0009] A method for preparing a Prussian blue cathode material for sodium-ion batteries includes the following steps: S1. The wet material of the synthesized and filtered sodium-ion battery Prussian blue cathode material is uniformly spread onto a carrier in a protective atmosphere; the carrier is a material with high thermal conductivity. S2. Use liquid nitrogen to perform deep cryogenic quick-freezing treatment on the carrier containing the wet material, so that the water in the wet material solidifies into microcrystalline ice. S3. The carrier and wet material after deep cryogenic quick-freezing are vacuum freeze-dried at a temperature below -60°C to obtain primary dry powder. S4. The primary dry powder is heat-treated under vacuum conditions at 120~150°C in a protective atmosphere to remove residual coordination water, thereby obtaining the Prussian blue cathode material for sodium-ion batteries.
[0010] This invention uniformly spreads wet material onto a highly thermally conductive carrier in a protective atmosphere, increasing the heat exchange area and shortening the heat conduction path to lay the foundation for subsequent rapid and uniform freezing. Furthermore, utilizing the synergistic effect of the ultra-low temperature of liquid nitrogen and the high thermal conductivity of the carrier, the moisture in the wet material bypasses the ice crystal nucleation period within seconds to tens of seconds, directly solidifying into micro-nano-sized ice crystals. Unlike existing technologies where slow freezing at -20°C leads to the expansion of large ice crystals that damage the three-dimensional framework of Prussian blue, this invention achieves instantaneous and uniform freezing of moisture, maximally inhibiting ice crystal growth and fundamentally avoiding physical damage to the crystal framework. Simultaneously, this invention freeze-dries the deep-cryogenically frozen material under high vacuum conditions below -60°C throughout the process. The solid ice in the material sublimates directly into water vapor without passing through a liquid state and is captured by the cold trap. Because the sublimation of ice crystals leaves in-situ through-channels corresponding to the ice crystal morphology within the material, the resulting primary dried powder is loose and porous. Unlike existing technologies that raise the temperature to 50°C during freeze-drying, causing ice crystals to melt, liquid water to form, and consequently particle agglomeration and skeletal degradation, this invention uses a freeze-drying process that remains below zero throughout, completely avoiding ice crystal melting and capillary forces, thus ensuring no hard agglomeration between particles.
[0011] In step S3, lyophilization removes most of the free water and some weakly bound water, but it struggles to remove the coordinated water, which has a strong affinity for metal ions. This invention further employs vacuum heat treatment at a mild temperature of 120-150°C to specifically remove the strong coordinated water remaining after lyophilization. These two steps form a complementary, progressive dehydration synergy, neither of which can be omitted, together achieving deep removal of various types of water of crystallization, including coordinated water, under mild conditions ≤150°C.
[0012] In particular, the wet material laying process in S1 and the liquid nitrogen quick-freezing process in S2 were both completed in a protective atmosphere, and the heat treatment in S4 was also carried out in a protective atmosphere, effectively preventing the Fe in Prussian blue from being released. 2+ The oxidation of low-valence metal ions is achieved, while avoiding the dried product from absorbing water again upon contact with air, thus ensuring the high purity and batch consistency of the material.
[0013] As a further preferred embodiment of the above technical solution, in S1, the thermal conductivity of the carrier is greater than 200 W / (m·K), and the thickness of the carrier is 0.05~0.2 mm. The carrier selected in this invention has excellent cold energy conduction capability, which can rapidly transfer the ultra-low temperature of liquid nitrogen to the entire thin layer of wet material. Combined with the carrier thickness of 0.05~0.2 mm, it ensures sufficient mechanical strength to support the wet material while avoiding the increase in thermal resistance caused by an excessively thick carrier.
[0014] As a further preferred embodiment of the above technical solution, the carrier is aluminum foil or copper foil.
[0015] As a further preferred embodiment of the above technical solution, in S1, the carrier is pre-cooled before the wet material is laid. Pre-cooling prevents localized warming when the carrier at room temperature comes into contact with the wet material.
[0016] As a further preferred embodiment of the above technical solution, in S1, the thickness of the wet material laid on the carrier is less than 5 mm, and more preferably 1-3 mm. The thickness design of the wet material shortens the path of heat conduction from the surface layer to the bottom layer, ensuring that the entire wet material layer can be frozen synchronously in a very short time when immersed in liquid nitrogen.
[0017] As a further preferred embodiment of the above technical solution, in S2, the deep cryogenic quick-freezing treatment time is 30s to 3min, and the entire deep cryogenic quick-freezing treatment process is completed in a protective atmosphere.
[0018] As a further preferred embodiment of the above technical solution, in S3, the drying time of the vacuum freeze-drying operation is 24~72h, and the vacuum degree is less than 0.02mbar.
[0019] As a further preferred embodiment of the above technical solution, in S3, before performing the vacuum freeze-drying operation, the freeze dryer is pre-cooled to a cold trap temperature below -60°C, more preferably below -64°C. Pre-cooling the freeze dryer to a cold trap temperature below -60°C before performing the vacuum freeze-drying operation ensures that the cryogenically frozen material will not reheat due to contact with a room-temperature sample holder during the transfer process.
[0020] As a further preferred embodiment of the above technical solution, in S4, the heat treatment time is 2~10h, and the absolute pressure of the vacuum condition is less than 100Pa.
[0021] Based on the same technical concept, the present invention also provides a Prussian blue cathode material for sodium-ion batteries, which is prepared by the above-mentioned preparation method. The Prussian blue cathode material for sodium-ion batteries is a powder with a loose porous structure and no obvious hard agglomeration between particles. The mass percentage of residual water of crystallization in the Prussian blue cathode material for sodium-ion batteries is ≤2.3%.
[0022] The present invention has the following beneficial effects: (1) The present invention uses liquid nitrogen for ultra-low temperature quick freezing and a high thermal conductivity metal carrier to spread the wet material to less than 5 mm. By increasing the heat exchange area and shortening the heat conduction path, the water in the wet material can instantly pass through the ice crystal nucleation period within a few seconds to tens of seconds and directly solidify into micro-nano-scale fine ice crystals. This suppresses ice crystal growth to the greatest extent and avoids the expansion and damage of large ice crystals to the three-dimensional skeleton of Prussian blue, thus protecting the integrity of the crystal skeleton of the material from the root.
[0023] (2) In this invention, the material after deep freezing is freeze-dried under conditions of -60°C and high vacuum throughout the process. The solid ice sublimates directly without passing through the liquid state. After the ice crystals sublimate, they leave through-holes in the material corresponding to the ice crystal morphology in situ. The resulting powder is loose and porous. The material temperature is always below zero degrees throughout the freeze-drying process, which completely avoids the adverse effects of ice crystal melting, capillary force and surface tension, and ensures that there is no hard agglomeration between particles. This morphology is conducive to the rapid wetting of electrolyte and the rapid transport of ions.
[0024] (3) In this invention, the freeze-drying step and the low-temperature heat treatment step are functionally differentiated and work together. The freeze-drying step is responsible for removing most of the free water and some of the weakly bound water, while protecting the structure and preventing agglomeration. The subsequent low-temperature vacuum heat treatment removes the strongly coordinated water that is difficult to remove by freeze-drying. The two steps form a two-step progressive dehydration, neither of which can be omitted, and together they achieve the deep removal of various types of crystal water, including coordinated water, under mild conditions of ≤150℃.
[0025] (4) The Prussian blue cathode material prepared by the method of the present invention has a complete crystal structure, a loose and porous non-agglomerated morphology and an extremely low crystal water content. After being assembled into a sodium-ion battery, it exhibits high specific capacity, high initial coulombic efficiency and excellent cycle stability, effectively solving the application bottlenecks such as side reactions, capacity decay and gas expansion caused by crystal water.
[0026] (5) The method of the present invention is not only applicable to iron-based Prussian blue systems, but also to other transition metal Prussian blue analogue systems such as manganese-based systems, and has strong versatility. All the equipment used are mature and general-purpose equipment, and the high thermal conductivity carrier can be reused or replaced at low cost. By optimizing the carrier and batch pre-freezing method, it can be transitioned to pilot-scale and even large-scale production, and has good industrialization prospects. Attached Figure Description
[0027] Figure 1 These are scanning electron microscope (SEM) images of the Prussian blue cathode materials for sodium-ion batteries in Examples 1, 1, 2, and 3 of this invention. Figure 2 The X-ray diffraction (XRD) patterns of the Prussian blue cathode material for sodium-ion batteries in Examples 1, 1, 2, and 3 of this invention are shown. Figure 3 Thermogravimetric analysis (TG) diagrams of Prussian blue cathode materials for sodium-ion batteries in Examples 1, 1, 2, and 3 of this invention; Figure 4 This is a comparison chart of the cycle performance of sodium-ion half-cells assembled with Prussian blue cathode materials in Examples 1, 2, and 3 of the present invention at a 1C rate. Figure 5The first charge-discharge curves of sodium-ion half-cells assembled from Prussian blue cathode materials of Examples 1, 1, 2, and 3 of this invention at a rate of 0.1C are shown. Detailed Implementation
[0028] To facilitate understanding of the present invention, the invention will be described more fully and in detail below with reference to the accompanying drawings and preferred embodiments, but the scope of protection of the present invention is not limited to the following specific embodiments.
[0029] Unless otherwise defined, all technical terms used herein have the same meaning as commonly understood by those skilled in the art. The technical terms used herein are for the purpose of describing particular embodiments only and are not intended to limit the scope of protection of the invention.
[0030] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this invention can be purchased from the market or prepared by existing methods.
[0031] Example 1: The iron-based Prussian blue cathode material (Na) in this embodiment x Fe[Fe(CN)6] y ·nH2O) was prepared using the following method: S1. Coprecipitation Synthesis: Weigh 5.56 g of ferrous sulfate heptahydrate and 14.7056 g of sodium citrate and dissolve them in deionized water to prepare 1000 mL of solution A; weigh 9.6816 g of sodium ferrocyanide decahydrate and dissolve it in deionized water to prepare 1000 mL of solution B. Stir solutions A and B separately at 800 rpm for 30 min. Slowly add solution A to solution B dropwise using a peristaltic pump while stirring slowly and evenly. After the addition is complete, continue stirring for 10 min, then allow to stand for 24 h. Remove the supernatant, centrifuge to separate the precipitate, wash three times with deionized water and centrifuge again to obtain a Prussian blue wet filter cake.
[0032] S2. Pretreatment: In an argon atmosphere glove box, take a piece of aluminum foil (thickness 0.1mm, size 10cm×10cm) that has been pre-cooled to -40℃, and spread the wet filter cake obtained in step S1 evenly on the aluminum foil to form a uniform thin layer with a thickness of about 2mm.
[0033] S3. Liquid nitrogen quick-freezing: Hold the edge of the aluminum foil with tweezers and quickly immerse the entire foil into the liquid nitrogen Dewar flask. Hold for 60 seconds until no more bubbles are generated and the material is completely solidified.
[0034] S4. Freeze-drying: The frozen aluminum foil-ice cake composite was quickly transferred to the sample rack of the freeze dryer that had been pre-cooled to -60°C. The chamber cover was closed, the vacuum pump was started, and the pressure inside the chamber was maintained below 0.02 mbar. The cold trap temperature was -64°C, and the mixture was sublimated and dried for 48 hours to obtain the primary dried powder.
[0035] S5. Low-temperature vacuum heat treatment: The freeze-dried blue loose powder was transferred to a vacuum oven and heat-treated for 6 hours under an argon atmosphere at an absolute pressure below 100 Pa and a temperature of 120°C to obtain the Prussian blue cathode material with low crystal water content in this embodiment. Its SEM and XRD patterns are shown below. Figure 1 As shown ( Figure 1 (a, b, c, and d are SEM images of Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3, respectively) Figure 2 As shown, the Prussian blue cathode material of the sodium-ion battery in this embodiment exhibits a loose and porous granular structure.
[0036] Thermogravimetric analysis was performed on the Prussian blue cathode material for sodium-ion batteries, and the results are as follows: Figure 3 As shown in Table 1.
[0037] Comparative Example 1: The preparation method of the Prussian blue cathode material in this comparative example is exactly the same as that in Example 1. The Prussian blue wet filter cake obtained in S1 of this comparative example is directly placed in a vacuum oven at 120°C and dried for 12 hours to obtain the sodium-ion battery Prussian blue cathode material of this comparative example. Its SEM image and XRD pattern are shown below. Figure 1 As shown and Figure 2 As shown.
[0038] Thermogravimetric analysis was performed on the Prussian blue cathode material of the sodium-ion battery in this comparative example, and the results are as follows: Figure 3 As shown in Table 1.
[0039] Comparative Example 2: The preparation method of the Prussian blue cathode material in this comparative example is basically the same as that in Example 1. The only difference is that the aluminum foil carrier in step S2 is replaced with a regular centrifuge tube. All other steps and process parameters are the same as in Example 1.
[0040] The SEM and XRD patterns of the Prussian blue cathode material for this comparative sodium-ion battery are shown below. Figure 1 As shown and Figure 2 As shown.
[0041] Comparative Example 3: The preparation method of the Prussian blue cathode material in this comparative example is basically the same as that in Example 1. The only difference is that the low-temperature vacuum heat treatment in step S5 is omitted in this comparative example. That is, the product is collected directly after the freeze-drying in step S4. The remaining steps and process parameters are the same as those in Example 1.
[0042] The SEM and XRD patterns of the Prussian blue cathode material for this comparative sodium-ion battery are shown below. Figure 1 As shown and Figure 2 As shown.
[0043] Example 2: The preparation method of the manganese-based Prussian blue cathode material in this embodiment is basically the same as that in Example 1. The only difference is that in S1 of this embodiment, ferrous sulfate heptahydrate is replaced with an equimolar amount of manganese sulfate monohydrate. The remaining steps and process parameters are exactly the same as those in Example 1, and the manganese-based Prussian blue cathode material is finally obtained.
[0044] Comparative Example 4: The preparation method of the Prussian blue cathode material in this comparative example is exactly the same as that in Example 2, S1. The wet Prussian blue filter cake obtained in S1 was directly placed in a vacuum oven at 120°C and dried for 12 hours to obtain the sodium-ion battery Prussian blue cathode material of this comparative example. SEM images of the Prussian blue cathode material of this comparative example were analyzed. The SEM images showed that the particles were severely agglomerated into large clumps, making it difficult to discern the initial cubic morphology. Thermogravimetric analysis was performed on the sodium-ion battery Prussian blue cathode material of this comparative example, and the results are shown in Table 1.
[0045] Comparative Example 5: The preparation method of the Prussian blue cathode material in this comparative example is basically the same as that in Example 2, except that the aluminum foil carrier in step S2 is replaced with a regular centrifuge tube. All other steps and process parameters are the same as in Example 2. SEM and thermogravimetric analyses were performed on the sodium-ion battery Prussian blue cathode material of this comparative example, and the results are shown in Table 1.
[0046] Comparative Example 6: The preparation method of the Prussian blue cathode material in this comparative example is basically the same as that in Example 2, except that the low-temperature vacuum heat treatment in step S5 is omitted, i.e., the product is collected directly after freeze-drying in step S4. The remaining steps and process parameters are the same as in Example 2. SEM and thermogravimetric analysis were performed on the sodium-ion battery Prussian blue cathode material of this comparative example, and the results are shown in Table 1.
[0047] The Prussian blue cathode materials of sodium-ion batteries in each embodiment and comparative example were used as cathode active materials, and electrode sheets were prepared by mixing them with conductive carbon black and PVDF binder in a 7:2:1 ratio. Sodium metal was used as the counter electrode, and CR2032 coin cells were assembled for testing. The electrolyte was 1M NaClO4 in EC / DEC (1:1), 5% FEC. The first-cycle charge-discharge capacity and coulombic efficiency were tested at 0.1C rate, and the capacity retention rate after 200 cycles was tested at 1C rate. The results are shown in Table 1. Figure 4 , Figure 5 As shown.
[0048] Results analysis: 1. Comparing Example 1 with Comparative Examples 1, 2, and 3, it is evident that only by simultaneously employing the two key features of "metal foil + liquid nitrogen quick-freezing" and "freeze-drying followed by low-temperature heat treatment" can the lowest water of crystallization content (2.1 wt%) and optimal cycle stability (88% retention rate) be achieved. Eliminating the metal foil (Comparative Example 2) or the post-treatment (Comparative Example 3) both resulted in a significant decrease in performance.
[0049] 2. Although Comparative Example 3 was freeze-dried, the residual water of crystallization was as high as 6.4 wt%, indicating that freeze-drying could not completely remove the coordinated water and low-temperature heat treatment was necessary.
[0050] 3. Although conventional heat drying (Comparative Example 1) has a low water of crystallization content (2.8 wt%), hard agglomeration leads to a much lower cycle stability than in Example 1.
[0051] 4. The manganese-based systems (Example 2 and Comparative Examples 4-6) showed the same trend, demonstrating the universality of the method of the present invention.
[0052] The above embodiments and comparative examples fully demonstrate that the present invention can effectively solve the problems of structural damage and particle agglomeration in the dehydration process of Prussian blue materials, and can completely remove crystal water, including coordination water, thus significantly improving its comprehensive electrochemical performance as a cathode material for sodium-ion batteries.
[0053] Table 1: Electrochemical performance test results of sodium-ion battery cathode materials in each embodiment and comparative example
[0054] The above are merely preferred embodiments of the present invention, and the scope of protection of the present invention is not limited to the above embodiments. For those skilled in the art, improvements and modifications obtained without departing from the inventive concept should also be considered within the scope of protection of the present invention.
[0055] Although embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of the present invention.
Claims
1. A method for preparing Prussian blue cathode material for sodium-ion batteries, characterized in that, Includes the following steps: S1. The wet material of the synthesized and filtered sodium-ion battery Prussian blue cathode material is uniformly spread onto a carrier in a protective atmosphere; the carrier is a material with high thermal conductivity. S2. Use liquid nitrogen to perform deep cryogenic quick-freezing treatment on the carrier containing the wet material, so that the water in the wet material solidifies into microcrystalline ice. S3. The carrier and wet material after deep cryogenic quick-freezing are vacuum freeze-dried at a temperature below -60°C to obtain primary dry powder. S4. The primary dry powder is heat-treated under vacuum conditions at 120~150°C in a protective atmosphere to remove residual coordination water, thereby obtaining the Prussian blue cathode material for sodium-ion batteries.
2. The method for preparing the Prussian blue cathode material for sodium-ion batteries according to claim 1, characterized in that, In S1, the thermal conductivity of the carrier is greater than 200 W / (m·K), and the thickness of the carrier is 0.05~0.2 mm.
3. The method for preparing the Prussian blue cathode material for sodium-ion batteries according to claim 2, characterized in that, The carrier is aluminum foil or copper foil.
4. The method for preparing the Prussian blue cathode material for sodium-ion batteries according to claim 1, characterized in that, In S1, the carrier is pre-cooled before the wet material is laid.
5. The method for preparing the Prussian blue cathode material for sodium-ion batteries according to claim 1, characterized in that, In S1, the thickness of the wet material laid on the carrier is less than 5 mm.
6. The method for preparing the Prussian blue cathode material for sodium-ion batteries according to any one of claims 1-5, characterized in that, In S2, the cryogenic quick-freezing treatment takes 30 seconds to 3 minutes, and the entire cryogenic quick-freezing process is completed in a protective atmosphere.
7. The method for preparing the Prussian blue cathode material for sodium-ion batteries according to any one of claims 1-5, characterized in that, In S3, the drying time of the vacuum freeze-drying operation is 24~72h, and the vacuum degree is less than 0.02mbar.
8. The method for preparing the Prussian blue cathode material for sodium-ion batteries according to any one of claims 1-5, characterized in that, In S3, before performing vacuum freeze-drying, the freeze dryer is pre-cooled to a cold trap temperature below -60°C.
9. The method for preparing the Prussian blue cathode material for sodium-ion batteries according to any one of claims 1-5, characterized in that, In S4, the heat treatment time is 2 to 10 hours, and the absolute pressure of the vacuum condition is less than 100 Pa.
10. A Prussian blue cathode material for sodium-ion batteries, characterized in that, The sodium-ion battery Prussian blue cathode material is prepared by any one of the preparation methods described in claims 1-9. The Prussian blue cathode material is a powder with a loose and porous structure and no obvious hard agglomeration between particles. The mass percentage of residual water of crystallization in the sodium-ion battery Prussian blue cathode material is ≤2.3%.
Citation Information
Patent Citations
Preparation method of sodium ion battery positive electrode Prussian blue material