A method for preparing large-size optical fiber preforms
By employing specific hydrogen-oxygen flow rate fusion splicing, silicon nitride windshield deposition, and vertical sintering processes, the problems of fusion zone strength, deposition efficiency, and sintering defects in large-size optical fiber preforms were solved, enabling the stable fabrication of high-quality, long-distance optical fiber preforms that meet communication optical fiber standards.
Patent Information
- Application Number
- CN202611410336.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-11
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies are difficult to stably prepare ultra-large optical fiber preforms, and there are problems such as low strength of the fusion splice zone, low deposition efficiency, easy generation of defects in the sintering process, and uneven optical performance, which lead to unstable optical fiber performance.
The core rod and seed rod are fused using a horizontal flame device with specific hydrogen and oxygen flow rates. The outer cladding is deposited using a blowtorch windproof cover made of silicon nitride. High strength, uniformity and optical performance are controlled by a vertical sintering process combined with dehydration, stepped heating and slow cooling annealing.
It has achieved the preparation of high-strength, uniform and long-distance drawn optical fiber preforms, ensuring the consistency of optical performance and efficient production, and meeting the G.652.D standard.
Smart Images

Figure CN123105969A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of optical fiber manufacturing technology, and in particular to a method for preparing large-size optical fiber preforms. Background Technology
[0002] Optical fiber preforms are the matrix for manufacturing communication optical fibers, and their size, quality, and manufacturing efficiency directly determine the production cost and performance of the optical fiber. With the explosive growth of global data traffic, especially the advancement of 5G, data centers, and the "East-to-West Data Transfer" project, the market demand for optical fibers continues to rise, which places higher demands on the large-scale, low-cost, and high-quality manufacturing of optical fiber preforms.
[0003] Currently, the mainstream optical fiber preform fabrication technologies in the industry mainly include in-tube chemical vapor deposition (such as MCVD and PCVD) and out-of-tube vapor deposition (such as VAD and OVD). To increase the drawing length of a single preform and reduce unit cost, the fabrication of large-size preforms has become a clear technological development direction. However, in the process of significantly increasing the size of preforms (especially their diameter), existing technologies generally suffer from the following technical problems:
[0004] 1. As the size of the preform increases, the size and weight of its core rod (as the deposition substrate) also increase accordingly. After the core rod is prepared using methods such as VAD, it needs to be welded to the end handle to facilitate clamping and rotation in subsequent processes. Traditional welding processes, for large-sized, high-purity core rods, struggle to ensure the strength of the weld zone while effectively preventing impurity contamination or thermal stress concentration caused by uneven high-temperature heating. This area is prone to becoming a weak point in subsequent deposition and wire drawing.
[0005] 2. In current technologies, when using multi-torch chemical vapor deposition (CVD) equipment for cladding deposition, the large-sized mandrel results in a significant increase in the deposition surface area. If the deposition process parameters are not matched with the equipment configuration, it can lead to low deposition efficiency and uneven density and poor porosity distribution in the deposited SiO2 loose body. Temperature field control at the edge of the deposition area is particularly critical. If the torch shield material is not heat-resistant or has uneven heat conduction, it will disturb the flame flow field, directly affecting the uniformity and density of the particle deposition, creating potential problems for subsequent sintering.
[0006] 3. Sintering large-sized loose preforms presents a significant technical challenge. Improper control of the heating rate, holding temperature, and time during the dehydration and vitrification processes can easily lead to defects such as macroscopic cracks and microscopic bubbles due to uneven internal stress release or poor gas expulsion. Furthermore, controlling the radial uniform shrinkage of large preforms from a loose to a dense glassy state during sintering is difficult, easily resulting in poor roundness and large diameter fluctuations in the final preform, affecting the stability of the fiber drawing process and the consistency of optical fiber geometry.
[0007] 4. Traditional fabrication methods often rely on random sampling to inspect the optical properties of the final preform (such as cutoff wavelength, dispersion, and mode field diameter), lacking a closed-loop control system that is strongly correlated with the fabrication process parameters. For large-size preforms, even minute defects in any region can lead to fiber breakage or performance degradation during long-distance fiber drawing. Therefore, more precise and comprehensive optical testing is needed to ensure that the uniformity of performance along its entire length meets stringent standards such as G.652.D.
[0008] In summary, there is currently a lack of a complete, controllable, and industrialized method for the stable fabrication of ultra-large-sized, high-performance optical fiber preforms suitable for ultra-long-distance fiber drawing. Summary of the Invention
[0009] The technical solution adopted by the present invention to solve the above-mentioned technical problems is as follows:
[0010] A method for fabricating a large-size optical fiber preform includes the following steps:
[0011] S1. Mandrel preparation and welding: The mandrel and the end seed rod are welded together using a horizontal glass lathe.
[0012] S2, Outer cladding deposition: Using a multi-torch longitudinal chemical vapor deposition equipment, SiO2 particles are deposited on the outside of the mandrel obtained in step S1 to form a porous body;
[0013] S3, Vertical sintering: The loose body obtained in step S2 is placed in a vertical sintering furnace for dehydration and vitrification sintering to obtain a dense optical fiber preform.
[0014] S4. Optical testing: Perform optical property testing on the optical fiber preform obtained in step S3.
[0015] Furthermore, in step S1, the hydrogen flow rate of the torch in the horizontal flame device is controlled at 200L / min to 300L / min, and the oxygen flow rate is controlled at 55L / min to 80L / min.
[0016] Furthermore, in step S2, the material of the blower wind shield of the multi-blower longitudinal chemical vapor deposition equipment is silicon nitride.
[0017] Furthermore, in step S2, the overall deposition efficiency of the deposition equipment is controlled to be 110~200g / min, and the outer diameter of the loose body formed by deposition is 310mm~460mm.
[0018] Furthermore, step S3 specifically includes the following steps:
[0019] S31, Dehydration stage: The loose material is kept at 1280℃ for 2-4 hours to remove hydroxyl groups;
[0020] S32, Sintering and densification stage: The loose body that has completed the dehydration stage is heated from 1280℃ to above 1500℃ at a rate of 3-5℃ / min, and held at 1340℃ and 1440℃ for 0.5 hours respectively during the heating process;
[0021] S33. Cooling and annealing stage: After the sintered preform is cooled to 800℃ at a rate of 1-2℃ / min, it is allowed to cool naturally.
[0022] Furthermore, in step S32, the loose body is controlled to shrink uniformly from a diameter of 310mm~460mm to 140mm~180mm.
[0023] Furthermore, in step S4, the optical characteristic test includes at least: testing the cutoff wavelength of the optical fiber preform, the dispersion in the 1285nm band, and the mode field diameter.
[0024] Furthermore, the single-strand drawing length of the optical fiber preform prepared according to this method is 2000~5000km.
[0025] Furthermore, the diameter of the optical fiber preform prepared according to this method is 140mm~180mm.
[0026] The advantages of this invention are:
[0027] 1. This invention solves the technical problems of low strength and easy introduction of thermal stress and contamination in the fusion zone of large-sized core rods by using a horizontal flame device with specific hydrogen flow rates (200L / min~300L / min) and oxygen flow rates (55L / min~80L / min) for the fusion of core rods and seed rods. The precisely controlled flame parameters can create a stable and pure high-temperature field locally, achieving rapid and complete melting and bonding of the core rod and seed rod, forming a high-strength, low-defect fusion zone. This provides a reliable mechanical basis for subsequent high-speed rotary deposition of large-sized loose bodies.
[0028] 2. This invention solves the technical problems of low deposition efficiency and poor uniformity and density of the deposited layer in large-size preforms by using a silicon nitride blower shield in a multi-blower longitudinal chemical vapor deposition (CVD) system and controlling the overall deposition efficiency to 110-200 g / min. Silicon nitride material possesses excellent high-temperature stability and wear resistance, effectively stabilizing the blower flame flow field and reducing turbulence. Combined with the optimized deposition efficiency, SiO2 particles can be deposited on the mandrel surface at a high rate and with high uniformity, forming a giant loose body with an outer diameter of 310 mm-460 mm, a dense interlayer structure, and uniform pore distribution, laying the structural foundation for obtaining a high-quality sintered body.
[0029] 3. This invention solves the technical problems of cracking, bubble formation, and uneven shrinkage during the sintering of large-sized loose materials by employing a vertical sintering process that includes specific dehydration, stepped heating sintering, and slow cooling annealing stages, and by controlling the uniform shrinkage of the loose material from 310mm~460mm to 140mm~180mm. Thorough dehydration at 1280℃ effectively removes hydroxyl groups, avoiding water peak loss. Subsequent heating at a rate of 3-5℃ / min, with segmented holding at 1340℃ and 1440℃, allows the loose material to gradually and uniformly complete the glass transition, ensuring the orderly expulsion of internal gases and preventing defects. Precise radial shrinkage control combined with final slow cooling annealing (cooling down to 800℃ at 1-2℃ / min) ensures that the final preform has extremely high diameter accuracy (140mm~180mm), excellent roundness, and a uniform glassy structure, reducing internal defects. Attached Figure Description
[0030] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0031] Figure 1 This is a schematic diagram of the mandrel structure.
[0032] Figure 2 This is a schematic diagram of a loose body structure.
[0033] Figure 3 This is a diagram showing the refractive index distribution.
[0034] Among them: 1. core rod; 2. A-end quartz rod; 3. B-end quartz rod; 4. B-end seed rod. Detailed Implementation
[0035] The technical solution of the present invention will now be clearly and completely described with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0036] Example 1:
[0037] The specific embodiments of the present invention will be described in detail below. It should be understood that the described embodiments are merely some, not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention. The embodiments of the present invention provide an industrial-scale preparation method for large-size optical fiber preforms, aiming to solve a series of bottleneck problems encountered by existing methods mentioned in the background art when preparing ultra-large-size (e.g., diameter up to 180mm) preforms, such as poor fusion splicing reliability, low deposition efficiency and uniformity, easy generation of defects in the sintering process, and difficulty in ensuring product performance consistency. This method, through precise and coordinated process steps and key parameter control, achieves stable and efficient preparation of ultra-large-size, ultra-high uniformity, and ultra-long drawn fiber preforms.
[0038] The purpose of this method is to prepare high-quality optical fiber preforms for communication with a diameter of 140mm~180mm, a single-strand drawing length of 2000km~5000km, and optical performance that fully meets standards such as G.652.D. The method mainly includes four core steps, which together constitute a complete process chain:
[0039] Step S1: Mandrel preparation and welding -> Step S2: Outer cladding deposition -> Step S3: Vertical sintering -> Step S4: Optical inspection.
[0040] The following will elaborate on the specific implementation methods, equipment selection, process parameters, and principles of each step.
[0041] Step S1: Mandrel preparation and welding
[0042] The goal of this step is to provide a high-quality, high-strength support substrate for subsequent cladding deposition, namely a mandrel with a pre-designed refractive index profile, and to reliably weld it to a seed rod used for equipment clamping and rotation. For a final preform with a target diameter of 180 mm, the mandrel diameter is typically increased accordingly, with a mass reaching tens of kilograms. The welded area (joint) must possess mechanical strength close to that of the base material, extremely high purity, and must not break or become a source of contamination during subsequent high-speed rotation and high-temperature processing. Traditional welding processes suffer from unstable flames and uneven thermal fields, easily leading to bubbles, microcracks, or impurity accumulation in the welded area, becoming weak points in the overall preform structure. In this process, the mandrel and seed rod are prepared using the industry-standard VAD (axial vapor deposition) method to produce a mandrel that meets the design requirements. This mandrel has a precise refractive index profile, and its ends are ground and polished, resulting in a smooth and clean end face. The seed rod is made of high-purity synthetic quartz glass, with a diameter and strength sufficient to support the weight of the large-sized final product. A dedicated horizontal flame welding device is used. The core of this equipment is a hydrogen-oxygen burner (blowtorch) with precisely controllable flow rate and mixing ratio. The blowtorch and its support mechanism can move horizontally (laterally) to provide annular heating at the joint between the vertically clamped mandrel and the seed rod. The mandrel and seed rod are aligned coaxially on the equipment, with their end faces in slight contact. The blowtorch is activated, and the hydrogen flow rate is precisely controlled at 200 L / min ~ 300 L / min, and the oxygen flow rate at 55 L / min ~ 80 L / min. This specific flow ratio results in a neutral or slightly reducing flame, with a flame temperature reaching approximately 2800°C, sufficient to rapidly and fully melt quartz glass (SiO2, melting point approximately 1700°C). The high hydrogen flow rate ensures sufficient heat input to handle the large heat capacity of the mandrel, allowing the entire joint area to reach the melting temperature uniformly and avoiding uneven heating. The precisely controlled oxygen flow rate (55 L / min ~ 80 L / min) ensures complete hydrogen combustion, resulting in a straight, stable flame with minimal disturbance. An overly oxygen-rich flame may introduce excessive reactive oxygen, adversely affecting the chemical composition of high-purity quartz; an overly combustible flame may produce soot (carbon particle) pollution due to incomplete combustion. The flame under these parameters is chemically pure, introducing virtually no foreign impurities. A stable, uniform high-temperature field allows the weld zone to melt and resolidify synchronously and uniformly from the inside out, greatly reducing quenching stress caused by temperature differences and effectively preventing microcracks from forming in the weld zone after cooling. The torch is slowly moved laterally along the joint several times to ensure the entire annular joint surface is uniformly heated, melted, and diffused together. Small axial pressure can be applied during the welding process to promote interface fusion. After welding, the weld is slowly cooled to room temperature in a controlled cooling environment (such as in an annealing furnace) to eliminate residual thermal stress.
[0043] The above process can produce a high-quality mandrel-seed rod composite with high joint strength, no visible defects, and low impurity content. This provides a reliable mechanical basis for the loose outer cladding in subsequent steps and for withstanding the centrifugal force of high-speed rotation, eliminating the risk of scrapping the entire expensive preform due to failure of the weld zone.
[0044] Step S2: Deposition of the outer cladding layer
[0045] The goal of this step is to deposit a loose body of SiO2 particles with uniform thickness and consistent pore structure onto the exterior of the high-strength mandrel prepared in step S1. Specifically, a VAD (External Vapor Deposition) chemical vapor deposition process is used, with a longitudinal device to coat the prepared mandrel with SiO2 particles layer by layer. Multiple main torches work together, achieving a deposition rate of 12-20 g / min per torch, an equipment deposition efficiency of 110-200 g / min, and an absorption rate of 50%-70% to form a loose body with an outer diameter of approximately 310-460 mm. Further, the deposition equipment is a multi-torch longitudinal chemical vapor deposition device, i.e., an OVD (External Vapor Deposition) lathe. The mandrel-seed rod composite is horizontally clamped and rotated at high speed on the spindle, with multiple torches arranged below the mandrel, reciprocating along the mandrel's axial direction. The torches mix and spray a mixture of high-purity SiCl4 (silicon tetrachloride) vapor, fuel gas (such as hydrogen or methane), and carrier / combustion-supporting gas (such as oxygen or air). In the flame, SiCl4 undergoes hydrolysis or oxidation to generate extremely fine SiO2 particles. In this invention, the wind shield around the torch flame outlet is made of silicon nitride. Silicon nitride has a long-term operating temperature exceeding 1650°C and exhibits almost no oxidation, creep, or deformation in the high-temperature environment near the torch flame, maintaining geometric stability over a long period. Furthermore, its moderate thermal conductivity and low coefficient of thermal expansion allow it to withstand the severe thermal shock caused by frequent torch start-ups and power changes without cracking. The smooth, high-temperature-resistant silicon nitride inner wall provides a stable and undisturbed flow path for the ejected high-temperature mixed gas. This effectively isolates it from external air turbulence, maintaining a high degree of stability in flame shape, length, and temperature distribution. The deposition efficiency of 110~200 g / min of the equipment in this invention, combined with the stable thermal field of the silicon nitride wind shield, allows SiO2 particles to impact and adhere to the mandrel surface at appropriate humidity and velocity, accumulating layer by layer to ultimately form a cylindrical loose body with an outer diameter controlled between 310 mm and 460 mm. This loose body has a porous internal structure with good bonding between layers and a uniform density distribution. By using a silicon nitride wind shield to stabilize the flame field and combining it with an optimized deposition efficiency of 110~200g / min, this invention can successfully prepare SiO2 loose bodies with precise dimensions (Φ310~460mm), minimal axial and radial density fluctuations, no hard agglomerates, and a uniform pore structure.
[0046] Step S3: Vertical sintering
[0047] The purpose of this step is to transform the porous SiO2 loose material obtained in step S2 into a completely dense, transparent glassy optical fiber preform, and to control its diameter to shrink uniformly from 310mm~460mm to a final size of 140mm~180mm. Specifically, sintering is carried out in a dedicated vertical sintering furnace. The loose material with an outer diameter of 310mm~460mm is vertically suspended in the center of the furnace to facilitate symmetrical thermal field and uniform shrinkage under gravity. The sintering process is strictly divided into three stages:
[0048] Stage S31: Dehydration Stage
[0049] The furnace temperature was raised to 1280°C at a slow rate (e.g., 5-10°C / min) and held at this temperature for 2 hours. The loose material contained a large number of hydroxyl groups (-OH) in the form of Si-OH. Since hydroxyl groups are the source of the 1383nm water peak loss in optical fibers, they must be completely removed before glassization. The temperature of 1280°C is higher than the strain point of quartz glass, and the material begins to exhibit viscous flow, with the pores slowly closing, but not yet fully glassized. Holding at this temperature for 2 hours, under a chlorine / inert atmosphere, ensured the removal of hydroxyl groups from the loose material through diffusion and chemical reaction (≡Si-OH + Cl2 → ≡Si-Cl + HCl↑), achieving sufficient dehydration.
[0050] Stage S32: Sintering densification stage
[0051] After dehydration, the temperature is slowly increased from 1280°C to above 1500°C (e.g., 1520-1550°C) at a rate of 3-5°C / min. During the heating process, the temperature is paused at two specific points: 1340°C and 1440°C, and held for 0.5 hours at each point. The entire heating process is conducted in a pure helium or vacuum environment. Due to the temperature gradient between the inside and outside of large objects, excessively rapid heating would cause the outer layer to vitrify and seal the pores, preventing the gas generated inside from escaping and forming large bubbles. Slow heating keeps the internal and external temperatures as synchronized as possible, allowing time for the orderly diffusion and expulsion of gas. Holding at 1340°C, slightly above the annealing point of quartz glass, further reduces the material's viscosity, initiating significant viscous flow and pore shrinkage. Holding for 0.5 hours allows the loose material to undergo a preliminary, gradual densification at a lower viscosity, turning most open pores into closed pores, but not completely closing them. Holding at 1440°C results in higher viscosity and accelerated shrinkage. Holding for 0.5 hours further promotes the continued shrinkage and spheroidization of remaining closed pores under surface tension, dissolving into the glass network during this process (or being expelled through the high diffusivity of helium). Holding at these two temperature steps avoids the drastic and uneven shrinkage caused by a rapid decrease in viscosity due to a continuous and rapid temperature rise, thus effectively preventing the formation of cracks and microbubble clusters. Through the above steps, combined with the highly uniform radial thermal field within the vertical furnace, the loose material, driven by surface tension and viscous flow, shrinks uniformly and synchronously towards the center along a radial path starting from an outer diameter of 310mm~460mm. Throughout the process, the diameter of the preform is monitored in real time (using a high-temperature diameter gauge), and feedback control is achieved through fine-tuning the furnace temperature distribution to ensure a final diameter of 140mm~180mm, with a small taper and excellent roundness.
[0052] Stage S33: Cooling and Annealing Stage
[0053] Once the temperature reaches above 1500°C and is briefly homogenized to ensure complete vitrification and the absence of residual pores, programmed cooling begins. First, the preform is cooled from the sintering temperature to 800°C at a controlled rate of 1-2°C / min. Then, the heating power is cut off, allowing the preform to cool naturally to room temperature within the furnace. When quartz glass cools from a high temperature, the difference in cooling rates between the inside and outside creates permanent thermal stress (tempering stress). Slow cooling at 1-2°C / min allows the preform to pass through the glass's strain point and transition temperature range at a gradual rate, starting from a temperature above the annealing point, thus eliminating thermal stress and creating a low-stress state inside the preform. This low-stress preform deforms more stably when reheated in the drawing furnace, resulting in stronger drawn optical fibers. After cooling to below 800°C, the glass structure is essentially frozen and can be safely allowed to cool naturally. This invention transforms a giant porous loose body into an optical fiber preform with a diameter of 140mm~180mm, complete transparency, no visible cracks or bubbles, extremely low internal stress, and uniform glass transition height through a vertical sintering process of full dehydration-step heating sintering-velocity annealing.
[0054] Step S4: Optical Inspection
[0055] Test samples are prepared from sintered preforms through grinding and polishing, or by directly scanning the end faces of the preforms. Key testing items include:
[0056] Cutoff wavelength test: Ensure single-mode transmission characteristics. By measuring the refractive index profile of the preform or by actual measurement through drawing a short section of optical fiber, the cutoff wavelength is controlled within the range of 1190~1330nm, and its cutoff wavelength must meet the requirements of the G.652.D standard.
[0057] 1285nm Dispersion Test: Dispersion is a key parameter affecting high-speed transmission. The dispersion coefficient of the preform in the 1285nm window needs to be tested to ensure that it is within the range specified in the standard (e.g., close to zero dispersion wavelength).
[0058] Mode field diameter test: The mode field diameter is an important parameter for the coupling of optical fiber with light source and connector. It is necessary to measure the mode field diameter at a wavelength of 1310nm to ensure that it meets the standard specifications.
[0059] This step involves comprehensive optical performance testing of the preform produced in step S3 to quantitatively verify the quality of its internal waveguide structure and ensure its suitability for manufacturing communication optical fibers conforming to the G.652.D standard. Optical testing is a crucial part of closed-loop quality control, serving not only as acceptance testing for the final product but also providing data feedback to the front-end core preparation (S1 front-end process) and deposition process optimization. Only products that simultaneously meet the geometric accuracy of 140mm~180mm and the aforementioned optical specifications can be recognized as qualified large-size preforms successfully prepared by the method of this invention.
[0060] In summary, this invention provides a complete and industrially feasible process for fabricating ultra-large-size optical fiber preforms, encompassing equipment improvements (silicon nitride wind shields), process innovations (precise splicing parameters, stepped sintering curves), and end-to-end quality control (optical inspection). This process systematically solves the key technical challenges brought about by large-size production, ultimately achieving a leapfrog improvement in product size, performance, and efficiency, and possesses significant industrial application value.
[0061] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for producing a large-size optical fiber preform, characterized by, Includes the following steps: S1. Mandrel preparation and welding: The mandrel and the end seed rod are welded together using a horizontal glass lathe. S2. Outer cladding deposition: Using a multi-torch longitudinal chemical vapor deposition equipment, SiO2 particles are deposited on the outside of the mandrel obtained in step S1 to form a porous body; S3, Vertical sintering: The loose body obtained in step S2 is placed in a vertical sintering furnace for dehydration and vitrification sintering to obtain a dense optical fiber preform. S4. Optical testing: Perform optical property testing on the optical fiber preform obtained in step S3.
2. The method of claim 1, wherein the method further comprises: In step S1, the hydrogen flow rate of the torch in the horizontal flame device is controlled at 200L / min to 300L / min, and the oxygen flow rate is controlled at 55L / min to 80L / min.
3. A method of producing a large-size optical fiber preform according to claim 2, wherein In step S2, the material of the blower wind shield of the multi-blower longitudinal chemical vapor deposition equipment is silicon nitride.
4. The method of claim 3, wherein the method further comprises the step of: In step S2, the overall deposition efficiency of the deposition equipment is controlled to be 110~200g / min, and the outer diameter of the loose body formed by deposition is 310mm~460mm.
5. The method of claim 1, wherein the method further comprises: Step S3 specifically includes the following steps: S31, Dehydration stage: The loose material is kept at 1280℃ for 2-4 hours to remove hydroxyl groups; S32, Sintering and densification stage: The loose body that has completed the dehydration stage is heated from 1280℃ to above 1500℃ at a rate of 3-5℃ / min, and held at 1340℃ and 1440℃ for 0.5~2 hours respectively during the heating process; S33. Cooling and annealing stage: After the sintered preform is cooled to 800℃ at a rate of 1-2℃ / min, it is allowed to cool naturally.
6. A method of producing a large-size optical fiber preform according to claim 5, wherein In step S32, the loose material is controlled to shrink uniformly from a diameter of 310mm~460mm to 140mm~180mm.
7. The method of claim 1, wherein the method further comprises the step of: In step S4, the optical property test includes at least: testing the cutoff wavelength of the optical fiber preform, the dispersion in the 1285nm band, and the mode field diameter. 8. The method of claim 1, wherein the method further comprises: The fiber preforms prepared according to this method have a single drawn length of 2000~5000km.
9. The method of claim 1, wherein the method further comprises the step of: The diameter of the optical fiber preform prepared according to this method is 140mm~180mm.