A method for preparing zinc oxide-coated MOF-derived carbon aerogel and its application in lithium-ion battery anodes.
By uniformly coating zinc oxide nanoparticles onto MOFs-derived carbon aerogels, the problem of high irreversible lithium loss in MOFs-derived carbon aerogels as anode materials for lithium-ion batteries was solved, improving the material's first coulombic efficiency and rate performance while maintaining the integrity of its porous structure.
Patent Information
- Application Number
- CN202611369364.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-04
- Publication Date
- 2026-11-17
AI Technical Summary
In the existing technology, MOFs-derived carbon aerogels have problems such as high irreversible lithium loss, low initial coulombic efficiency, and insufficient rate performance and cycle stability in lithium-ion battery anode materials. Directly applying zinc oxide coating process can easily destroy its three-dimensional porous framework structure.
By dispersing MOF-derived carbon aerogels in an aqueous zinc chloride solution and adjusting the pH to generate zinc hydroxide, followed by calcination under a protective atmosphere to convert it into zinc oxide, uniform coating of nanoparticles is achieved, maintaining the porous structure and conductivity of the material.
Zinc oxide nanoparticles are uniformly coated on the surface and inner walls of carbon aerogel channels, forming a continuous conductive network. This improves the material's initial coulombic efficiency and rate performance, and enhances lithium-ion transport capability and cycle stability.
Smart Images

Figure CN123105703A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium-ion battery technology, and in particular to a method for preparing zinc oxide-coated MOFs-derived carbon aerogel and its application in the negative electrode of lithium-ion batteries. Background Technology
[0002] Faced with the dual challenges of fossil fuel depletion and ecological degradation, lithium-ion batteries, with their excellent energy density and environmentally friendly characteristics, have become an indispensable core technology in the modern energy storage field. Graphite is currently the most widely used anode material in commercially available lithium-ion batteries, but its theoretical specific capacity is only 372 mAh / g, which is insufficient to meet the development needs of high-energy-density energy storage devices. Furthermore, the small interlayer spacing of graphite restricts lithium-ion diffusion kinetics under fast-charging conditions, easily leading to lithium precipitation and deposition, posing serious safety hazards. Rate performance and safety in use still need further improvement. Therefore, the development of new high-capacity, high-rate lithium-ion battery anode materials is of great practical significance.
[0003] Metal-organic framework (MOF)-derived carbon aerogels inherit the structural advantages of MOF materials, possessing high specific surface area, hierarchical porous structure, and a stable and continuous three-dimensional carbon network framework. When used as a negative electrode in lithium-ion batteries, they exhibit high reversible capacity and excellent cycle stability. Compared to traditional graphite anodes, MOF-derived carbon aerogels have larger interlayer spacing and pore size, which is beneficial for lithium-ion transport. Their stable framework structure also enables long-term cycling. However, these materials still have significant drawbacks: firstly, their intrinsic conductivity is insufficient; secondly, their high specific surface area results in a large number of active interfaces, making them prone to excessive interfacial side reactions when in contact with the electrolyte, causing severe irreversible lithium loss. This leads to low initial coulombic efficiency, limiting further improvement in rate performance and cycle stability, and restricting the practical application of MOF-derived carbon aerogels in lithium-ion battery anodes.
[0004] While existing technologies utilize zinc oxide to coat and modify carbon-based anode materials, these studies primarily focus on conventional carbon substrates such as graphite, graphene aerogels, and phenolic carbon aerogels. The pore structure, surface defect levels, and interfacial chemical states of these conventional carbon substrates differ significantly from those of MOF-derived carbon aerogels. Conventional carbon substrates do not exhibit the severe interfacial side reaction problems caused by their ultra-high specific surface area and numerous intrinsic carbon defects. Current research on zinc oxide coating modification mainly focuses on improving the overall conductivity of the material or increasing the lithium storage active sites of the electrode. The improvement goal is not to address the inherent shortcomings of MOF-derived carbon aerogel materials, such as excessively high irreversible lithium loss and low first-pass coulombic efficiency. While MOF-derived carbon aerogels possess hierarchical porous structures and continuous three-dimensional conductive networks, exhibiting high lithium storage capacity potential, their high specific surface area and numerous carbon skeleton defects, stemming from MOF precursors, make them prone to continuous and intense interfacial side reactions during electrode-electrolyte contact. This results in the irreversible consumption of a large amount of lithium source, directly reducing the initial coulombic efficiency. This problem is a unique technical bottleneck for this type of material.
[0005] Directly applying zinc oxide coating processes designed for ordinary carbon substrates to MOF-derived carbon aerogels is problematic due to the material's high activity, fragile framework, and intricate pore structure. This can easily lead to zinc oxide particle agglomeration, clogging of internal micropores and mesopores, and disruption of the original three-dimensional porous framework. Consequently, it can impair the material's lithium-ion transport capacity, failing to achieve the modification goals of suppressing interfacial side reactions and reducing irreversible lithium loss. Therefore, developing modification methods adapted to MOF-derived carbon aerogels, precisely controlling their electrode-electrolyte interface behavior, effectively suppressing side reactions, reducing irreversible lithium loss, and simultaneously improving the material's initial coulombic efficiency, rate performance, and long-term cycling stability are pressing technical challenges that need to be overcome in this field. Summary of the Invention
[0006] The purpose of this invention is to provide a method for preparing zinc oxide-coated MOFs-derived carbon aerogel and its application in the negative electrode of lithium-ion batteries, so as to solve the problems existing in the prior art.
[0007] To achieve the above objectives, the present invention provides the following solution: One of the technical solutions of this invention provides a method for preparing zinc oxide-coated MOFs-derived carbon aerogels, comprising the following steps: (1) Disperse MOFs-derived carbon aerogel in an aqueous solution of zinc chloride, adjust the pH of the resulting dispersion system to 7-8, generate zinc hydroxide in situ and coat the surface of the MOFs-derived carbon aerogel, and after separation, washing and drying, obtain zinc hydroxide-coated MOFs-derived carbon aerogel precursor. (2) The zinc hydroxide-coated MOFs-derived carbon aerogel precursor is calcined under a protective atmosphere to achieve the pyrolysis of zinc hydroxide into zinc oxide, thereby obtaining the zinc oxide-coated MOFs-derived carbon aerogel.
[0008] The MOFs-derived carbon aerogel of the present invention is a three-dimensional porous carbon aerogel material obtained by carbonization of MOFs.
[0009] Furthermore, the zinc content in the zinc oxide-coated MOFs-derived carbon aerogel is 5% by mass.
[0010] Furthermore, the pH value of the dispersion system is adjusted using ammonia.
[0011] Furthermore, in step (2), the calcination temperature is 250-350℃ and the time is 1-3h.
[0012] Further, the temperature is increased to the calcination temperature at a heating rate of 3-8°C / min.
[0013] Furthermore, the drying process employs vacuum drying.
[0014] The second technical solution of the present invention provides zinc oxide-coated MOFs-derived carbon aerogel prepared by the above preparation method.
[0015] The third technical solution of this invention provides the application of the above-mentioned zinc oxide-coated MOFs-derived carbon aerogel as a negative electrode material for lithium-ion batteries.
[0016] The fourth technical solution of the present invention provides a lithium-ion battery that uses the above-mentioned zinc oxide-coated MOFs-derived carbon aerogel as the negative electrode.
[0017] The present invention discloses the following technical effects: This invention provides a zinc oxide-coated MOF-derived carbon aerogel, achieving the coating modification of zinc oxide nanoparticles on the surface of the carbon aerogel framework. The zinc oxide nanoparticles are uniformly anchored on the carbon sheet surface and the inner walls of the pores. This material completely preserves the three-dimensional cross-linked hierarchical porous framework of the carbon aerogel, constructing a continuous and interconnected conductive network. The loose and porous structure of the carbon aerogel can provide a large number of active sites and shorten the ion transport distance. The zinc oxide coating on the surface further increases the number of active sites, fully utilizing the inherent functional properties of zinc oxide.
[0018] The aerogel material provided by this invention synergistically combines the excellent conductivity of MOFs-derived carbon aerogels with the functional advantages of zinc oxide. It also features a porous structure, high conductivity, and abundant active sites. The preparation method is simple, and it has good application prospects in electrochemical energy storage, adsorption, catalysis and other fields. Attached Figure Description
[0019] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0020] Figure 1 The image shows a SEM image of the zinc oxide-coated MOFs-derived carbon aerogel composite material prepared in Example 1.
[0021] Figure 2 The graphs show the electrochemical performance of the coin cell; (a) is the cyclic voltammetry curve, (b) is the electrochemical impedance spectroscopy, (c) is the rate charge-discharge performance curve, and (d) is the long-cycle charge-discharge performance curve. Detailed Implementation
[0022] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0023] It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the invention. Furthermore, with respect to numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Any stated value or intermediate value within a stated range, as well as each smaller range between any other stated value or intermediate value within said range, is also included in this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.
[0024] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this invention. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.
[0025] Various modifications and variations can be made to the specific embodiments described in this specification without departing from the scope or spirit of the invention, as will be apparent to those skilled in the art. Other embodiments derived from this specification will also be readily apparent to those skilled in the art. This specification and embodiments are merely exemplary.
[0026] The terms “include,” “including,” “have,” “contain,” etc., used in this article are all open-ended terms, meaning that they include but are not limited to.
[0027] It should be noted that any aspects not described in detail in this invention are conventional practices in the field and are not the focus of this invention.
[0028] The MOFs-derived carbon aerogels used in the following embodiments of the present invention were purchased from Suzhou Maofushi Technology Co., Ltd.
[0029] Example 1 This embodiment provides a zinc oxide-coated MOFs-derived carbon aerogel, and the preparation steps are as follows: (1) Preparation of zinc hydroxide-coated MOFs-derived carbon aerogels: Weigh 0.2 g of MOFs-derived carbon aerogel; dissolve 0.0427 g of anhydrous zinc dichloride in 5 mL of deionized water to prepare a zinc salt solution; The MOFs-derived carbon aerogel was added to the zinc salt solution and stirred at room temperature for 30 min to fully disperse the carbon aerogel. Ammonia was slowly added dropwise while stirring continuously to adjust the pH of the system to 7, so that zinc chloride was converted into zinc hydroxide in situ and coated on the surface of the MOFs-derived carbon aerogel. After stirring for another 30 min, the product was washed with deionized water and then vacuum dried at 60 °C for 12 h to obtain zinc hydroxide-coated MOFs-derived carbon aerogel precursor powder.
[0030] (2) Preparation of zinc oxide-coated MOFs-derived carbon aerogels: The precursor powder obtained above was placed in a tube furnace and heated to 300°C at a heating rate of 5°C / min under a nitrogen protective atmosphere. The temperature was then maintained for 2 h to allow zinc hydroxide to pyrolyze into zinc oxide. The mixture was then naturally cooled to room temperature to obtain a zinc oxide-coated MOFs-derived carbon aerogel composite material with a zinc element mass fraction of 5%.
[0031] Figure 1 This is a SEM image of the zinc oxide-coated MOFs-derived carbon aerogel composite material prepared in Example 1. Figure 1 It can be seen that the material retains the hierarchical porous framework structure of the three-dimensional cross-linking of carbon aerogel, and the framework overlaps to form a continuous conductive network; the zinc oxide nanoparticles are uniformly dispersed and attached to the surface of the carbon sheet and the inner wall of the pores, without obvious large-scale agglomeration and clumping, and the overall loose and porous composite micromorphology is maintained.
[0032] Preparation of negative electrode sheet for lithium-ion battery and assembly of coin cell half-cell: (1) Preparation of negative electrode slurry and electrode sheet: The zinc oxide-coated MOFs-derived carbon aerogel composite material, binder (CMC to SBR mass ratio of 2:1), and superconducting carbon black prepared in this embodiment were mixed at a mass ratio of 68:22:10 to obtain a negative electrode slurry; the negative electrode slurry was uniformly coated onto a copper foil current collector using a coater, and dried in a vacuum oven at 120 ℃ for 12 h. After drying, a negative electrode sheet with a diameter of 13 mm was obtained. At the same time, the original MOFs-derived carbon aerogel (i.e., unmodified MOFs-derived carbon aerogel) without zinc oxide coating treatment was used as the active material, and the same slurry ratio, coating, drying, and cutting process was used to prepare the control group negative electrode sheet for assembling the control group coin half cell.
[0033] (2) Assembly of coin cell: The cut negative electrode sheet was used as the working electrode, the PP separator as the separating membrane, and the lithium metal sheet as the counter electrode. The electrolyte was a 1.0 mol / L lithium hexafluorophosphate (LiPF6) solution, with a solvent consisting of a 1:1:1 volume ratio of ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC). 10.0% fluoroethylene carbonate (FEC) and 1.0% ethylene carbonate (VC) were added to the electrolyte as functional additives. The coin cell assembly was completed in a glove box filled with high-purity argon. The control group coin cell used the negative electrode sheet prepared above, with the original MOFs-derived carbon aerogel as the active material, as the working electrode. The separator, counter electrode, electrolyte, and assembly conditions were completely consistent with the aforementioned coin cell.
[0034] All electrochemical tests in this embodiment were conducted on the assembled coin half-cell. Except for the working electrode active material, which was respectively zinc oxide-coated MOFs-derived carbon aerogel and unmodified MOFs-derived carbon aerogel prepared in this invention, the other battery components such as the separator, counter electrode, and electrolyte were kept completely identical to characterize the electrochemical performance of the active material itself. The separator, electrolyte, and lithium metal counter electrode were only used as test systems and were not improvements of this invention.
[0035] The electrochemical performance of coin half-cells assembled from zinc oxide-coated MOFs-derived carbon aerogel samples prepared in Example 1 was tested at room temperature using the Shanghai Chenhua Electrochemical Workstation and the Blue Battery Testing System.
[0036] Figure 2 The graphs show the electrochemical performance of the coin cell; (a) is the cyclic voltammetry curve, (b) is the electrochemical impedance spectroscopy, (c) is the rate charge-discharge performance curve, and (d) is the long-cycle charge-discharge performance curve.
[0037] Cyclic voltammetry (CV) tests were performed on zinc oxide-coated MOF-derived carbon aerogels using a Shanghai Chenhua CHI660E electrochemical workstation at a scan rate of 0.1 mV / s. The test results are as follows: Figure 2 As shown in (a), an irreversible process occurred at the electrode during the first scan, which mainly originated from the formation of the SEI film and the decomposition of the electrolyte. The subsequent second and third scan curves showed almost no significant difference, indicating that the composite material has good electrode reaction reversibility and cycle stability.
[0038] Electrochemical impedance spectroscopy (EIS) was performed using a Shanghai Chenhua CHI660E electrochemical workstation. The test results are as follows: Figure 2 As shown in (b), the smaller diameter of the charge transfer semicircle corresponding to this composite material indicates that the charge transfer impedance of the electrode is effectively reduced and the interfacial charge transport dynamics are improved after zinc oxide coating modification. The impedance spectrum shows a steeply sloping straight line in the low-frequency region, demonstrating that the three-dimensional porous framework structure is conducive to lithium ion migration and diffusion. This further proves that the zinc oxide-coated composite structure obtained in this invention can accelerate the transfer of ions and charges inside the electrode and play a positive role in improving the electrochemical performance of the material.
[0039] Rate charge-discharge tests were conducted, and comparative tests were performed on coin half-cells equipped with zinc oxide-coated MOFs-derived carbon aerogel and unmodified MOFs-derived carbon aerogel. The test results are as follows: Figure 2 As shown in (c), both coin cells exhibited high initial discharge specific capacity during the first discharge cycle; the coin cell equipped with unmodified MOFs-derived carbon aerogel had a first-cycle discharge specific capacity of 2970.45 mAh·g. -1 The coin half-cell equipped with zinc oxide-coated MOFs-derived carbon aerogel exhibited a first-round discharge specific capacity of 3124.32 mAh·g. -1 The irreversible capacity generated in the first cycle mainly comes from the formation of the SEI film and the decomposition of the electrolyte. During the test, the discharge specific capacity of both coin cells decreased to some extent under high-rate conditions. However, the coin cell equipped with zinc oxide-coated MOFs-derived carbon aerogel had a higher discharge specific capacity than the coin cell equipped with unmodified MOFs-derived carbon aerogel throughout the entire test rate range. Under 5C high-current charge-discharge conditions, the coin cell equipped with zinc oxide-coated MOFs-derived carbon aerogel could output approximately 850 mAh·g. -1 The reversible capacity of the coin half-cell equipped with unmodified MOFs-derived carbon aerogel is only about 700 mAh·g. -1 The reversible capacity; when the charge / discharge current returns to 0.1C, the coin cell equipped with zinc oxide-coated MOFs-derived carbon aerogel can still output approximately 1900 mAh·g. -1The reversible capacity. The above test results show that the MOFs-derived carbon aerogel modified with zinc oxide coating can still maintain its structural integrity after high current charge and discharge, thus giving the coin cell excellent rate performance.
[0040] Long-cycle charge-discharge tests were conducted on coin cells equipped with two different types of electrodes at a 0.5C rate. The test results are as follows: Figure 2 As shown in (d), both materials exhibited high initial discharge specific capacity in the first cycle, with the zinc oxide-coated MOFs-derived carbon aerogel achieving a first-cycle discharge specific capacity of 3000 mAh·g. -1 The first-cycle discharge specific capacity of the unmodified MOFs-derived carbon aerogel is approximately 2900 mAh·g. -1 The initial coulombic efficiency of zinc oxide-coated MOFs-derived carbon aerogel reached 85.78%, while that of unmodified MOFs-derived carbon aerogel was only 67.39%. During subsequent cycles, the zinc oxide-coated MOFs-derived carbon aerogel consistently maintained a higher reversible capacity. These test results demonstrate that zinc oxide coating modification can effectively improve the initial coulombic efficiency of MOFs-derived carbon aerogel, while also enhancing the reversible capacity of the electrode.
[0041] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.
Claims
1. A method for preparing zinc oxide-coated MOFs-derived carbon aerogel, characterized in that, Includes the following steps: (1) Disperse MOFs-derived carbon aerogel in an aqueous solution of zinc chloride, adjust the pH of the resulting dispersion system to 7-8, generate zinc hydroxide in situ and coat the surface of the MOFs-derived carbon aerogel, and after separation, washing and drying, obtain zinc hydroxide-coated MOFs-derived carbon aerogel precursor. (2) The zinc hydroxide-coated MOFs-derived carbon aerogel precursor is calcined under a protective atmosphere to achieve the pyrolysis of zinc hydroxide into zinc oxide, thereby obtaining the zinc oxide-coated MOFs-derived carbon aerogel.
2. The preparation method according to claim 1, characterized in that, The zinc content in the zinc oxide-coated MOFs-derived carbon aerogel is 5%.
3. The preparation method according to claim 1, characterized in that, The pH value of the dispersion system was adjusted using ammonia.
4. The preparation method according to claim 1, characterized in that, In step (2), the calcination temperature is 250~350℃ and the time is 1~3h.
5. The preparation method according to claim 4, characterized in that, The temperature is increased to the calcination temperature at a heating rate of 3~8℃ / min.
6. The preparation method according to claim 1, characterized in that, The drying process employs vacuum drying.
7. Zinc oxide-coated MOFs-derived carbon aerogel prepared by the preparation method according to any one of claims 1-6.
8. The application of zinc oxide-coated MOFs-derived carbon aerogel as described in claim 7 as a negative electrode material for lithium-ion batteries.
9. A lithium-ion battery, characterized in that, The zinc oxide-coated MOFs-derived carbon aerogel described in claim 7 is used as the negative electrode.