A harmless treatment process for co-processing tungsten slag in cement kilns

By using a cement kiln co-processing technology and pretreatment and special additives, the harmful components in tungsten slag are decomposed and stabilized, solving the environmental and economic problems of tungsten slag disposal, protecting equipment and reducing land occupation.

CN123106029APending Publication Date: 2026-11-17ZHEJIANG HONGSHI ENVIRONMENTAL PROTECTION SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611300842.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-26
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing methods for disposing of tungsten slag have drawbacks such as large land area requirements, high costs, risks of secondary pollution, limited resource recovery efficiency, and inability to achieve complete harmlessness.

Method used

The cement kiln co-processing technology is adopted. By mixing pretreated tungsten slag with cement raw materials, special additives and acid pickling corrosion inhibitors, the harmful components in the tungsten slag are decomposed and stabilized by the preheating, decomposition and calcination process of the cement kiln, and a protective film is formed at high temperature to protect the equipment.

Benefits of technology

It achieves the complete and harmless disposal of tungsten slag, with no secondary pollution, reduces equipment corrosion, saves land resources, and has both environmental and economic benefits.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention relates to a harmless treatment process for tungsten slag co-processing in cement kilns, belonging to the field of solid waste treatment technology. The tungsten slag is crushed and dried; the dried tungsten slag, cement raw materials, and special additives are mixed evenly to obtain a mixture; the mixture is fed into a cement kiln, where it undergoes preheating, decomposition, and calcination sequentially; the calcined material is cooled to room temperature and used as cement clinker, thus completing the harmless treatment of the tungsten slag; the acid pickling corrosion inhibitor is prepared from mercaptoacetic acid distillation residue, acrylate industrial wastewater, and sodium carbonate; this invention can achieve complete harmless treatment and resource utilization of tungsten slag.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of solid waste treatment technology, and in particular to a harmless treatment process for co-processing tungsten slag in cement kilns. Background Technology

[0002] Tungsten is an important strategic metal widely used in metallurgy, machinery, electronics, aerospace, and other fields. my country has abundant tungsten resources and a large-scale tungsten smelting industry. In the production of ammonium paratungstate (APT), every ton of APT produced generates 2-3 tons of tungsten slag, resulting in millions of tons of tungsten slag emissions annually. Tungsten slag is classified as hazardous waste, containing various harmful substances such as WO3, Mn, As, Pb, and Cr. If directly dumped or landfilled, the heavy metal ions within it can easily leach out through rainwater, polluting soil, groundwater, and surface water, posing a serious threat to the ecological environment and human health.

[0003] Chinese Patent CN110066146A discloses a method for recycling and reusing tungsten slag, comprising: S1. recovering valuable metals from tungsten slag to obtain secondary tungsten slag, the valuable metals including tungsten, iron and manganese; S2. calcining and activating kaolin to obtain metakaolin, and ball milling the metakaolin; S3. mixing blast furnace slag, ball-milled metakaolin and secondary tungsten slag according to a preset ratio, and adding an alkaline activator and water for mixing; S4. casting the mixed slurry into molds; S5. curing and demolding the molds to obtain tungsten slag geopolymer.

[0004] Chinese Patent CN121802174A: This invention relates to the field of resource recovery technology for tungsten slag, and more particularly to a method for resource recovery of tungsten slag. The method achieves resource recovery of tungsten slag through steps such as acid leaching, extraction, back-extraction, precipitation, and roasting.

[0005] Currently, the main methods for disposing of tungsten slag include landfilling, solidification / stabilization, and resource recovery. Landfilling requires a large area and poses a risk of secondary pollution, failing to meet environmental protection requirements. Solidification / stabilization requires the addition of large amounts of solidifying agents, resulting in high disposal costs, and the subsequent disposal of the solidified material is difficult. Resource recovery is mainly used to recover tungsten from the slag, but its recovery efficiency is limited, and the remaining residue still requires further treatment, failing to achieve complete harmlessness of the tungsten slag. Summary of the Invention

[0006] To address the aforementioned problems, this invention provides a harmless treatment process for the co-processing of tungsten slag in cement kilns, the operation steps of which are as follows, in parts by weight:

[0007] S1: Crush and dry the tungsten slag;

[0008] S2: Mix 2-8 parts of dried tungsten slag, 68-96 parts of cement raw meal, 1-5 parts of special additives, and 0.8-2.2 parts of pickling corrosion inhibitor evenly to obtain a mixture.

[0009] S3: The mixture is fed into the cement kiln and undergoes preheating, decomposition, and calcination in sequence;

[0010] S4: Cool the calcined material to room temperature and use it as cement clinker to complete the harmless treatment of tungsten slag.

[0011] Preferably, the drying in S1 is performed using a drum dryer, with a drying temperature of 120-150℃ and a drying time of 30-60 minutes.

[0012] Preferably, the main components of the cement raw material in S2 are calcium carbonate 62.53 wt%, silicon dioxide 21.35 wt%, aluminum oxide 5.71 wt%, iron oxide 4.64 wt%, and magnesium oxide 1.15 wt%.

[0013] Preferably, the special additive in S2 is a mixture of 40-60 parts activated vermiculite, 15-25 parts calcium lignosulfonate, 10-20 parts fluorite, and 5-10 parts boric acid.

[0014] Preferably, the mixing in S2 is carried out using a twin-shaft mixer with a mixing speed of 50-100 r / min and a mixing time of 15-30 min.

[0015] Preferably, the preheating temperature in S3 is 300-500℃, and the preheating time is 15-20min.

[0016] Preferably, the decomposition temperature in S3 is 850-950℃, and the decomposition time is 30-40 min.

[0017] Preferably, the calcination temperature in S3 is 1300-1450℃, and the calcination time is controlled within 15-30 minutes.

[0018] Preferably, the cooling in S4 is performed using a grate cooler, with a cooling time of 20-35 minutes.

[0019] Preferably, the preparation method of the pickling corrosion inhibitor in S2 is as follows:

[0020] By weight, 24-46 parts of mercaptoacetic acid distillation residue and 120-230 parts of 7-11 wt% acrylate industrial wastewater are mixed, and 0.15-0.6 parts of sodium carbonate are added as a catalyst. The mixture is stirred and reacted at 55-75℃ for 65-105 min. After the reaction, the mixture is filtered to remove impurities. The filtrate is purified by ultrafiltration and recycled. The remaining material is subjected to low-temperature rotary evaporation and vacuum freeze-drying to obtain the acid pickling corrosion inhibitor.

[0021] Reaction mechanism:

[0022] After being crushed, dried and pretreated, tungsten slag is uniformly mixed with cement raw materials and special additives. In the preheating, decomposition and gradient calcination temperature field of the cement kiln, harmful components such as tungsten trioxide and heavy metals in the tungsten slag are gradually decomposed and reconstructed, while beneficial components such as silicon and calcium participate in the formation of mineral crystal phases in cement clinker, realizing the resource-compatible utilization of waste slag.

[0023] In a weakly alkaline sodium carbonate catalytic system, the active mercapto groups of mercaptoacetic acid undergo a Michael addition-mercapto-olefin addition reaction with the carbon-carbon double bonds of acrylate. The sulfur-containing carboxyl groups of sodium carbonate then add to the corrosion-inhibiting organic matter, generating stable sulfur-containing carboxyl organic functional components. These components can be directionally adsorbed onto the metal surface of carbon steel equipment in cement kilns, self-assembling to form a dense, hydrophobic protective film. This protective film can isolate the equipment from high-temperature acidic flue gas and media corrosion within the kiln, effectively inhibiting oxidation corrosion and hydrogen evolution corrosion without interfering with the decomposition of tungsten slag, solidification of heavy metals, or normal calcination of cement clinker.

[0024] Technical effects:

[0025] The present invention provides a harmless treatment process for co-processing tungsten slag in cement kilns. Compared with the prior art, the present invention has the following significant advantages:

[0026] 1. Through a combination of pretreatment, special additive formulation and gradient calcination in cement kiln, the toxic components and heavy metals in tungsten slag can be completely decomposed and stably solidified, with no secondary pollution generated throughout the disposal process.

[0027] 2. The functional corrosion inhibitor can form a stable protective film under acidic and high-temperature conditions, effectively protecting the carbon steel equipment of the cement kiln, delaying the corrosion and loss of the medium, and extending the service life of the equipment.

[0028] 3. Beneficial components such as silicon and calcium in tungsten slag can replace some cement raw materials in clinker synthesis, reducing the consumption of primary minerals and saving solid waste landfill resources, thus achieving both environmental and economic benefits. Detailed Implementation

[0029] To further illustrate the technical means and effects adopted by the present invention to achieve the intended purpose, the following detailed description is provided in conjunction with embodiments and comparative examples:

[0030] 1. The tungsten slag comes from the Ganbei Tungsten Industry in Xiushui County. Its main components are: 10.76 wt% moisture, 5.96 wt% silicon dioxide, 19.67 wt% calcium oxide, 58.47 wt% iron oxide, 1.84 wt% aluminum oxide, 2.55 wt% tungsten trioxide, and 0.53 wt% magnesium oxide.

[0031] 2. Thioglycolic acid distillation residue: This residue comes from industrial enterprises in the Shengzhou Fine Chemical Industrial Park, Shaoxing City, and is the bottom residue from the distillation and refining process of thioglycolic acid. Its main components are: 62.23 wt% thioglycolic acid, 16.57 wt% dithiodiacetic acid, 10.61 wt% small molecule organic acids, and 8.36 wt% high-boiling organic residue.

[0032] 3. Acrylate industrial wastewater: originating from industrial enterprises in the petrochemical industrial park of Dushan Port Economic Development Zone, Pinghu City, Jiaxing City, it is process wastewater from the calcium acrylate synthesis section. Its main components are: 10.74 wt% calcium acrylate, with the remainder being inorganic salt aqueous solution and trace amounts of acrylic acid oligomers.

[0033] Heavy metal leaching concentration detection: The horizontal oscillation method in GB5085.3-2007 "Identification Standard for Hazardous Waste - Leaching Toxicity Identification" was used for detection, and the concentration of heavy metals such as tungsten, iron, and aluminum in the leachate was determined by inductively coupled plasma mass spectrometry.

[0034] Tungsten trioxide residue detection: The detection was carried out in accordance with GB / T176-2017 "Cement Chemical Analysis Methods", and the residual tungsten trioxide in cement clinker was determined by spectrophotometry.

[0035] Example 1

[0036] A harmless treatment process for co-processing tungsten slag in cement kilns, comprising the following steps:

[0037] S1: Crush and dry the tungsten slag;

[0038] S2: Mix 2kg of dried tungsten slag, 68kg of cement raw meal, 1kg of special additives, and 0.8kg of pickling corrosion inhibitor evenly to obtain a mixture.

[0039] S3: The mixture is fed into the cement kiln and undergoes preheating, decomposition, and calcination in sequence;

[0040] S4: Cool the calcined material to room temperature and use it as cement clinker to complete the harmless treatment of tungsten slag.

[0041] The drying process in S1 uses a drum dryer with a drying temperature of 120℃ and a drying time of 30 minutes.

[0042] The main components of the cement raw material in S2 are calcium carbonate 62.53 wt%, silicon dioxide 21.35 wt%, aluminum oxide 5.71 wt%, iron oxide 4.64 wt%, and magnesium oxide 1.15 wt%.

[0043] The special additive in S2 is composed of 40 kg of activated vermiculite, 15 kg of calcium lignosulfonate, 10 kg of fluorite, and 5 kg of boric acid.

[0044] The mixing in S2 is carried out using a twin-shaft mixer with a mixing speed of 50 r / min and a mixing time of 15 min.

[0045] The preheating temperature in S3 is 300℃ and the preheating time is 15min.

[0046] The decomposition temperature in S3 is 850℃, and the decomposition time is 30 min.

[0047] The calcination temperature in S3 is 1300℃, and the calcination time is controlled at 15min.

[0048] The cooling in S4 uses a grate cooler with a cooling time of 20 minutes.

[0049] The preparation method of the pickling corrosion inhibitor in S2 is as follows:

[0050] 24 kg of mercaptoacetic acid distillation residue and 120 kg of 7 wt% acrylate industrial wastewater were mixed, and 0.15 kg of sodium carbonate was added as a catalyst. The mixture was stirred and reacted at 55 °C for 65 min. After the reaction, the mixture was filtered to remove impurities. The filtrate was purified by ultrafiltration and recycled. The remaining material was subjected to low-temperature rotary evaporation and vacuum freeze-drying to obtain an acid pickling corrosion inhibitor.

[0051] Example 2

[0052] A harmless treatment process for co-processing tungsten slag in cement kilns, comprising the following steps:

[0053] S1: Crush and dry the tungsten slag;

[0054] S2: Mix 4 kg of dried tungsten slag, 75 kg of cement raw meal, 2 kg of special additives, and 1.3 kg of pickling corrosion inhibitor evenly to obtain a mixture.

[0055] S3: The mixture is fed into the cement kiln and undergoes preheating, decomposition, and calcination in sequence;

[0056] S4: Cool the calcined material to room temperature and use it as cement clinker to complete the harmless treatment of tungsten slag.

[0057] The drying process in S1 uses a drum dryer with a drying temperature of 130℃ and a drying time of 40 minutes.

[0058] The main components of the cement raw material in S2 are calcium carbonate 62.53 wt%, silicon dioxide 21.35 wt%, aluminum oxide 5.71 wt%, iron oxide 4.64 wt%, and magnesium oxide 1.15 wt%.

[0059] The special additive in S2 is composed of 45 kg of activated vermiculite, 18 kg of calcium lignosulfonate, 14 kg of fluorite, and 6 kg of boric acid.

[0060] The mixing in S2 is carried out using a twin-shaft mixer with a mixing speed of 60 r / min and a mixing time of 20 min.

[0061] The preheating temperature in S3 is 350℃ and the preheating time is 16min.

[0062] The decomposition temperature in S3 is 880℃, and the decomposition time is 35 min.

[0063] The calcination temperature in S3 is 1350℃, and the calcination time is controlled at 20min.

[0064] The cooling in S4 uses a grate cooler with a cooling time of 25 minutes.

[0065] The preparation method of the pickling corrosion inhibitor in S2 is as follows:

[0066] 32 kg of mercaptoacetic acid distillation residue and 160 kg of 8 wt% acrylate industrial wastewater were mixed, and 0.3 kg of sodium carbonate was added as a catalyst. The mixture was stirred and reacted at 60 °C for 75 min. After the reaction, the mixture was filtered to remove impurities. The filtrate was purified by ultrafiltration and recycled. The remaining material was subjected to low-temperature rotary evaporation and vacuum freeze-drying to obtain an acid pickling corrosion inhibitor.

[0067] Example 3

[0068] A harmless treatment process for co-processing tungsten slag in cement kilns, comprising the following steps:

[0069] S1: Crush and dry the tungsten slag;

[0070] S2: Mix 6 kg of dried tungsten slag, 88 kg of cement raw meal, 4 kg of special additives, and 1.8 kg of pickling corrosion inhibitor evenly to obtain a mixture.

[0071] S3: The mixture is fed into the cement kiln and undergoes preheating, decomposition, and calcination in sequence;

[0072] S4: Cool the calcined material to room temperature and use it as cement clinker to complete the harmless treatment of tungsten slag.

[0073] The drying process in S1 uses a drum dryer with a drying temperature of 140℃ and a drying time of 50 minutes.

[0074] The main components of the cement raw material in S2 are calcium carbonate 62.53 wt%, silicon dioxide 21.35 wt%, aluminum oxide 5.71 wt%, iron oxide 4.64 wt%, and magnesium oxide 1.15 wt%.

[0075] The special additive in S2 is composed of 55 kg of activated vermiculite, 23 kg of calcium lignosulfonate, 18 kg of fluorite, and 8 kg of boric acid.

[0076] The mixing in S2 is carried out using a twin-shaft mixer with a mixing speed of 80 r / min and a mixing time of 25 min.

[0077] The preheating temperature in S3 is 450℃ and the preheating time is 18min.

[0078] The decomposition temperature in S3 is 930℃, and the decomposition time is 35 min.

[0079] The calcination temperature in S3 is 1430℃, and the calcination time is controlled at 25min.

[0080] The cooling in S4 uses a grate cooler with a cooling time of 30 minutes.

[0081] The preparation method of the pickling corrosion inhibitor in S2 is as follows:

[0082] 40 kg of mercaptoacetic acid distillation residue and 200 kg of 10 wt% acrylate industrial wastewater were mixed, and 0.45 kg of sodium carbonate was added as a catalyst. The mixture was stirred and reacted at 70 °C for 95 min. After the reaction, the mixture was filtered to remove impurities. The filtrate was purified by ultrafiltration and recycled. The remaining material was subjected to low-temperature rotary evaporation and vacuum freeze-drying to obtain an acid pickling corrosion inhibitor.

[0083] Example 4

[0084] A harmless treatment process for co-processing tungsten slag in cement kilns, comprising the following steps:

[0085] S1: Crush and dry the tungsten slag;

[0086] S2: Mix 8 kg of dried tungsten slag, 96 kg of cement raw meal, 5 kg of special additives, and 2.2 kg of pickling corrosion inhibitor evenly to obtain a mixture.

[0087] S3: The mixture is fed into the cement kiln and undergoes preheating, decomposition, and calcination in sequence;

[0088] S4: Cool the calcined material to room temperature and use it as cement clinker to complete the harmless treatment of tungsten slag.

[0089] The drying process in S1 uses a drum dryer with a drying temperature of 150℃ and a drying time of 60 minutes.

[0090] The main components of the cement raw material in S2 are calcium carbonate 62.53 wt%, silicon dioxide 21.35 wt%, aluminum oxide 5.71 wt%, iron oxide 4.64 wt%, and magnesium oxide 1.15 wt%.

[0091] The special additive in S2 is composed of 60 kg of activated vermiculite, 25 kg of calcium lignosulfonate, 20 kg of fluorite, and 10 kg of boric acid.

[0092] The mixing in S2 is carried out using a twin-shaft mixer with a mixing speed of 100 r / min and a mixing time of 30 min.

[0093] The preheating temperature in S3 is 500℃ and the preheating time is 20min.

[0094] The decomposition temperature in S3 is 950℃, and the decomposition time is 40 min.

[0095] The calcination temperature in S3 is 1450℃, and the calcination time is controlled at 30min.

[0096] The cooling in S4 uses a grate cooler with a cooling time of 35 minutes.

[0097] The preparation method of the pickling corrosion inhibitor in S2 is as follows:

[0098] 46 kg of mercaptoacetic acid distillation residue and 230 kg of 11 wt% acrylate industrial wastewater were mixed, and 0.6 kg of sodium carbonate was added as a catalyst. The mixture was stirred and reacted at 75 °C for 105 min. After the reaction, the mixture was filtered to remove impurities. The filtrate was purified by ultrafiltration and recycled. The remaining material was subjected to low-temperature rotary evaporation and vacuum freeze-drying to obtain an acid pickling corrosion inhibitor.

[0099] Comparative Example 1

[0100] A harmless treatment process for co-processing tungsten slag in cement kilns, comprising the following steps:

[0101] S1: Crush and dry the tungsten slag;

[0102] S2: Mix 2kg of dried tungsten slag, 68kg of cement raw meal, and 1kg of special additive evenly to obtain a mixture.

[0103] S3: The mixture is fed into the cement kiln and undergoes preheating, decomposition, and calcination in sequence;

[0104] S4: Cool the calcined material to room temperature and use it as cement clinker to complete the harmless treatment of tungsten slag.

[0105] The drying process in S1 uses a drum dryer with a drying temperature of 120℃ and a drying time of 30 minutes.

[0106] The main components of the cement raw material in S2 are calcium carbonate 62.53 wt%, silicon dioxide 21.35 wt%, aluminum oxide 5.71 wt%, iron oxide 4.64 wt%, and magnesium oxide 1.15 wt%.

[0107] The special additive in S2 is composed of 40 kg of activated vermiculite, 15 kg of calcium lignosulfonate, 10 kg of fluorite, and 5 kg of boric acid.

[0108] The mixing in S2 is carried out using a twin-shaft mixer with a mixing speed of 50 r / min and a mixing time of 15 min.

[0109] The preheating temperature in S3 is 300℃ and the preheating time is 15min.

[0110] The decomposition temperature in S3 is 850℃, and the decomposition time is 30 min.

[0111] The calcination temperature in S3 is 1300℃, and the calcination time is controlled at 15min.

[0112] The cooling in S4 uses a grate cooler with a cooling time of 20 minutes.

[0113] Comparative Example 2

[0114] A harmless treatment process for co-processing tungsten slag in cement kilns, comprising the following steps:

[0115] S1: Crush and dry the tungsten slag;

[0116] S2: Mix 2kg of dried tungsten slag, 68kg of cement raw meal, 1kg of special additives, and 0.8kg of pickling corrosion inhibitor evenly to obtain a mixture.

[0117] S3: The mixture is fed into the cement kiln and undergoes preheating, decomposition, and calcination in sequence;

[0118] S4: Cool the calcined material to room temperature and use it as cement clinker to complete the harmless treatment of tungsten slag.

[0119] The drying process in S1 uses a drum dryer with a drying temperature of 120℃ and a drying time of 30 minutes.

[0120] The main components of the cement raw material in S2 are calcium carbonate 62.53 wt%, silicon dioxide 21.35 wt%, aluminum oxide 5.71 wt%, iron oxide 4.64 wt%, and magnesium oxide 1.15 wt%.

[0121] The special additive in S2 is composed of 40 kg of activated vermiculite, 15 kg of calcium lignosulfonate, 10 kg of fluorite, and 5 kg of boric acid.

[0122] The mixing in S2 is carried out using a twin-shaft mixer with a mixing speed of 50 r / min and a mixing time of 15 min.

[0123] The preheating temperature in S3 is 300℃ and the preheating time is 15min.

[0124] The decomposition temperature in S3 is 850℃, and the decomposition time is 30 min.

[0125] The calcination temperature in S3 is 1300℃, and the calcination time is controlled at 15min.

[0126] The cooling in S4 uses a grate cooler with a cooling time of 20 minutes.

[0127] The acid pickling corrosion inhibitor in S2 is mercaptoacetic acid distillation residue.

[0128] Comparative Example 3

[0129] A harmless treatment process for co-processing tungsten slag in cement kilns, comprising the following steps:

[0130] S1: Crush and dry the tungsten slag;

[0131] S2: Mix 2kg of dried tungsten slag, 68kg of cement raw meal, 1kg of special additives, and 0.8kg of pickling corrosion inhibitor evenly to obtain a mixture.

[0132] S3: The mixture is fed into the cement kiln and undergoes preheating, decomposition, and calcination in sequence;

[0133] S4: Cool the calcined material to room temperature and use it as cement clinker to complete the harmless treatment of tungsten slag.

[0134] The drying process in S1 uses a drum dryer with a drying temperature of 120℃ and a drying time of 30 minutes.

[0135] The main components of the cement raw material in S2 are calcium carbonate 62.53 wt%, silicon dioxide 21.35 wt%, aluminum oxide 5.71 wt%, iron oxide 4.64 wt%, and magnesium oxide 1.15 wt%.

[0136] The special additive in S2 is composed of 40 kg of activated vermiculite, 15 kg of calcium lignosulfonate, 10 kg of fluorite, and 5 kg of boric acid.

[0137] The mixing in S2 is carried out using a twin-shaft mixer with a mixing speed of 50 r / min and a mixing time of 15 min.

[0138] The preheating temperature in S3 is 300℃ and the preheating time is 15min.

[0139] The decomposition temperature in S3 is 850℃, and the decomposition time is 30 min.

[0140] The calcination temperature in S3 is 1300℃, and the calcination time is controlled at 15min.

[0141] The cooling in S4 uses a grate cooler with a cooling time of 20 minutes.

[0142] The acid pickling corrosion inhibitor in S2 is 7wt% acrylate industrial wastewater.

[0143] Table 1 shows the test results for tungsten leaching concentration, iron leaching concentration, aluminum leaching concentration, and tungsten trioxide residue in the specific implementation plan.

[0144] Tungsten leaching concentration (mg / L) Iron leaching concentration (mg / L) Aluminum leaching concentration (mg / L) Tungsten trioxide residue (wt%) Example 1 0.12 0.27 0.14 0.07 Example 2 0.10 0.25 0.13 0.05 Example 3 0.07 0.22 0.11 0.03 Example 4 0.06 0.21 0.10 0.02 Comparative Example 1 0.52 1.35 0.86 0.35 Comparative Example 2 0.31 0.75 0.38 0.19 Comparative Example 3 0.25 0.56 0.31 0.13

[0145] Table 1. Summary of Detection Results for Tungsten Leaching Concentration, Iron Leaching Concentration, Aluminum Leaching Concentration, and Tungsten Trioxide Residue

[0146] The leaching levels of tungsten, iron, and aluminum, as well as the residual amount of tungsten trioxide, in this embodiment of the invention are superior to those in the comparative example, and the harmless solidification effect of tungsten slag is excellent. Conventional cement kiln co-processing relies solely on high-temperature calcination to solidify waste residue, lacking supporting equipment corrosion protection and having only moderate control over harmful component residues. This invention innovatively uses the Michael addition reaction of mercaptoacetic acid residue and acrylate wastewater to prepare a corrosion inhibitor, simultaneously achieving the dual goals of equipment protection and waste residue disposal. Combined with special additives and a gradient temperature control process in cement kilns, it not only enhances the solidification and sealing effect of heavy metals and tungsten components in tungsten slag, but also solves the problem of equipment corrosion under high-temperature acidic conditions, demonstrating significant advantages in process adaptability and comprehensive treatment.

[0147] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.

Claims

1. A harmless treatment process for co-processing tungsten slag in a cement kiln, the operation steps of which are as follows, in parts by weight: S1: Crush and dry the tungsten slag; S2: Mix 2-8 parts of dried tungsten slag, 68-96 parts of cement raw meal, 1-5 parts of special additives, and 0.8-2.2 parts of pickling corrosion inhibitor evenly to obtain a mixture. S3: The mixture is fed into the cement kiln and undergoes preheating, decomposition, and calcination in sequence; S4: Cool the calcined material to room temperature and use it as cement clinker to complete the harmless treatment of tungsten slag; The pickling corrosion inhibitor in S2 is obtained by reacting mercaptoacetic acid distillation residue, acrylate industrial wastewater, and sodium carbonate, filtering to remove impurities, purifying the filtrate by ultrafiltration and recycling, and then evaporating the remaining material by low-temperature rotary evaporation and vacuum freeze-drying.

2. The harmless treatment process for co-processing tungsten slag in cement kilns according to claim 1, characterized in that: The drying process in S1 uses a drum dryer with a drying temperature of 120-150℃ and a drying time of 30-60 minutes.

3. The harmless treatment process for co-processing tungsten slag in cement kilns according to claim 1, characterized in that: The main components of the cement raw material in S2 are calcium carbonate 62.53 wt%, silicon dioxide 21.35 wt%, aluminum oxide 5.71 wt%, iron oxide 4.64 wt%, and magnesium oxide 1.15 wt%.

4. The harmless treatment process for co-processing tungsten slag in cement kilns according to claim 1, characterized in that: The special additive in S2 is composed of 40-60 parts activated vermiculite, 15-25 parts calcium lignosulfonate, 10-20 parts fluorite, and 5-10 parts boric acid.

5. The harmless treatment process for co-processing tungsten slag in cement kilns according to claim 1, characterized in that: The mixing in S2 is carried out using a twin-shaft mixer with a mixing speed of 50-100 r / min and a mixing time of 15-30 min.

6. The harmless treatment process for co-processing tungsten slag in cement kilns according to claim 1, characterized in that: The preheating temperature in S3 is 300-500℃, and the preheating time is 15-20min.

7. The harmless treatment process for co-processing tungsten slag in cement kilns according to claim 1, characterized in that: The decomposition temperature in S3 is 850-950℃, and the decomposition time is 30-40 min.

8. The harmless treatment process for co-processing tungsten slag in cement kilns according to claim 1, characterized in that: The calcination temperature in S3 is 1300-1450℃, and the calcination time is controlled at 15-30min.

9. The harmless treatment process for co-processing tungsten slag in cement kilns according to claim 1, characterized in that: The cooling in S4 uses a grate cooler, and the cooling time is 20-35 minutes.

10. The harmless treatment process for co-processing tungsten slag in cement kilns according to claim 1, characterized in that: The preparation method of the pickling corrosion inhibitor in S2 is as follows: By weight, 24-46 parts of mercaptoacetic acid distillation residue and 120-230 parts of 7-11 wt% acrylate industrial wastewater are mixed, and 0.15-0.6 parts of sodium carbonate are added as a catalyst. The mixture is stirred and reacted at 55-75℃ for 65-105 min. After the reaction, the mixture is filtered to remove impurities. The filtrate is purified by ultrafiltration and recycled. The remaining material is subjected to low-temperature rotary evaporation and vacuum freeze-drying to obtain the acid pickling corrosion inhibitor.

Citation Information

Patent Citations

  • Recycle and reuse method for tungsten slag

    CN110066146A

  • Resource recycling method for tungsten slag

    CN121802174A