A method for preparing battery-grade lithium carbonate from waste lithium iron phosphate black powder
The direct preparation of battery-grade lithium carbonate through a fully membrane-integrated process solves the problems of long process, high consumption of auxiliary materials, difficulty in removing impurities, and high wastewater treatment costs in the existing lithium iron phosphate battery recycling process, and realizes efficient and environmentally friendly lithium recycling and lithium carbonate preparation.
Patent Information
- Application Number
- CN202611447175.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-17
- Publication Date
- 2026-11-17
AI Technical Summary
Existing lithium iron phosphate battery recycling processes are lengthy, consume large amounts of auxiliary materials, produce low-purity lithium carbonate products, generate large amounts of high-salt wastewater, are environmentally unfriendly, require large equipment investments, and have a high lithium loss rate.
A complete membrane integrated process is adopted, which includes chemical precipitation for coarse impurity removal, membrane separation for fine purification, bipolar membrane acid-base regeneration, and membrane carbonization. Battery-grade lithium carbonate is directly prepared through chemical impurity removal, nanofiltration membrane, and bipolar membrane electrodialysis, avoiding the traditional evaporation and concentration process and realizing full internal circulation.
Shorten the process flow, reduce production costs, reduce auxiliary material consumption, improve lithium recovery rate, reduce wastewater and waste residue, improve lithium carbonate purity, and achieve both environmental protection and economic benefits.
Smart Images

Figure CN123105686A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of battery recycling technology, and relates to a method for preparing battery-grade lithium carbonate from waste lithium iron phosphate black powder. Background Art Lithium iron phosphate (LFP) batteries have become the first choice for many battery companies in the early stages of production due to their advantages such as long cycle life, high safety, low cost, and less environmental pollution. However, as the service life of batteries increases, their energy will decay, and the amount of scrapped LFP batteries will increase exponentially. As a result, the importance and urgency of the LFP battery recycling and disposal problem are growing day by day.
[0002] The current mainstream process for lithium extraction from lithium iron phosphate battery black powder involves first preparing a slurry of lithium iron phosphate powder with water, then adding industrial-grade sulfuric acid for acidification. After controlling the pH value appropriately, hydrogen peroxide is added for oxidative delithiation, converting lithium into lithium sulfate, which enters the liquid phase. Most of the other substances, such as graphite, iron phosphate, aluminum, and copper, remain in the solid phase. A small amount of iron phosphate, copper, and aluminum form soluble ions, becoming impurities in the lithium sulfate solution. The lithium sulfate solution is then purified, mainly by adjusting the pH value and adding precipitants such as lime and sodium fluoride for further purification. The purified lithium sulfate is then concentrated by evaporation to enrich lithium to above 30 g / L. The lithium-rich solution reacts with sodium carbonate solution to precipitate industrial-grade lithium carbonate. The industrial-grade lithium carbonate undergoes a second purification to become battery-grade lithium carbonate. The lithium precipitation mother liquor is then desalted by adding acid to remove carbonate ions and adding alkali to adjust the pH value to meet the operating conditions of the evaporator, producing sodium sulfate as a byproduct. The disadvantages of this process are that it has a long process flow, high consumption of auxiliary materials, high energy consumption, low purity of lithium carbonate products, generates a large amount of high-salt wastewater which is environmentally unfriendly, large equipment investment, and great difficulty in automation integration.
[0003] Therefore, developing a lithium iron phosphate black powder recovery process with high lithium recovery rate, short process flow, low auxiliary material consumption, high purity of lithium carbonate products, environmental friendliness and lower cost is an urgent technical problem to be solved. Summary of the Invention
[0004] To address the shortcomings of existing technologies, the present invention aims to provide a method for preparing battery-grade lithium carbonate from waste lithium iron phosphate black powder. The method provided by this invention eliminates the need for first preparing industrial-grade lithium carbonate followed by secondary purification to obtain battery-grade lithium carbonate. Instead, it directly produces a product superior to battery-grade lithium carbonate standards. This solves the problems of high production costs, large consumption of auxiliary materials, difficulty in removing impurities, and high wastewater treatment costs associated with traditional processes. Furthermore, the absence of large amounts of waste residue, byproducts such as sodium sulfate, and wastewater reduces lithium loss and thus improves lithium recovery rates.
[0005] To achieve this objective, the present invention adopts the following technical solution: This invention provides a method for preparing battery-grade lithium carbonate from waste lithium iron phosphate black powder, the method comprising the following steps: S1. Mixed acid solution, oxidant and waste lithium iron phosphate black powder are subjected to oxidative leaching, and the pH value is adjusted to obtain leaching residue and lithium-containing leaching solution; S2. The lithium-containing leaching solution described in S1 is subjected to chemical purification, nanofiltration purification, and first resin adsorption purification in sequence to obtain a purified solution. The purified solution is then concentrated by a concentration membrane and then subjected to second resin adsorption purification to obtain a lithium-rich solution. S3. The lithium-rich solution described in S2 is subjected to bipolar membrane electrodialysis to obtain an acid solution and a preliminary lithium hydroxide solution. S4. The preliminary lithium hydroxide solution described in S3 is subjected to nanofiltration to remove sulfate ions, thereby obtaining a purified lithium hydroxide solution. S5. The purified lithium hydroxide solution described in S4 is subjected to a carbonization reaction to obtain battery-grade lithium carbonate.
[0006] In one embodiment of the present invention, the acid solution in step S1 includes a sulfuric acid solution; the concentration of the acid solution in step S1 is 1.5 mol / L to 3 mol / L, preferably 1.8 mol / L to 2 mol / L.
[0007] In one embodiment of the present invention, the actual molar amount of the oxidant used in step S1 is 1.05 to 2 times the theoretical molar amount.
[0008] In one embodiment of the present invention, the waste lithium iron phosphate black powder in step S1 includes any one or a combination of at least two of the following: retired lithium iron phosphate battery powder, retired lithium iron phosphate electrode powder, or lithium iron phosphate electrode scrap black powder.
[0009] In one embodiment of the present invention, the mixing in step S1 includes: mixing an acid solution and waste lithium iron phosphate black powder to form a slurry, and then adding an oxidant for oxidative leaching; the liquid-to-solid ratio during the mixing and slurrying process is (3~8):1mL / g.
[0010] In one embodiment of the present invention, step S1 involves adjusting the pH value to 1.8-4, preferably 1.8-2.2.
[0011] In one embodiment of the present invention, the chemical purification in step S2 includes neutralization purification and calcium precipitation purification.
[0012] In one embodiment of the present invention, the flow rate of the first resin adsorption and impurity removal in step S2 is 2 BV / h to 8 BV / h.
[0013] In one embodiment of the present invention, after the concentration treatment by the concentration membrane in step S2, the lithium ion concentration in the concentrate is 8 g / L to 20 g / L; the concentration membrane in step S2 includes a desalination membrane.
[0014] In one embodiment of the present invention, the flow rate of the second resin adsorption and impurity removal in step S2 is 2 BV / h to 8 BV / h.
[0015] In one embodiment of the present invention, the lithium ion concentration in the lithium-rich solution in step S2 is 8 g / L to 20 g / L.
[0016] In one embodiment of the present invention, the acid solution described in step S3 is reused in step S1.
[0017] In one embodiment of the present invention, the concentration of the acid solution in step S3 is 1.5 mol / L to 3 mol / L.
[0018] In one embodiment of the present invention, the concentration of the preliminary lithium hydroxide solution in step S3 is 1.5 mol / L to 2.3 mol / L, and the concentration of sulfate ions in the preliminary lithium hydroxide solution in step S3 is 4 g / L to 8 g / L.
[0019] In one embodiment of the present invention, the nanofiltration in step S4 is performed ≥ 2 times.
[0020] In one embodiment of the present invention, after nanofiltration in step S4, nanofiltrate and purified lithium hydroxide solution are obtained. The nanofiltrate is reused in step S1 to adjust the pH value. The sulfate ion content in the nanofiltrate is 20 g / L to 30 g / L.
[0021] In one embodiment of the present invention, the concentration of sulfate ions in the purified lithium hydroxide solution in step S4 is ≤280ppm.
[0022] In one embodiment of the present invention, the carbon source used in the carbonization process in step S5 includes gaseous carbon dioxide and / or lithium bicarbonate. In one embodiment of the present invention, the carbonization temperature of the carbonization process in step S5 is 50°C to 80°C, and the carbonization pH value of the carbonization process in step S5 is 10 to 11.
[0023] In one embodiment of the present invention, after the carbonization reaction in step S5, battery-grade lithium carbonate and lithium precipitation mother liquor are obtained. The lithium precipitation mother liquor reacts with carbon dioxide to obtain a lithium bicarbonate solution. The lithium bicarbonate solution is concentrated by reverse osmosis, and the resulting lithium bicarbonate concentrate is used as a carbon source for reuse in the carbonization process.
[0024] In one embodiment of the present invention, the carbon source used in the carbonization process of step S5 includes gaseous carbon dioxide.
[0025] Compared with the prior art, the present invention has the following beneficial effects: This invention provides a method for preparing battery-grade lithium carbonate from waste lithium iron phosphate black powder. Through the synergistic cooperation of various recycling processes, a fully integrated membrane process system is constructed with "chemical precipitation for coarse impurity removal—membrane separation for fine purification—bipolar membrane acid-base regeneration—membrane carbonization" as its core. This reduces the process flow, eliminating the need to first prepare industrial-grade lithium carbonate and then purify it a second time to obtain battery-grade lithium carbonate. Instead, it can directly produce products that exceed the standards for battery-grade lithium carbonate. The method provided by this invention solves the problems of high production costs, large consumption of auxiliary materials, difficulty in removing impurities, and high wastewater treatment costs associated with traditional methods. After obtaining the lithium-containing leachate in step S1, in step S2, chemical impurity removal, nanofiltration membrane impurity removal, and first resin adsorption ensure that the lithium-containing solution (lithium sulfate solution) meets the requirements for bipolar membrane inlet, while eliminating the traditional secondary purification step. The impurity-removed liquid is enriched by a concentration membrane and then adsorbed by a second resin to obtain a high-concentration lithium-rich solution. In step S3, bipolar membrane electrodialysis is used to remove lithium sulfate from the lithium-rich solution in situ. The lithium sulfate solution is ionized into hydrogen and hydroxide ions, allowing it to recombine into sulfuric acid and lithium hydroxide. This directly replaces the traditional process of purchasing acids and alkalis (saving up to 95% of acid and alkali usage) and completely avoids the waste salt generated by evaporation, concentration, and crystallization. In step S4, residual sulfate ions in the lithium hydroxide solution are removed by an alkali-resistant nanofiltration membrane, achieving deep purification of the lithium hydroxide solution. Then, in step S5, a simple carbonization process yields battery-grade lithium carbonate. This invention replaces the traditional thermal evaporation and concentration process entirely with nanofiltration membranes, concentration membranes, and bipolar membranes, while significantly reducing the consumption of auxiliary materials such as sodium fluoride, quicklime, sodium carbonate, and sodium hydroxide. The process water is largely recycled internally, eliminating high-salt wastewater and sodium sulfate byproducts, and producing no large amount of waste residue. This eliminates lithium loss caused by wastewater, waste residue, and byproducts in traditional processes, significantly improving the total lithium yield and greatly reducing recycling costs. It is an economical and environmentally friendly method for preparing battery-grade lithium carbonate. Attached Figure Description
[0026] Figure 1 This is a process flow diagram of the method for preparing battery-grade lithium carbonate from waste lithium iron phosphate black powder provided in Embodiment 1 of the present invention.
[0027] Figure 2 This is a process flow diagram of the method for preparing battery-grade lithium carbonate from waste lithium iron phosphate black powder, provided in Comparative Example 1 of the present invention. Detailed Implementation
[0028] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.
[0029] The "range" disclosed in this invention can be defined in the form of a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of the specific range. This type of range definition can include or exclude endpoints; any endpoint can be independently included or excluded, and they can be arbitrarily combined, meaning any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60~120 and 80~110 are listed for specific parameters, it is understood that ranges of 60~110 and 80~120 are also expected. Furthermore, if minimum range values 1 and 2 are listed, and maximum range values 3, 4, and 5 are also listed, then the following ranges are all expected: 1~3, 1~4, 1~5, 2~3, 2~4, and 2~5. In this invention, unless otherwise stated, the numerical range "a~b" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0~5" indicates that all real numbers between "0" and "5" have been listed in this article; "0~5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is described as an integer ≥2, it is equivalent to listing integers such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc. For instance, when a parameter is described as an integer selected from "2~10", it is equivalent to listing the integers 2, 3, 4, 5, 6, 7, 8, 9, and 10.
[0030] In this invention, "a combination of at least two" refers to a quantity greater than or equal to two, unless otherwise specified. For example, "any combination of one or at least two" means one or more or more items. It can be understood that when referring to "a combination of at least two," it refers to any suitable combination of multiple items, that is, a combination of "at least two" items carried out in a manner that does not conflict with and enables the implementation of this invention.
[0031] Unless otherwise specified, all embodiments and optional embodiments of the present invention can be combined with each other to form new technical solutions.
[0032] The term "embodiment" as used in this invention means that a specific feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment or implementation of the invention. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a mutually exclusive, independent, or alternative embodiment. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described in this invention can be combined with other embodiments.
[0033] In this invention, open-ended technical features or solutions described using terms such as "comprising" do not exclude additional members beyond those listed unless otherwise specified. They can be considered as providing both closed-ended features or solutions comprised of the listed members and open-ended features or solutions that include additional members beyond the listed members. For example, A includes a1, a2, and a3. Unless otherwise specified, it may also include other members or exclude additional members. This can be considered as providing both technical features or solutions where "A is composed of a1, a2, and a3" or "A is selected from a1, a2, and a3," and technical features or solutions where "A includes not only a1, a2, and a3, but also other members."
[0034] In this invention, the terms "first aspect," "second aspect," "third aspect," "fourth aspect," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance or quantity, nor should they be construed as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first," "second," "third," "fourth," etc., serve only as a non-exhaustive enumeration and should be understood not to constitute a closed limitation on the quantity.
[0035] In this invention, unless otherwise specified, the features or solutions corresponding to "and / or" include any one of two or more of the related listed items, as well as any and all combinations of the related listed items. These arbitrary and all combinations include any two related listed items, any more related listed items, or a combination of all related listed items. For example, "A and / or B" represents a group consisting of A, B, and "a combination of A and B". "Containing A and / or B" can mean "containing A, containing B, and containing A and B", or "containing A, containing B, or containing A and B", and can be appropriately understood according to the context.
[0036] In this invention, "room temperature" generally refers to 4℃~35℃, and can refer to 20℃±5℃. In some embodiments of this invention, room temperature refers to 20℃~30℃.
[0037] In one embodiment, the present invention provides a method for preparing battery-grade lithium carbonate from waste lithium iron phosphate black powder, the method comprising the following steps: S1. Mixed acid solution, oxidant and waste lithium iron phosphate black powder are subjected to oxidative leaching, and the pH value is adjusted to obtain leaching residue and lithium-containing leaching solution; S2. The lithium-containing leaching solution described in S1 is subjected to chemical purification, nanofiltration purification, and first resin adsorption purification in sequence to obtain a purified solution. The purified solution is then concentrated by a concentration membrane and then subjected to second resin adsorption purification to obtain a lithium-rich solution. S3. The lithium-rich solution described in S2 is subjected to bipolar membrane electrodialysis to obtain an acid solution and a preliminary lithium hydroxide solution. S4. The preliminary lithium hydroxide solution described in S3 is subjected to nanofiltration to remove sulfate ions, thereby obtaining a purified lithium hydroxide solution. S5. The purified lithium hydroxide solution described in S4 is subjected to a carbonization reaction to obtain battery-grade lithium carbonate.
[0038] This invention provides a method for preparing battery-grade lithium carbonate from waste lithium iron phosphate black powder. Through the synergistic cooperation of various recycling processes, a fully integrated membrane process system is constructed with "chemical precipitation for coarse impurity removal—membrane separation for fine purification—bipolar membrane acid-base regeneration—membrane carbonization" as its core. This reduces the process flow, eliminating the need to first prepare industrial-grade lithium carbonate and then purify it a second time to obtain battery-grade lithium carbonate. Instead, it can directly produce products that exceed the standards for battery-grade lithium carbonate. The method provided by this invention solves the problems of high production costs, large consumption of auxiliary materials, difficulty in removing impurities, and high wastewater treatment costs associated with traditional methods. After obtaining the lithium-containing leachate in step S1, in step S2, chemical impurity removal, nanofiltration membrane impurity removal, and first resin adsorption ensure that the lithium-containing solution (lithium sulfate solution) meets the requirements for bipolar membrane inlet, while eliminating the traditional secondary purification step. The impurity-removed liquid is enriched by a concentration membrane and then adsorbed by a second resin to obtain a high-concentration lithium-rich solution. In step S3, bipolar membrane electrodialysis is used to remove lithium sulfate from the lithium-rich solution in situ. The lithium sulfate solution is ionized into hydrogen and hydroxide ions, allowing it to recombine into sulfuric acid and lithium hydroxide. This directly replaces the traditional process of purchasing acids and alkalis (saving up to 95% of acid and alkali usage) and completely avoids the waste salt generated by evaporation, concentration, and crystallization. In step S4, residual sulfate ions in the lithium hydroxide solution are removed by an alkali-resistant nanofiltration membrane, achieving deep purification of the lithium hydroxide solution. Then, in step S5, a simple carbonization process yields battery-grade lithium carbonate. This invention replaces the traditional thermal evaporation and concentration process entirely with nanofiltration membranes, concentration membranes, and bipolar membranes, while significantly reducing the consumption of auxiliary materials such as sodium fluoride, quicklime, sodium carbonate, and sodium hydroxide. The process water is largely recycled internally, eliminating high-salt wastewater and sodium sulfate byproducts, and producing no large amount of waste residue. This eliminates lithium loss caused by wastewater, waste residue, and byproducts in traditional processes, significantly improving the total lithium yield and greatly reducing recycling costs. It is an economical and environmentally friendly method for preparing battery-grade lithium carbonate.
[0039] In some embodiments, the acid solution in step S1 includes a sulfuric acid solution; the concentration of the acid solution in step S1 is 1.5 mol / L to 3 mol / L, for example, 1.5 mol / L, 1.8 mol / L, 1.9 mol / L, 2 mol / L, 2.3 mol / L, 2.5 mol / L, 2.8 mol / L or 3 mol / L, etc.; preferably 1.8 mol / L to 2 mol / L.
[0040] This invention uses a relatively low concentration of dilute sulfuric acid solution as the pulping raw material for lithium iron phosphate black powder, which is beneficial to the normal progress of subsequent processes.
[0041] In some embodiments, the actual molar amount of oxidant used in step S1 is 1.05 to 2 times the theoretical molar amount, for example, 1.05 times, 1.1 times, 1.2 times, 1.3 times, 1.4 times, 1.5 times, 1.6 times, 1.7 times, 1.8 times, 1.9 times or 2 times.
[0042] It is understood that the theoretical molar amount of oxidant in this application is the amount of oxidant calculated based on the substance to be oxidized in lithium iron phosphate black powder; the present invention can make the reaction more thorough and the lithium leaching effect more excellent by adding an appropriate excess of oxidant.
[0043] This invention does not limit the specific type of oxidant; conventional oxidants can be used without departing from the overall technical concept of this invention.
[0044] As an example, the oxidant includes at least one of hydrogen peroxide, air, oxygen, ozone, lithium persulfate, or lithium ferrate, preferably hydrogen peroxide.
[0045] In some embodiments, the waste lithium iron phosphate black powder in step S1 includes any one or a combination of at least two of the following: retired lithium iron phosphate battery powder, retired lithium iron phosphate electrode powder, or lithium iron phosphate electrode scrap black powder.
[0046] The source of the waste lithium iron phosphate black powder in this invention is not unique. It can be powder obtained from retired lithium iron phosphate batteries or waste materials from the preparation process. Those skilled in the art can make adaptive selections and adjustments according to actual needs.
[0047] In some embodiments, the mixing in step S1 includes: mixing the acid solution and waste lithium iron phosphate black powder to form a slurry, and then adding an oxidant for oxidative leaching; the liquid-to-solid ratio during the mixing and slurrying process is (3~8):1mL / g, for example 3:1mL / g, 4:1mL / g, 5:1mL / g, 6:1mL / g, 7:1mL / g or 8:1mL / g, etc.
[0048] In some embodiments, step S1 involves adjusting the pH value to 1.8 to 4, such as 1.8, 1.9, 2, 2.1, 2.2, 2.5, 2.8, 3, 3.5, 3.8, or 4; preferably 1.8 to 2.2.
[0049] In some embodiments, the chemical purification in step S2 includes neutralization purification and calcium precipitation purification.
[0050] As an example, the neutralization and impurity removal includes adding lime water for precipitation and impurity removal, while calcium precipitation and impurity removal can use lithium carbonate as the impurity removal precipitant.
[0051] In some embodiments, the flow rate of the first resin adsorption and impurity removal in step S2 is 2BV / h to 8BV / h, for example, 2BV / h, 3BV / h, 4BV / h, 5BV / h, 6BV / h, 7BV / h or 8BV / h.
[0052] In some embodiments, the nanofiltration impurity removal in step S2 is performed using a nanofiltration membrane, and the nanofiltration membrane can be a conventional type that can separate monovalent metal ions and non-monovalent metal ions.
[0053] In some embodiments, after the concentration treatment by the concentration membrane in step S2, the lithium ion concentration in the concentrate is 8 g / L to 20 g / L, such as 8 g / L, 9 g / L, 10 g / L, 11 g / L, 12 g / L, 13 g / L, 14 g / L, 15 g / L, 16 g / L, 17 g / L, 18 g / L, 19 g / L, or 20 g / L; the concentration membrane in step S2 includes a desalination membrane.
[0054] This invention uses a seawater desalination membrane as a concentration membrane, which can achieve deep concentration of the purified liquid.
[0055] In some embodiments, the flow rate of the second resin adsorption and impurity removal in step S2 is 2BV / h to 8BV / h, for example, 2BV / h, 3BV / h, 4BV / h, 5BV / h, 6BV / h, 7BV / h or 8BV / h.
[0056] It is understood that the present invention does not specifically limit the resins used for the first resin adsorption and the second resin adsorption and purification. Conventional resin types are applicable to the present invention without departing from the overall technical concept of the present invention; for example, imprinting resin.
[0057] In some embodiments, the lithium ion concentration in the lithium-rich solution described in step S2 is 8 g / L to 20 g / L, for example, 8 g / L, 9 g / L, 10 g / L, 11 g / L, 12 g / L, 13 g / L, 14 g / L, 15 g / L, 16 g / L, 17 g / L, 18 g / L, 19 g / L, or 20 g / L.
[0058] In some embodiments, the acid solution described in step S3 is reused in step S1.
[0059] In some embodiments, the concentration of the acid solution in step S3 is 1.5 mol / L to 3 mol / L, for example, 1.5 mol / L, 1.8 mol / L, 1.9 mol / L, 2 mol / L, 2.3 mol / L, 2.5 mol / L, 2.8 mol / L or 3 mol / L.
[0060] In some embodiments, the concentration of the initial lithium hydroxide solution in step S3 is 1.5 mol / L to 3 mol / L, for example, 1.5 mol / L, 1.8 mol / L, 1.9 mol / L, 2 mol / L, 2.3 mol / L, 2.5 mol / L, 2.8 mol / L, or 3 mol / L.
[0061] In some embodiments, the concentration of sulfate ions in the preliminary lithium hydroxide solution in step S3 is 4 g / L to 8 g / L, for example, 4 g / L, 5 g / L, 6 g / L, 7 g / L or 8 g / L.
[0062] In step S3 of this invention, after obtaining a preliminary lithium hydroxide solution through bipolar membrane electrodialysis, there are still a large number of sulfate ions present. If these sulfate ions are not desulfurized, they will seriously affect the quality of the final lithium carbonate.
[0063] In some implementations, the nanofiltration in step S4 is performed ≥2 times.
[0064] In step S4 of this invention, sulfate ions in the initial lithium hydroxide solution are effectively removed by nanofiltration using a nanofiltration membrane. In particular, the removal effect is more significant when the number of nanofiltrations is controlled to be ≥2.
[0065] In some embodiments, after nanofiltration in step S4, a nanofiltrate and a purified lithium hydroxide solution are obtained. The nanofiltrate is reused in step S1 to adjust the pH value. The sulfate ion content in the nanofiltrate is 20 g / L to 30 g / L, for example, 20 g / L, 21 g / L, 22 g / L, 23 g / L, 24 g / L, 25 g / L, 26 g / L, 27 g / L, 28 g / L, 29 g / L, or 30 g / L.
[0066] In some embodiments, the concentration of sulfate ions in the purified lithium hydroxide solution described in step S4 is ≤280ppm, such as 150ppm, 180ppm, 200ppm, 210ppm, 220ppm, 230ppm, 240ppm, 250ppm, 260ppm, 270ppm, or 280ppm.
[0067] After step S4, the present invention achieves a significant reduction in sulfate ions in the lithium hydroxide solution, which can be directly used in the subsequent carbonization process to prepare battery-grade lithium carbonate without the need for first preparing industrial-grade lithium carbonate and then undergoing a secondary purification process.
[0068] In some embodiments, the carbon source used in the carbonization process of step S5 includes gaseous carbon dioxide and / or lithium bicarbonate. In some embodiments, the carbonization temperature of the carbonization process in step S5 is 50°C to 80°C, such as 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, or 80°C.
[0069] In some embodiments, the carbonization pH value of the carbonization treatment in step S5 is 10 to 11, such as 10, 10.1, 10.2, 10.3, 10.4, 10.5, 10.6, 10.7, 10.8, 10.9 or 11.
[0070] In some embodiments, after the carbonization reaction in step S5, battery-grade lithium carbonate and lithium precipitation mother liquor are obtained. The lithium precipitation mother liquor reacts with carbon dioxide to obtain a lithium bicarbonate solution. The lithium bicarbonate solution is concentrated by reverse osmosis, and the resulting lithium bicarbonate concentrate is reused as a carbon source in the carbonization process.
[0071] In some embodiments, the carbon source used in the carbonization process of step S5 includes gaseous carbon dioxide.
[0072] This invention uses gaseous carbon dioxide as a carbon source and utilizes a microporous membrane structure in a gas-liquid reactor to break down the gaseous carbon dioxide into more tiny bubbles, thereby significantly reducing reaction time and energy consumption. The numerical range described in this invention includes not only the point values listed above, but also any point values within the numerical ranges not listed above. Due to space limitations and for the sake of brevity, this invention will not exhaustively list all the specific point values included in the range.
[0073] Example 1 This embodiment provides a method for preparing battery-grade lithium carbonate from waste lithium iron phosphate black powder, such as... Figure 1 As shown, the method includes the following steps: S1. Use 1.8 mol / L dilute sulfuric acid solution to prepare a slurry from decommissioned lithium iron phosphate electrode powder (waste lithium iron phosphate black powder) with a liquid-to-solid ratio of 5:1. After slurry preparation, add hydrogen peroxide to the slurry. The amount of hydrogen peroxide added is 1.5 times the theoretical amount. Add the hydrogen peroxide slowly and control the reaction temperature at 60℃. After the hydrogen peroxide is added, react for 2 hours. After the reaction, add a pH adjuster (lithium hydroxide solution) to adjust the pH of the slurry to 2.0 and then filter to obtain leaching residue and lithium-containing solution (lithium sulfate solution). The leaching residue is phosphorus iron slag. S2. Lime water is added to the lithium-containing solution to remove impurities, and then excess calcium is removed by lithium carbonate to obtain a first-stage impurity-removed solution. The primary impurity removal solution is subjected to nanofiltration membrane for deep impurity removal to obtain a deeply impurity-removed solution. The liquid after deep impurity removal is subjected to first resin adsorption (imprinting resin) at a flow rate of 4 BV / h to obtain a second impurity removal liquid; The secondary impurity removal solution is concentrated by a concentration membrane (seawater desalination membrane) to obtain a concentrate. The concentrate is then subjected to a second resin adsorption (imprinting resin) at a flow rate of 4 BV / h to remove impurities, resulting in a lithium-rich solution with a lithium concentration of 12 g / L. S3. The lithium-rich solution is treated by bipolar membrane electrodialysis to ionize lithium sulfate in the lithium-rich solution into hydrogen ions and hydroxide ions in situ. The lithium sulfate in the lithium-rich solution is then recombined into sulfuric acid and lithium hydroxide to obtain 1.8 mol / L membrane acid (dilute sulfuric acid solution). The membrane acid is recycled to the pulping in step (1) and at the same time, 1.8 mol / L membrane alkali (preliminary lithium hydroxide solution) is generated. The sulfate content in the membrane alkali is 6 g / L. S4. The alkali produced by the membrane is passed through two nanofiltration membranes to intercept sulfate ions, resulting in nanofiltration membrane concentrate and high-purity lithium hydroxide solution. The concentration of lithium hydroxide in the nanofiltration membrane concentrate and high-purity lithium hydroxide solution remains basically unchanged, maintaining at about 1.8 mol / L. The sulfate content in the nanofiltration membrane concentrate is 24 g / L, and the sulfate concentration in the purified lithium hydroxide solution is 276 ppm. S5. Carbon dioxide is introduced into the purified lithium hydroxide solution to complete the carbonization reaction. The temperature of the carbonization reaction is controlled at 70℃. After the reaction pH stabilizes at 10.5, the solution is filtered. The filter cake is dried and crushed to obtain battery-grade lithium carbonate. The filtrate obtained from filter cake filtration is lithium precipitation mother liquor, which contains about 2 g / L of lithium. Carbon dioxide is introduced into the lithium precipitation mother liquor to convert lithium carbonate, which has low solubility, into lithium bicarbonate, which has high solubility. The lithium bicarbonate solution is then concentrated through a reverse osmosis membrane to obtain reverse osmosis membrane concentrate, which contains about 7 g / L of lithium. The reverse osmosis membrane concentrate produced by this method can be used as a carbon source to precipitate lithium carbonate again.
[0074] Example 2 This embodiment provides a method for preparing battery-grade lithium carbonate from waste lithium iron phosphate black powder, the method comprising the following steps: S1. Use a 2 mol / L dilute sulfuric acid solution to prepare a slurry from decommissioned lithium iron phosphate electrode powder (waste lithium iron phosphate black powder), with a slurry-to-solid ratio of 4:1. After slurry preparation, add hydrogen peroxide to the slurry. The amount of hydrogen peroxide added is twice the theoretical amount. Add the hydrogen peroxide slowly and control the reaction temperature at 60℃. After the hydrogen peroxide is added, react for 2 hours. After the reaction, add a pH adjuster (lithium hydroxide solution) to adjust the pH of the slurry to 2.5 and then filter to obtain leaching residue and lithium-containing solution (lithium sulfate solution). The leaching residue is phosphorus-iron slag. S2. Lime water is added to the lithium-containing solution to remove impurities, and then excess calcium is removed by lithium carbonate to obtain a first-stage impurity-removed solution. The primary impurity removal solution is subjected to nanofiltration membrane for deep impurity removal to obtain a deeply impurity-removed solution. The liquid after deep impurity removal is subjected to first resin adsorption (imprinting resin) at a flow rate of 2 BV / h to remove impurities, resulting in a second impurity removal liquid; The secondary impurity removal solution is concentrated by a concentration membrane (seawater desalination membrane) to obtain a concentrate. The concentrate is then subjected to a second resin adsorption (imprinting resin) at a flow rate of 2 BV / h to remove impurities, resulting in a lithium-rich solution with a lithium concentration of 15 g / L. S3. The lithium-rich solution is treated by bipolar membrane electrodialysis to ionize lithium sulfate in the lithium-rich solution into hydrogen ions and hydroxide ions in situ. The lithium sulfate in the lithium-rich solution is then recombined into sulfuric acid and lithium hydroxide to obtain 2 mol / L membrane acid (dilute sulfuric acid solution). The membrane acid is recycled to the pulping in step (1) and at the same time, 2 mol / L membrane alkali (preliminary lithium hydroxide solution) is generated. The sulfate content in the membrane alkali is 6 g / L. S4. The alkali produced by the membrane is passed through two nanofiltration membranes to intercept sulfate ions, resulting in nanofiltration membrane concentrate and high-purity lithium hydroxide solution. The concentration of lithium hydroxide in the nanofiltration membrane concentrate and high-purity lithium hydroxide solution remains basically unchanged, maintaining at around 2 mol / L. The sulfate content in the nanofiltration membrane concentrate is 20 g / L and is recycled in step S1 as a pH adjuster. The sulfate concentration in the purified lithium hydroxide solution is 250 ppm. S5. Lithium bicarbonate is added to the purified lithium hydroxide solution to complete the carbonization reaction. The carbonization reaction temperature is controlled at 50℃. After the reaction pH stabilizes at 10, the solution is filtered. The filter cake is dried and crushed to obtain battery-grade lithium carbonate. The filtrate obtained from filter cake filtration is lithium precipitation mother liquor, which contains about 2 g / L of lithium. Carbon dioxide is introduced into the lithium precipitation mother liquor to convert lithium carbonate, which has low solubility, into lithium bicarbonate, which has high solubility. The lithium bicarbonate solution is then concentrated through a reverse osmosis membrane to obtain reverse osmosis membrane concentrate, which contains about 7 g / L of lithium. The reverse osmosis membrane concentrate produced by this method can be used as a carbon source to precipitate lithium carbonate again.
[0075] Example 3 This embodiment provides a method for preparing battery-grade lithium carbonate from waste lithium iron phosphate black powder, the method comprising the following steps: S1. Use 1.8 mol / L dilute sulfuric acid solution to prepare a slurry from decommissioned lithium iron phosphate electrode powder (waste lithium iron phosphate black powder), with a slurry-to-solid ratio of 6:1. After slurry preparation, add hydrogen peroxide to the slurry. The amount of hydrogen peroxide added is 1.05 times the theoretical amount. Add the hydrogen peroxide slowly and control the reaction temperature at 60℃. After the hydrogen peroxide is added, react for 2 hours. After the reaction, add a pH adjuster (lithium hydroxide solution) to adjust the pH of the slurry to 4 and then filter to obtain leaching residue and lithium-containing solution (lithium sulfate solution). The leaching residue is phosphorus iron slag. S2. Lime water is added to the lithium-containing solution to remove impurities, and then excess calcium is removed by lithium carbonate to obtain a primary impurity removal solution. The contents of each impurity element in the primary impurity removal solution are Al 0.26ppm, Ni 0.01ppm, Co 0.01ppm, Mn 0.01ppm, Fe 0.06ppm, Ca 2.22ppm, and Mg 0.01ppm, respectively. The primary impurity removal solution is subjected to nanofiltration membrane for deep impurity removal to obtain a deeply impurity-removed solution. The liquid after deep impurity removal is subjected to first resin adsorption (imprinting resin) at a flow rate of 8 BV / h to remove impurities, resulting in a second impurity removal liquid. The secondary impurity removal solution is concentrated by a concentrating membrane (seawater desalination membrane) to obtain a concentrated solution. The concentrated solution is then subjected to a second resin adsorption (imprinting resin) at a flow rate of 8 BV / h to remove impurities, resulting in a lithium-rich solution with a lithium concentration of 20 g / L. S3. The lithium-rich solution is treated by bipolar membrane electrodialysis to ionize lithium sulfate in the lithium-rich solution into hydrogen ions and hydroxide ions in situ. The lithium sulfate in the lithium-rich solution is then recombined into sulfuric acid and lithium hydroxide to obtain 3 mol / L membrane acid (dilute sulfuric acid solution). The membrane acid is recycled to the pulping in step (1) and at the same time, 3 mol / L membrane alkali (preliminary lithium hydroxide solution) is generated. The sulfate content in the membrane alkali is 7 g / L. S4. The alkali produced by the membrane is passed through a nanofiltration membrane three times to intercept sulfate ions, resulting in nanofiltration membrane concentrate and high-purity lithium hydroxide solution. The concentration of lithium hydroxide in the nanofiltration membrane concentrate and high-purity lithium hydroxide solution remains basically unchanged, maintaining at about 3 mol / L. The sulfate content in the nanofiltration membrane concentrate is 30 g / L, and the sulfate concentration in the purified lithium hydroxide solution is 220 ppm. S5. Carbon dioxide is passed into the purified lithium hydroxide solution to complete the carbonization reaction. The carbonization reaction temperature is controlled at 80℃. After the reaction pH stabilizes at 11, the solution is filtered. The filter cake is dried and crushed to obtain battery-grade lithium carbonate. The filtrate obtained from filter cake filtration is lithium precipitation mother liquor, which contains about 2 g / L of lithium. Carbon dioxide is introduced into the lithium precipitation mother liquor to convert lithium carbonate, which has low solubility, into lithium bicarbonate, which has high solubility. The lithium bicarbonate solution is then concentrated through a reverse osmosis membrane to obtain reverse osmosis membrane concentrate, which contains about 7 g / L of lithium. The reverse osmosis membrane concentrate produced by this method can be used as a carbon source to precipitate lithium carbonate again.
[0076] Example 4 The difference between this embodiment and embodiment 1 is that in step S4 of this embodiment, the alkali produced by the membrane is intercepted by a nanofiltration membrane once.
[0077] All other conditions remain the same as in Example 1.
[0078] Comparative Example 1 This comparative example provides a method for preparing battery-grade lithium carbonate from waste lithium iron phosphate black powder, such as... Figure 2 As shown, the method includes the following steps: S1. Use the washing slag solution of ferric phosphate to make a slurry from retired lithium iron phosphate electrode powder (waste lithium iron phosphate black powder). The slurry liquid-solid ratio is 5:1. After slurry preparation, add concentrated sulfuric acid to the slurry to control the pH value between 1.5 and 2.5. At the same time, add hydrogen peroxide. The molar amount of hydrogen peroxide added is 1.05 times the theoretical molar amount. Sulfuric acid and hydrogen peroxide are added slowly. Control the reaction temperature at 60℃. After the hydrogen peroxide is added, react for 2 hours. Test the ferrous ion concentration in the liquid. If the ferrous ion concentration is less than 1g / L, the oxidation is complete. Finally, adjust the pH value of the slurry to 4 with sodium hydroxide. The slurry after the reaction is completed is filtered through a plate and frame filter to obtain a lithium-containing leaching solution (lithium sulfate solution). The filter residue is slurried through a plate and frame filter three times with pure water and washed countercurrently. The wash water is used for raw material slurry preparation. The residue after three washings is ferric phosphate residue. S2. Lime water is added to the lithium-containing solution to remove impurities, mainly fluoride, aluminum, copper, nickel, and cobalt ions. Sodium carbonate is added to the filtered liquid to remove calcium, reducing the calcium ion concentration from 400 ppm to below 20 ppm. The filtrate is then treated with sulfuric acid to control the pH at 2-3 to remove excess carbonate. Sodium hydroxide is then used to adjust the pH to 7-9. This liquid is the purified liquid. The lithium concentration in the purified liquid is too low, which affects the efficiency of subsequent lithium precipitation. Therefore, it needs to be evaporated and concentrated to increase the lithium concentration to above 20 g / L. This is the concentrated evaporated liquid.
[0079] S3. The concentrated evaporation solution from the previous process is fed into a reaction vessel and reacted with a sodium carbonate solution. This allows lithium sulfate to react with sodium carbonate to form lithium carbonate precipitate. The reaction temperature is controlled at approximately 90℃, and the concentration of unprecipitated lithium in the liquid is controlled below 2.5 g / L, and the concentration of carbonate ions is controlled below 20 g / L. The lithium carbonate separated by centrifugation has excessive levels of sulfate, sodium, calcium, and magnesium ions, so its quality only reaches the level of crude lithium carbonate. Therefore, the crude lithium carbonate needs to be carbonized. This involves re-slurrying the lithium carbonate with pure water, adding carbon dioxide to dissolve the lithium carbonate into lithium bicarbonate, and releasing impurities. Because the lithium bicarbonate solution is unstable, heating will cause the lithium bicarbonate to decompose and regenerate lithium carbonate. Through this process of redissolution and crystallization, the finished lithium carbonate product meets battery-grade requirements.
[0080] S4. In the previous process, lithium carbonate precipitation will produce lithium precipitation mother liquor. The mother liquor contains unprecipitated lithium that needs to be recovered, so the mother liquor needs to be pretreated. First, the mother liquor is acidified by adding sulfuric acid to adjust the pH value to 3, so that lithium carbonate is converted into lithium sulfate. Then, sodium hydroxide is added to adjust the pH value to 7-9. The pretreated liquid is fed into the evaporator for concentration. Since the liquid after lithium precipitation contains a large amount of sodium sulfate, the sodium sulfate will crystallize after reaching saturation. The sodium sulfate is separated by centrifuge and becomes by-product sodium sulfate. When the lithium content is concentrated from 3g / L to 20g / L, this liquid is returned to the previous process to continue lithium precipitation. When the system impurity concentration is too high and lithium precipitation is not possible, the liquid needs to be thoroughly treated and enter the next process to produce by-product lithium phosphate. S5. After the concentrated lithium sulfate solution is added, trisodium phosphate is added. The lithium combines with the phosphate to form lithium phosphate, which is less soluble. After precipitation, the lithium content of the liquid is less than 200 ppm. Since this liquid contains excessive phosphate, it needs to be treated as wastewater and sent to the plant's sewage treatment system for treatment. After the water meets the standards, it can be discharged, or it can be evaporated and concentrated to achieve zero discharge.
[0081] Comparative Example 2 The difference between this comparative example and Example 1 is that this comparative example does not perform nanofiltration purification using a nanofiltration membrane in step S2, but directly performs first resin purification after chemical purification.
[0082] All other conditions remain the same as in Example 1.
[0083] Comparative Example 3 The difference between this comparative example and Example 1 is that this comparative example does not perform step S4, that is, it does not perform the nanofiltration process for removing sulfate ions after bipolar membrane electrodialysis.
[0084] All other conditions remain the same as in Example 1.
[0085] The lithium carbonate recovered in the examples and comparative examples was tested using the ICP test method to determine the main mass content of lithium carbonate and the mass content of each impurity. The test results are shown in Table 1.
[0086] Table 1 From Table 1, we can obtain: The method provided by this invention eliminates the need to first prepare industrial-grade lithium carbonate and then purify it a second time to obtain battery-grade lithium carbonate. Instead, it can directly produce products that are superior to battery-grade lithium carbonate standards. This solves the problems of high production costs, large consumption of auxiliary materials, difficulty in removing impurities, and high wastewater treatment costs associated with traditional processes. Furthermore, the absence of large amounts of waste residue, byproduct sodium sulfate, and wastewater leads to a lower lithium loss rate, thereby improving the lithium recovery rate.
[0087] The above description is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention fall within the protection and disclosure scope of the present invention.
Claims
1. A method for preparing battery-grade lithium carbonate from waste lithium iron phosphate black powder, characterized in that, The method includes the following steps: S1. Mixed acid solution, oxidant and waste lithium iron phosphate black powder are subjected to oxidative leaching, and the pH value is adjusted to obtain leaching residue and lithium-containing leaching solution; S2. The lithium-containing leaching solution described in S1 is subjected to chemical purification, nanofiltration purification, and first resin adsorption purification in sequence to obtain a purified solution. The purified solution is then concentrated by a concentration membrane and then subjected to second resin adsorption purification to obtain a lithium-rich solution. S3. The lithium-rich solution described in S2 is subjected to bipolar membrane electrodialysis to obtain an acid solution and a preliminary lithium hydroxide solution. S4. The preliminary lithium hydroxide solution described in S3 is subjected to nanofiltration to remove sulfate ions, thereby obtaining a purified lithium hydroxide solution. S5. The purified lithium hydroxide solution described in S4 is subjected to a carbonization reaction to obtain battery-grade lithium carbonate.
2. The method according to claim 1, characterized in that, The acid solution in step S1 includes a sulfuric acid solution; the concentration of the acid solution in step S1 is 1.5 mol / L to 3 mol / L, preferably 1.8 mol / L to 2 mol / L; And / or, the actual molar amount of the oxidant used in step S1 is 1.05 to 2 times the theoretical molar amount; And / or, the waste lithium iron phosphate black powder in step S1 includes any one or a combination of at least two of the following: retired lithium iron phosphate battery powder, retired lithium iron phosphate electrode powder, or lithium iron phosphate electrode scrap black powder.
3. The method according to claim 1 or 2, characterized in that, The mixing in step S1 includes: mixing the acid solution and waste lithium iron phosphate black powder to form a slurry, then adding an oxidant for oxidative leaching; the liquid-to-solid ratio during the mixing and slurrying process is (3~8):1mL / g; And / or, step S1 involves adjusting the pH value to 1.8-4, preferably 1.8-2.
2.
4. The method according to claim 1, characterized in that, The chemical purification process described in step S2 includes neutralization purification and calcium precipitation purification. And / or, in step S2, the flow rate of the first resin adsorption for impurity removal is 2 BV / h to 8 BV / h.
5. The method according to claim 1 or 4, characterized in that, After concentration treatment by the concentration membrane in step S2, the lithium ion concentration in the concentrate is 8 g / L to 20 g / L; the concentration membrane in step S2 includes a desalination membrane; And / or, in step S2, the flow rate of the second resin adsorption for impurity removal is 2 BV / h to 8 BV / h; And / or, the lithium ion concentration in the lithium-rich solution described in step S2 is 8 g / L to 20 g / L.
6. The method according to claim 1, characterized in that, The acid solution described in step S3 is reused in step S1; And / or, the concentration of the acid solution in step S3 is 1.5 mol / L to 3 mol / L; And / or, the concentration of the preliminary lithium hydroxide solution in step S3 is 1.5 mol / L to 3 mol / L, and the concentration of sulfate ions in the preliminary lithium hydroxide solution in step S3 is 4 g / L to 8 g / L.
7. The method according to claim 1, characterized in that, The number of nanofiltrations in step S4 is ≥ 2 times.
8. The method according to claim 1 or 7, characterized in that, After nanofiltration in step S4, nanofiltrate and purified lithium hydroxide solution are obtained. The nanofiltrate is reused in step S1 to adjust the pH value. The sulfate ion content in the nanofiltrate is 20 g / L to 30 g / L. And / or, the concentration of sulfate ions in the purified lithium hydroxide solution described in step S4 is ≤280ppm.
9. The method according to claim 1, characterized in that, The carbon source used in the carbonization process described in step S5 includes gaseous carbon dioxide and / or lithium bicarbonate. And / or, the carbonization temperature of the carbonization process in step S5 is 50℃~80℃, and the carbonization pH value of the carbonization process in step S5 is 10~11; And / or, after the carbonization reaction described in step S5, battery-grade lithium carbonate and lithium precipitation mother liquor are obtained. The lithium precipitation mother liquor reacts with carbon dioxide to obtain a lithium bicarbonate solution. The lithium bicarbonate solution is concentrated by reverse osmosis, and the resulting lithium bicarbonate concentrate is used as a carbon source for reuse in the carbonization process.
10. The method according to claim 9, characterized in that, The carbon source used in the carbonization process described in step S5 includes gaseous carbon dioxide.