A barium slag-based low-leaching wall brick material and its preparation method
By combining sodium thiosulfate pentahydrate pre-permeation with industrial calcium peroxide oxidation and aging with an alkali-activated gelation system, the problem of difficult penetration of reagents in barium slag stabilization treatment was solved, achieving stability and structural density of barium slag-based low-leaching wall bricks.
Patent Information
- Application Number
- CN202611321675.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-17
AI Technical Summary
Existing barium slag stabilization treatments suffer from problems such as insufficient penetration of reagents into the particle interior and inadequate treatment of internally migratable barium. Furthermore, residual migratable barium may be released again due to moisture migration during subsequent brick making and use, making it difficult to maintain a stable low barium leaching state in the wall bricks.
Barium slag is pre-permeable to sodium thiosulfate pentahydrate solution, followed by the addition of industrial calcium peroxide powder for oxidation and aging to form barium sulfate fixation. Combined with an alkali-activated cementing system of granulated blast furnace slag powder, fly ash, metakaolin and sodium metasilicate pentahydrate, wall bricks are produced by pressing and curing.
It promotes the transformation of sulfur-containing species within particle pores, reduces barium leaching, forms a continuous barium migration control process, improves the stability of the low-barium leaching state of wall bricks, avoids the concentration of reagent reaction on the outer surface of particles, and enhances the density of the brick structure.
Smart Images

Figure CN123106034A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of solid waste resource utilization and new wall materials, and relates to a barium slag-based low-leaching wall brick material and its preparation method. Background Technology
[0002] Barium slag is a solid waste generated during the production of barium salts. Its mineral composition is complex, containing not only components such as silicon, aluminum, and calcium that can participate in the cementation reaction, but also potentially migratable barium, sulfides, and unreacted barium-containing phases. When barium slag is stockpiled or used directly in building materials, the migratable barium may diffuse outwards with pore water, and the sulfides may also migrate or transform in acidic or humid environments. Therefore, stabilization treatment is necessary before resource utilization.
[0003] Existing methods for the resource recovery of barium slag typically involve treating barium and sulfides with sulfates, carbonates, ferric salts, or other stabilizing agents, followed by mixing the stabilized barium slag with cement, gypsum, or other cementitious materials to prepare bricks. While these methods can reduce some of the soluble barium content, the agents react preferentially on the particle surface and pores after mixing with the barium slag, forming insoluble precipitates or reaction product layers. As the amount of reaction products on the particle surface increases, the pores gradually narrow, restricting the migration of the agents into the internal pores and cracks of the particles, making it difficult to fully treat the residual migratable barium and sulfides inside.
[0004] During the subsequent processes of adding water, mixing, pressing, and curing, the pore water in the surface-stabilized barium slag will redistribute, and the unstable barium-containing phase inside the particles may dissolve again and enter the capillary channels of the brick. Hydration and changes in wet and dry conditions may also promote the migration and accumulation of soluble salts in the pores, resulting in a low initial leaching level in the finished product, but barium leaching will increase after curing, soaking, or long-term service. Simply increasing the amount of stabilizing agent can easily lead to excessively rapid external reactions of the particles, soluble salt residue, and gas release from the molding material, affecting the pore structure, strength, and durability of the brick.
[0005] Therefore, the technical problem that the existing technology needs to solve is that the existing barium slag stabilization treatment has the problem that the agent is difficult to fully penetrate into the interior of the particles and the treatment of the internal migratory barium is insufficient. Moreover, the residual migratory barium may be released again due to moisture migration during subsequent brick making and use, making it difficult to maintain the low barium leaching state of the wall bricks stably. Summary of the Invention
[0006] To address the shortcomings of existing technologies, the present invention aims to provide a barium slag-based low-leaching wall brick material and its preparation method. The barium slag is first pre-permeated with sodium thiosulfate pentahydrate aqueous solution, then oxidized and aged with industrial calcium peroxide powder. The resulting treated barium slag is mixed with granulated blast furnace slag powder, fly ash, metakaolin, sodium metasilicate pentahydrate, and anhydrous sodium carbonate, and then pressed and cured to obtain wall bricks. This method promotes the transformation of sulfur-containing species within the particle pores and reduces barium leaching by alkali-activated cementitious products that fix the barium-containing phase and seal migration channels.
[0007] To achieve this objective, the present invention adopts the following technical solution: In a first aspect, the present invention provides a barium slag-based low-leaching wall brick material, which is prepared by mixing, pressing and molding, and curing treated barium slag, granulated blast furnace slag powder, fly ash, metakaolin, sodium metasilicate pentahydrate and anhydrous sodium carbonate. The mass ratio of the solid feed amount of the barium slag, granulated blast furnace slag powder, fly ash, metakaolin, sodium metasilicate pentahydrate, and anhydrous sodium carbonate is 100:(45-52):(20-24):(7-9):(5.5-7.5):(1.8-2.3). The treated barium slag is obtained by first pre-permeating barium slag raw material with an aqueous solution of sodium thiosulfate pentahydrate, and then oxidizing and aging it with industrial calcium peroxide powder. The mass ratio of the barium slag raw material to sodium thiosulfate pentahydrate is 100:(0.8-1.8) on a dry basis, and the mass ratio of sodium thiosulfate pentahydrate to industrial calcium peroxide powder is 1:(2.5-3.0). The CaO2 content in the industrial calcium peroxide powder is 60-75 wt.%. The amount of solid feed material for the treated barium slag is the sum of the dry basis mass of the barium slag raw material, the mass of sodium thiosulfate pentahydrate, and the mass of industrial calcium peroxide powder added when preparing the treated barium slag. The raw materials for preparing the barium slag-based low-leaching wall brick material do not contain additional silicate cement clinker, cement containing silicate cement clinker, sulfoaluminate cement, dihydrate gypsum, hemihydrate gypsum, or anhydrous gypsum.
[0008] Preferably, the granulated blast furnace slag powder is selected from at least one of S95 grade granulated blast furnace slag powder and S105 grade granulated blast furnace slag powder; the fly ash is Class F, Grade II fly ash; the metakaolin contains 50-60 wt.% SiO2, 35-45 wt.% Al2O3, and the total content of SiO2 and Al2O3 is 85-98 wt.%.
[0009] Preferably, the purity of the sodium metasilicate pentahydrate is not less than 95 wt.%, the purity of the anhydrous sodium carbonate is not less than 98 wt.%, and the D90 of the industrial calcium peroxide powder is not greater than 150 μm.
[0010] Secondly, the present invention provides a method for preparing barium slag-based low-leaching wall brick material as described in the first aspect, comprising the following steps: S1, the barium slag is cleaned of impurities, crushed and screened, and the moisture content is adjusted to obtain barium slag raw material; S2, dissolve sodium thiosulfate pentahydrate in the first portion of water to obtain the first solution, add the first solution to the barium slag raw material in batches and mix, let stand for pre-permeation treatment to obtain the first mixture; S3, add industrial calcium peroxide powder to the first mixture in batches and mix, carry out non-sealed covering aging, stir and then carry out open aging to obtain treated barium slag; S4, granulated blast furnace slag powder, fly ash, metakaolin, sodium metasilicate pentahydrate and anhydrous sodium carbonate are mixed to obtain a second mixture; S5, the treated barium slag is mixed with the second mixture, a second portion of water is added in batches and mixing is continued to obtain a third mixture; S6, the third mixture is pressed into shape to obtain a brick blank, and the brick blank is subjected to sealed curing, moist heat curing and room temperature curing in sequence to obtain barium slag-based low leaching wall brick material.
[0011] Preferably, in S1, the barium slag raw material has a moisture content of 10-15 wt.% and a particle size of no more than 2 mm.
[0012] Preferably, in S2, the mass ratio of the barium slag raw material to the total mass of the water and the first portion of water contained in the barium slag raw material, based on dry weight, is 100:(25-35). The temperature of the first portion of water is 20-35℃. The first solution is added in 2-4 portions, and mixed for 3-8 minutes after each addition. After all the solution is added, mixing continues for 10-20 minutes. The settling temperature is 15-35℃ and the settling time is 0.5-2 hours.
[0013] Preferably, in S3, the D90 of the industrial calcium peroxide powder is not greater than 150 μm.
[0014] Preferably, the industrial calcium peroxide powder is added in 2-4 portions, and mixed for 5-10 minutes after each addition; the non-sealed covered aging temperature is 15-35℃ and the time is 6-18 hours; the open aging temperature is 15-35℃ and the time is 2-8 hours.
[0015] Preferably, in step S4, the mixing time of the granulated blast furnace slag powder, fly ash, metakaolin, sodium metasilicate pentahydrate, and anhydrous sodium carbonate is 3-10 minutes.
[0016] Preferably, in S5, based on the amount of 100 parts of the processed barium slag solid feed, the amount of water added in the second part is 5-12 parts.
[0017] Preferably, in step S6, the pressing pressure is 15-30 MPa.
[0018] Preferably, in S6, the temperature for sealing curing is 20-35℃ and the time is 12-36h; the temperature for damp heat curing is 40-65℃ and the relative humidity is not less than 90% and the time is 8-24h; the temperature for room temperature curing is 20-30℃ and the time is 7-28d.
[0019] Sodium thiosulfate pentahydrate dissolves in water to form thiosulfate and sodium ions. The resulting solution can migrate with capillary water between barium slag particles and within the pores of the particles. Compared to sulfate, thiosulfate has a weaker tendency to form insoluble precipitates with barium ions, and sulfate has not yet been concentratedly generated during the pre-permeation stage. Therefore, it can enter the pores, fissures, and adjacent regions of the unstabilized barium-containing phases of the barium slag before a large amount of precipitate products form on the particle surface. Adding the sodium thiosulfate pentahydrate aqueous solution in batches and allowing it to stand after mixing helps to reduce the local concentration difference in the material, allowing thiosulfate to diffuse with water and migrate capillarily into the interior of the particles and distribute in the pore liquid containing barium ions, sulfides, and alkaline components.
[0020] Industrial calcium peroxide hydrolyzes upon contact with aqueous materials, producing hydrogen peroxide and calcium hydroxide. Calcium hydroxide further provides calcium ions and hydroxide ions through dissolution equilibrium. In alkaline pore water, hydrogen peroxide can also be partially converted to hydrogen peroxide. Hydrogen peroxide and hydrogen peroxide can migrate with pore water and gradually participate in the oxidation reactions of sulfur-containing species. Thiosulfate ions can be gradually converted to sulfate ions via tetrathionate, sulfite, and other intermediate sulfur-containing species. Sulfides in barium slag can also be gradually oxidized to sulfur-containing species with different degrees of oxidation, such as elemental sulfur, polysulfides, thiosulfates, sulfites, and sulfates, thereby reducing the proportion of sulfide forms and the risk of releasing hydrogen sulfide under acidification conditions. This process does not require all sulfur-containing species to be converted to sulfate ions. The sulfate ions generated can form insoluble barium sulfate with barium ions in the pore water, reducing the activity and migration ability of barium ions in the pore water.
[0021] Because thiosulfate ions have already entered the interior of the barium slag particles before the addition of industrial calcium peroxide, and the soluble peroxide species formed by the hydrolysis of calcium peroxide can further migrate with pore water, the formation of sulfate ions and the precipitation and fixation of barium are no longer limited to the outer surface of the barium slag particles, but may also occur in the pores, cracks, and adjacent regions of barium-containing phases within the particles. This sequence helps to reduce the obstruction of subsequent mass transfer caused by the premature formation of a precipitation layer on the outer surface of the particles, and increases the possibility of fixing residual migratory barium inside the particles. The defined feeding ratio of sodium thiosulfate pentahydrate to industrial calcium peroxide can also form an appropriate balance between the oxidation of sulfur-containing species and the consumption of peroxides, avoiding the impact on the treatment effect due to a significant deficiency of one material.
[0022] Hydrogen peroxide released from industrial calcium peroxide can decompose and generate oxygen. Iron, manganese, and other transition metal components in barium slag may promote the decomposition of hydrogen peroxide and the oxidation of sulfur-containing species. Non-enclosed aging can limit the rapid loss of surface moisture while allowing gases such as oxygen produced in the reaction to escape, enabling the hydrolysis of calcium peroxide, diffusion of reactants, and oxidation of sulfur-containing species to continue within the water-containing pores. Turning and mixing can disrupt localized agglomeration zones, redistribute industrial calcium peroxide, pore water, and unreacted barium slag particles, and expose the reaction interfaces that were previously within the agglomerates. Subsequent open aging facilitates oxygen escape and continued consumption of residual active peroxides, reducing the possibility of concentrated decomposition and release of residual active oxygen during subsequent mixing, water addition, and pressing, thereby reducing the risk of pore formation, localized expansion, or microcracks within the brick blank.
[0023] Sodium metasilicate pentahydrate, when dissolved in mixed water, not only increases the alkalinity of the pore fluid but also directly provides soluble silicate ions. Anhydrous sodium carbonate, upon dissolution, provides sodium ions and carbonate ions, participating in the formation of an alkaline reaction environment through solution equilibrium. Under alkaline conditions, hydroxide ions promote the breaking of silicon-oxygen and aluminum-oxygen bonds in granulated blast furnace slag powder, fly ash, and metakaolin, allowing silicon, aluminum, calcium, and other reactive components to enter the liquid phase. The soluble silicon components provided by sodium metasilicate pentahydrate can also directly participate in subsequent condensation reactions, increasing the content of reactive silicon in the liquid phase during the initial stage of the gelation reaction.
[0024] The calcium released from granulated blast furnace slag powder reacts with dissolved silicon and aluminum components to form aluminum-calcium silicate gels; the silicon and aluminum components released from fly ash and metakaolin can form sodium-aluminum silicate gels with the participation of sodium ions. In systems with high calcium content and the coexistence of multiple silicon and aluminum raw materials, sodium-containing aluminum-calcium silicate gels or other cross-linked composite cementitious products may also be formed. These cementitious products can nucleate, grow, and intertwine on the surfaces of barium slag particles, blast furnace slag particles, fly ash particles, and metakaolin particles, connecting different solid particles into a continuous cementitious structure.
[0025] Anhydrous sodium carbonate provides carbonate ions that react with calcium ions in the pore fluid to form calcium carbonate. Calcium carbonate can contribute to micro-aggregate filling and nucleation, and interacts with the pore fluid ion balance and the formation of gelling products. A small amount of barium ions not fixed by sulfate can also precipitate with carbonate ions, but barium carbonate is less stable than barium sulfate under acidic conditions. Therefore, carbonate precipitation mainly serves to reduce the concentration of barium ions in the pore fluid. Barium stabilization can be achieved through a combination of barium sulfate precipitation, adsorption and binding of gelling products, and pore structure densification. Barium sulfate, due to its low solubility, serves as an important chemical fixation form.
[0026] Deprotonated silanol sites, aluminol sites, and negatively charged structural sites on the surface of gel products can bind barium ions in the pore fluid through electrostatic adsorption, ion exchange, or surface complexation. Some barium ions may also be encapsulated in the gel nanopores, the interface region between unreacted particles and the gel, or enter the local aluminosilicate structure as charge-balanced ions during the growth of the gel products, thereby further reducing their migration ability.
[0027] The calcium hydroxide and calcium ions produced by the hydrolysis of industrial calcium peroxide can also participate in the reaction of slag and other silica-alumina components, promoting the formation of alumina-calcium silicate cementitious products on the surface of barium slag particles and at the interparticle interface. Barium sulfate, other sulfur-containing oxidation products, calcium reaction products, and aluminosilicate cementitious products on the surface of barium slag particles together constitute the transition zone between the barium slag particles and the cementitious matrix. This transition zone helps reduce the pore connectivity between the barium slag particles and the cementitious matrix and restricts the direct entry of external moisture into the interior of the barium slag particles. The deposition of cementitious products in the particle pores, fissures, and interparticle spaces can divide the original continuous migration channels into closed or low-connectivity pores, thereby reducing the conditions for continuous pore water flow and barium ion diffusion and migration.
[0028] During the pressing process, barium slag particles, blast furnace slag particles, fly ash particles, and metakaolin particles rearrange themselves, reducing the interparticle spacing, allowing some pore water and air to escape, and increasing the contact area between solid particles. Flaky or irregular aluminosilicate particles can fill the voids between barium slag particles, while finer particles enter larger pores, forming a multi-scale particle packing structure. The particle contact interfaces formed during pressing provide reaction sites for subsequent dissolution, condensation, and gel bridging, and provide a foundation for maintaining the early shape of the brick blank and subsequent densification.
[0029] Sealed curing limits early moisture evaporation from the brick blank, keeping sodium metasilicate pentahydrate and anhydrous sodium carbonate in a dissolved and migrating state, and maintaining the continuous dissolution of slag, fly ash, and metakaolin. Moist heat curing accelerates ion migration, silica-alumina species condensation, and the nucleation and growth of cementitious products, extending these products into the interparticle pores and onto the surface of barium slag particles. During room temperature curing, unreacted silica-alumina components continue to participate in the reaction, further condensing and densifying the cementitious structure, gradually reducing the interconnected pores between particles. The resulting low-interconnected porosity structure extends the path for external moisture to enter the brick and for residual barium ions to migrate outwards.
[0030] Therefore, pre-permeation, oxidative aging, and alkali-activated gelation together form a continuous process for controlling barium migration. The pre-permeation stage allows thiosulfate ions to pre-enter the pores within the barium slag particles; the oxidative aging stage gradually transforms the pre-permeated thiosulfate ions and the original sulfides in the barium slag into higher oxidation states of sulfur-containing species, and the generated sulfate ions react with barium ions to form barium sulfate; the subsequent alkali-activated gelation stage further restricts the migration of residual barium through surface adsorption, ion exchange, particle encapsulation, interfacial bonding, and pore sealing. These processes prevent the stabilization reaction from becoming excessively concentrated on the outer surface of the barium slag particles, and also avoid relying solely on carbonate precipitation or conventional cement hydration products to maintain the barium's fixed state.
[0031] The technical concept of this solution lies in combining the pre-permeation of sodium thiosulfate pentahydrate aqueous solution with the subsequent oxidation and aging of industrial calcium peroxide in a specific sequence. This allows thiosulfate ions to first enter the interior of the barium slag particles, and then gradually oxidize within the particles and at the interface, participating in the fixation of barium sulfate. Simultaneously, the treated barium slag is introduced into an alkali-activated cementing system composed of granulated blast furnace slag powder, fly ash, metakaolin, sodium metasilicate pentahydrate, and anhydrous sodium carbonate. The barium migration is further restricted through the cementing products containing aluminum-calcium silicates, sodium-aluminum silicates, and the low-connectivity pore structure formed by pressing and curing. This creates a continuous treatment chain connecting the chemical fixation within the particles, the particle-matrix interface bonding, and the sealing of the brick pores, thereby improving the stability of the low-barium leaching state of the wall bricks.
[0032] Compared with existing technologies, the beneficial effects of this invention are as follows: This invention first uses a sodium thiosulfate pentahydrate aqueous solution to pre-permeate the barium slag, allowing thiosulfate ions to enter the pores, fissures, and adjacent areas of the barium-containing phase within the barium slag particles along with pore water. Then, peroxides released by industrial calcium peroxide gradually oxidize the sulfur-containing species, promoting the formation of sulfate ions inside the particles and their interaction with barium ions to form barium sulfate. This reduces the phenomenon where reaction products concentrate on the particle surface and pore openings, hindering the continued migration of the reagents. Oxidative aging also reduces the risk of hydrogen sulfide release from sulfides under acidification conditions. Non-sealed covering aging and open aging are beneficial for maintaining the moisture required for the reaction and venting reaction gases. The treated barium slag, granulated blast furnace slag powder, fly ash, and metakaolin form an alkali-activated cementitious system. The generated aluminum-calcium silicate gel and sodium-aluminum silicate gel can connect particles, coat the barium-containing phase, and seal interconnected pores, further limiting the migration of residual barium with pore water. Pressing and phased curing promote particle rearrangement, interfacial bonding, and the formation of cementitious structures, which connects the internal precipitation and fixation of barium particles, the interfacial adsorption and fixation, and the sealing of brick pores. This reduces barium leaching while realizing the utilization of barium slag as a wall material. Attached Figure Description
[0033] Figure 1 This is a physical image of the barium slag-based low-leaching wall brick material provided in Embodiment 1 of the present invention; Figure 2 This is a cross-sectional image of the barium slag-based low-leaching wall brick material provided in Embodiment 1 of the present invention. Detailed Implementation
[0034] The technical solutions of the present invention will be described in detail below with reference to specific embodiments and accompanying drawings. The embodiments described herein are specific implementations of the present invention, used to illustrate the concept of the present invention; these descriptions are explanatory and exemplary, and should not be construed as limiting the implementation methods or the scope of protection of the present invention. In addition to the embodiments described herein, those skilled in the art can employ other obvious technical solutions based on the content disclosed in the claims and specification of this application. These technical solutions include those that make any obvious substitutions and modifications to the embodiments described herein.
[0035] The chemical reagents used in the embodiments and comparative examples of this invention are all commercially available products and have not undergone any further purification treatment.
[0036] Example 1 This embodiment provides a method for preparing a barium slag-based low-leaching wall brick material, the preparation method comprising the following steps: S1, the barium slag is cleaned of impurities, crushed and screened, and the moisture content is adjusted to obtain barium slag raw material; the moisture content of the barium slag raw material is 15 wt.%, and the particle size is not greater than 1.5 mm; based on 100 parts of dry weight of the barium slag raw material, the moisture content of the barium slag raw material is 17.65 parts. S2, dissolve 1.5 parts of sodium thiosulfate pentahydrate in 14.35 parts of water in the first part to obtain a first solution; the temperature of the first part of water is 35℃; add the first solution to the barium slag raw material in 3 portions, mixing for 3 minutes after each addition, and continuing to mix for 17 minutes after all the solution has been added, and then let it stand at 28℃ for 2 hours for pre-permeation treatment to obtain a first mixture; the mass ratio of the barium slag raw material to the total mass of water and water in the first part of the barium slag raw material on a dry basis is 100:32; S3, 3.75 parts of industrial calcium peroxide powder are added to the first mixture in four portions, and mixed for 8 minutes after each addition; the mass ratio of sodium thiosulfate pentahydrate to industrial calcium peroxide powder is 1:2.5, the CaO2 content of the industrial calcium peroxide powder is 70 wt.%, and the D90 is not greater than 130 μm; after the addition is completed, the mixture is aged at 15°C under non-sealed cover for 14 hours, then stirred and aged at 28°C in an open manner for 4 hours to obtain treated barium slag; the solid feed amount of the treated barium slag is 105.25 parts; S4, taking 100 parts of the solid barium slag to be processed, 50 parts of S95 grade granulated blast furnace slag powder, 20 parts of F-grade II fly ash, 9 parts of metakaolin, 6.2 parts of sodium metasilicate pentahydrate, and 2.1 parts of anhydrous sodium carbonate are mixed for 10 minutes to obtain a second mixture; the metakaolin contains 56 wt.% SiO2 and 40 wt.% Al2O3, with a total content of 96 wt.% for SiO2 and Al2O3; the sodium metasilicate pentahydrate has a purity of 96 wt.% and the anhydrous sodium carbonate has a purity of 99 wt.%. S5, the treated barium slag is mixed with the second mixture, and based on the amount of the treated barium slag solid feed being 100 parts, 8 parts of the second part of water are added in batches and the mixture is continued to be mixed to obtain the third mixture; S6, the third mixture is pressed into shape under a pressure of 20 MPa to obtain a brick blank; the brick blank is sealed and cured at 30°C for 12 hours, then moist-heat cured at 56°C and 95% relative humidity for 18 hours, and then cured at room temperature at 20°C for 21 days to obtain a barium slag-based low-leaching wall brick material, such as... Figure 1 As shown, the prepared barium slag-based low-leaching wall brick material maintains a complete block structure, with regular brick shape and no large-area cracking or obvious delamination; Figure 2 As shown, no penetrating stratification was observed in the cross-section of the prepared barium slag-based low-leaching wall brick material, and the barium slag and cementitious material formed a continuous consolidated structure.
[0037] Example 2 This embodiment provides a method for preparing a barium slag-based low-leaching wall brick material, the preparation method comprising the following steps: S1, the barium slag is cleaned of impurities, crushed and screened, and the moisture content is adjusted to obtain barium slag raw material; the moisture content of the barium slag raw material is 10 wt.%, and the particle size is not greater than 2 mm; based on 100 parts of dry weight of the barium slag raw material, the moisture content of the barium slag raw material is 11.11 parts. S2, dissolve 0.8 parts of sodium thiosulfate pentahydrate in 23.89 parts of water in the first part to obtain a first solution; the temperature of the first part of water is 20°C; add the first solution to the barium slag raw material in two portions, mixing for 6.5 minutes after each addition, and continuing to mix for 10 minutes after all the solution has been added, and then let it stand at 35°C for 1 hour for pre-permeation treatment to obtain a first mixture; the mass ratio of the barium slag raw material to the total mass of water and water in the first part of the barium slag raw material on a dry basis is 100:35; S3, 2.24 parts of industrial calcium peroxide powder are added to the first mixture in three portions, and mixed for 5 minutes after each addition; the mass ratio of sodium thiosulfate pentahydrate to industrial calcium peroxide powder is 1:2.8, the CaO2 content of the industrial calcium peroxide powder is 75wt.%, and the D90 is not greater than 150μm; after the addition is completed, the mixture is aged at 28°C under non-sealed cover for 6 hours, then stirred and aged at 35°C in an open environment for 8 hours to obtain treated barium slag; the solid feed amount of the treated barium slag is 103.04 parts; S4, taking 100 parts of the solid barium slag to be processed, 45 parts of S105 grade granulated blast furnace slag powder, 23 parts of Class F II fly ash, 8.5 parts of metakaolin, 7.5 parts of sodium metasilicate pentahydrate, and 1.8 parts of anhydrous sodium carbonate are mixed for 5 minutes to obtain a second mixture; the metakaolin contains 50 wt.% SiO2 and 35 wt.% Al2O3, with a total content of 85 wt.% for SiO2 and Al2O3; the sodium metasilicate pentahydrate has a purity of 95 wt.% and the anhydrous sodium carbonate has a purity of 98 wt.%. S5, the treated barium slag is mixed with the second mixture, and based on the amount of the treated barium slag solid feed being 100 parts, 5 parts of the second part of water are added in batches and the mixture is continued to be mixed to obtain the third mixture; S6, the third mixture is pressed into shape under a pressure of 30MPa to obtain a brick blank; the brick blank is sealed and cured at 25°C for 28h, then moist heat cured at 40°C and relative humidity of 90% for 13h, and then cured at room temperature at 27°C for 7d to obtain barium slag-based low-leaching wall brick material.
[0038] Example 3 This embodiment provides a method for preparing a barium slag-based low-leaching wall brick material, the preparation method comprising the following steps: S1, the barium slag is cleaned, crushed and screened, and the moisture content is adjusted to obtain barium slag raw material; the moisture content of the barium slag raw material is 13wt.%, and the particle size is not greater than 1.2mm; based on 100 parts of dry weight of the barium slag raw material, the moisture content of the barium slag raw material is 14.94 parts. S2, dissolve 1.8 parts of sodium thiosulfate pentahydrate in 10.06 parts of water in the first part to obtain a first solution; the temperature of the first part of water is 30℃; add the first solution to the barium slag raw material in 4 portions, mixing for 8 minutes after each addition, and continuing to mix for 13 minutes after all the solution has been added, and then let it stand at 15℃ for 1.5 hours for pre-permeation treatment to obtain a first mixture; the mass ratio of the barium slag raw material to the total mass of water and water in the first part of the barium slag raw material on a dry basis is 100:25; S3, 4.77 parts of industrial calcium peroxide powder are added to the first mixture in two portions, and mixed for 10 minutes after each addition; the mass ratio of sodium thiosulfate pentahydrate to industrial calcium peroxide powder is 1:2.65, the CaO2 content of the industrial calcium peroxide powder is 60 wt.%, and the D90 is not greater than 90 μm; after the addition is completed, the mixture is aged at 35°C under non-sealed cover for 10 hours, then stirred and aged at 22°C in an open manner for 2 hours to obtain treated barium slag; the solid feed amount of the treated barium slag is 106.57 parts; S4, taking 100 parts of the solid barium slag to be processed, 52 parts of S95 grade granulated blast furnace slag powder, 21.5 parts of Class F II fly ash, 7 parts of metakaolin, 6.8 parts of sodium metasilicate pentahydrate, and 2.3 parts of anhydrous sodium carbonate are mixed for 3 minutes to obtain a second mixture; the metakaolin contains 52 wt.% SiO2 and 45 wt.% Al2O3, with a total content of 97 wt.% for SiO2 and Al2O3; the sodium metasilicate pentahydrate has a purity of 98 wt.% and the anhydrous sodium carbonate has a purity of 99.5 wt.%. S5, the treated barium slag is mixed with the second mixture, and 12 parts of the second part of water are added in batches based on the amount of solid barium slag being 100 parts, and the mixture is continued to be mixed to obtain the third mixture; S6, the third mixture is pressed into shape under a pressure of 15MPa to obtain a brick blank; the brick blank is sealed and cured at 35℃ for 20h, then moist heat cured at 65℃ and relative humidity of 98% for 8h, and then cured at room temperature at 23℃ for 28d to obtain barium slag-based low-leaching wall brick material.
[0039] Example 4 This embodiment provides a method for preparing a barium slag-based low-leaching wall brick material, the preparation method comprising the following steps: S1, the barium slag is cleaned of impurities, crushed and screened, and the moisture content is adjusted to obtain barium slag raw material; the moisture content of the barium slag raw material is 11.5 wt.%, and the particle size is not greater than 1.8 mm; based on 100 parts of dry weight of the barium slag raw material, the moisture content of the barium slag raw material is 13.00 parts. S2, dissolve 1.1 parts of sodium thiosulfate pentahydrate in 15.00 parts of water in the first part to obtain a first solution; the temperature of the first part of water is 25°C; add the first solution to the barium slag raw material in 3 portions, mixing for 5 minutes after each addition, and continuing to mix for 20 minutes after all the solution has been added, and then let it stand at 22°C for 0.5 hours for pre-permeation treatment to obtain a first mixture; the mass ratio of the barium slag raw material to the total mass of water and water in the first part of the barium slag raw material on a dry basis is 100:28; S3, 3.3 parts of industrial calcium peroxide powder are added to the first mixture in three portions, and mixed for 6.5 minutes after each addition; the mass ratio of sodium thiosulfate pentahydrate to industrial calcium peroxide powder is 1:3.0, the CaO2 content of the industrial calcium peroxide powder is 66 wt.%, and the D90 is not greater than 110 μm; after the addition is completed, the mixture is aged at 22°C under non-sealed cover for 18 hours, then stirred and aged at 15°C in an open environment for 6 hours to obtain treated barium slag; the solid feed amount of the treated barium slag is 104.4 parts; S4, taking 100 parts of the solid barium slag to be processed, 47 parts of S105 grade granulated blast furnace slag powder, 24 parts of Class F II fly ash, 7.5 parts of metakaolin, 5.5 parts of sodium metasilicate pentahydrate, and 2.0 parts of anhydrous sodium carbonate are mixed for 7 minutes to obtain a second mixture; the metakaolin contains 60 wt.% SiO2 and 38 wt.% Al2O3, with a total content of 98 wt.% for SiO2 and Al2O3; the sodium metasilicate pentahydrate has a purity of 97 wt.% and the anhydrous sodium carbonate has a purity of 98.5 wt.%. S5, the treated barium slag is mixed with the second mixture, and 10 parts of the second part of water are added in batches based on the amount of solid barium slag being 100 parts, and the mixture is continued to be mixed to obtain the third mixture; S6, the third mixture is pressed into shape under a pressure of 25MPa to obtain a brick blank; the brick blank is sealed and cured at 20°C for 36h, then moist heat cured at 48°C and relative humidity of 92% for 24h, and then cured at room temperature at 30°C for 14d to obtain barium slag-based low-leaching wall brick material.
[0040] Comparative Example 1 This comparative example provides a method for preparing a barium slag-based low-leaching wall brick material. The difference between this method and Example 1 is that sodium thiosulfate pentahydrate is not added in step S2. Instead, 14.35 parts of the first portion of water are added to the barium slag raw material in three additions, with mixing for 3 minutes after each addition. After all the water is added, mixing continues for 17 minutes. The mixture is then allowed to stand at 28°C for 2 hours to obtain the first mixture. In step S3, the mass ratio of sodium thiosulfate pentahydrate to industrial calcium peroxide powder is no longer limited, and the amount of solid barium slag used is 103.75 parts. The remaining steps and parameters are the same as in Example 1.
[0041] Comparative Example 2 This comparative example provides a method for preparing barium slag-based low-leaching wall brick material. The difference from Example 1 is that the order of adding sodium thiosulfate pentahydrate and industrial calcium peroxide powder is adjusted. In step S2, 3.75 parts of industrial calcium peroxide powder are added to the barium slag raw material in four portions, mixing for 8 minutes after each addition to obtain a first mixture. In step S3, 1.5 parts of sodium thiosulfate pentahydrate are dissolved in 14.35 parts of the first portion of water to obtain a first solution. This first solution is added to the first mixture in three portions, mixing for 3 minutes after each addition. After all the solution is added, mixing continues for 17 minutes. The mixture is then allowed to stand at 28°C for 2 hours, followed by non-sealed aging at 15°C for 14 hours. After stirring, it is left to age in an open environment at 28°C for 4 hours to obtain treated barium slag. The solid feed amount of the treated barium slag is 105.25 parts. The remaining steps and parameters are the same as in Example 1.
[0042] Comparative Example 3 This comparative example provides a method for preparing barium slag-based low-leaching wall brick material. The difference from Example 1 is that in step S2, 1.5 parts of sodium thiosulfate pentahydrate are dissolved in 14.35 parts of water to obtain a first solution. The first solution and 3.75 parts of industrial calcium peroxide powder are divided into four portions each. The corresponding portions of the first solution and industrial calcium peroxide powder are simultaneously added to the barium slag raw material. After each addition, the mixture is mixed for 8 minutes, and after all the material is added, mixing continues for 26 minutes. No static pre-permeation treatment is performed to obtain a first mixture. In step S3, the first mixture is aged at 15°C under non-sealed conditions for 14 hours, then stirred and aged at 28°C in an open environment for 4 hours to obtain treated barium slag. The solid feed amount of the treated barium slag is 105.25 parts. The remaining steps and parameters are the same as in Example 1.
[0043] Comparative Example 4 This comparative example provides a method for preparing barium slag-based low-leaching wall brick material. The difference between this method and Example 1 is that in step S3, 3.75 parts of industrial calcium peroxide powder are added to the first mixture in four batches, and the mixture is stirred for 8 minutes after each addition. After all the powder is added, there is no non-sealed covering aging or open aging. The treated barium slag is directly obtained and then processed in step S4. The amount of solid barium slag added is 105.25 parts. The remaining steps and parameters are the same as in Example 1.
[0044] Comparative Example 5 This comparative example provides a method for preparing barium slag-based low-leaching wall brick material. The difference between this method and Example 1 is that industrial calcium peroxide powder is not added in step S3. The first mixture is aged at 15°C under non-sealed cover for 14 hours, then stirred and aged at 28°C in an open environment for 4 hours to obtain treated barium slag. The mass ratio of sodium thiosulfate pentahydrate to industrial calcium peroxide powder is no longer limited in step S3. The solid feed amount of the treated barium slag is 101.5 parts. The remaining steps and parameters are the same as in Example 1.
[0045] Detection methods Sample pretreatment: After completing the appropriate curing, the barium slag-based low-leaching wall brick materials in each group were placed at a temperature of 20±2℃ and a relative humidity of 60±5% for 48 hours. Barium leaching concentration, compressive strength, water absorption, and efflorescence performance were all tested using wall brick materials that had undergone the above pretreatment and curing. The acidification-released sulfide content was tested using the treated barium slag obtained after S3 and before S4 in each group. Except for the curing conditions explicitly described in the examples and comparative examples, all groups used the same sampling method, sample pretreatment conditions, and testing conditions; the curing conditions for each comparative example were the same as in Example 1.
[0046] Barium leaching concentration test: The leachate was prepared according to the horizontal oscillation method specified in HJ 557—2010, and the barium concentration was determined by inductively coupled plasma atomic emission spectrometry (ICP-AES) according to HJ781—2016. Three wall bricks were randomly selected from each group, and samples were taken from different parts of each brick. The samples were independently crushed and mixed, and all samples were passed through a 3mm sieve. The moisture content of another sample was determined. A sample equivalent to 100.00g of dry sample was weighed and placed in a 2L polyethylene extraction bottle. Grade II water conforming to GB / T 6682 was added at a liquid-to-solid ratio of 10L / kg. The extraction bottle was vertically fixed on a horizontal oscillation device and oscillated at a frequency of 110±10 times / min and an amplitude of 40mm for 8 hours at room temperature, followed by standing for 16 hours. The leachate was filtered through a 0.45μm filter membrane, and the filtrate was acidified with nitric acid to a pH less than 2. The barium concentration was determined using ICP-AES at a wavelength of 455.403nm. One leachate sample was prepared independently for each wall brick, and three samples were tested for each group. The results were taken as the arithmetic mean and expressed in mg / L. If the sample concentration exceeded the range of the standard curve, it was appropriately diluted and tested again.
[0047] Test for sulfide content released during acidification: The test was conducted according to the acidification-blowing-absorption and methylene blue spectrophotometric principles specified in HJ 833—2017. After each group's S3 was completed, equal amounts of samples were immediately taken from the upper, middle, and lower parts of the treated barium slag and mixed. 20.00 g of the sample was weighed and placed in a 500 mL reaction flask, while another sample was taken to determine its dry matter content. 100 mL of deionized water and 5.0 mL of antioxidant solution prepared according to HJ 833—2017 were added to the reaction flask, and 10.0 mL of 10 g / L sodium hydroxide solution was added to the absorption tube. The acidification-blowing-absorption apparatus was connected and its airtightness was checked. The reaction flask was placed in a 100°C water bath, nitrogen gas was introduced, and pre-purged for 5 min. 20 mL of hydrochloric acid solution with a volume ratio of 1:1 was slowly added, and blowing continued for 30 min to allow the released hydrogen sulfide to enter the absorption liquid. The absorbent was prepared by adding N,N-dimethyl-p-phenylenediamine colorimetric solution and ferric ammonium sulfate solution according to HJ 833—2017, and the absorbance was measured at a wavelength of 665 nm. The content of sulfides released during acidification was calculated based on the sulfide standard curve and the dry matter content of the sample. Three parallel samples were tested in each group, and the results were calculated based on the dry weight of the treated barium slag and expressed as sulfur (S), in mg / kg.
[0048] Compressive strength test: The test shall be conducted in accordance with the method specified in GB / T 2542—2012. Ten intact wall bricks shall be randomly selected from each group. The pressure surface shall be treated according to the requirements of the corresponding brick type, ensuring that the specifications, compression direction, and pressure surface treatment of the samples in each group are consistent. The length and width of the pressure surface of the sample shall be measured, and the pressure area shall be calculated. The sample shall be placed centered on the compression testing machine and continuously and uniformly loaded until the sample fails, recording the maximum failure load. The compressive strength shall be calculated by dividing the maximum failure load by the pressure area. The result for each group shall be the arithmetic mean of the 10 samples, expressed in MPa.
[0049] Water absorption test: The test was conducted according to the method specified in GB / T 2542—2012 and under uniform immersion conditions. Five intact wall bricks were randomly selected from each group. The samples were dried at 105±5℃, and weighed every 2 hours. A constant weight was considered achieved when the mass change rate of two consecutive weighings did not exceed 0.2%. After cooling the samples to room temperature, the dried mass m0 was measured. The samples were then completely immersed in deionized water at 20±2℃ for 24 hours, with the upper surface of the sample at least 20 mm below the water surface. The samples were removed, and visible moisture was wiped off with a wrung-out damp cloth. The saturated mass m1 was measured within 2 minutes. The water absorption rate was calculated as (m1-m0) / m0×100%, and the result for each group was the arithmetic mean of the five samples, expressed as a percentage (%).
[0050] Efflorescence performance test: Following the principle of the efflorescence test for wall tiles specified in GB / T 2542—2012, and using a unified area grading method for evaluation. Five wall tiles with intact appearance were randomly selected from each group. After removing surface dust, they were placed vertically in a flat-bottomed container, and deionized water at 20±2℃ was added, ensuring the water level was 20mm from the bottom of the sample. During the test, the water depth was maintained at 20±2mm. The samples were placed in an environment of 20±2℃ and 60±5% relative humidity for 7 days, and then placed in the same environment for another 48 hours. The white efflorescence, powdering, and peeling on all surfaces except the bottom were observed, and the proportion of efflorescence area was estimated using a 10mm×10mm transparent grid. No visible salting-out material is recorded as Grade 0; a salting-out area ratio greater than 0 and not greater than 5% is recorded as Grade I; a salting-out area ratio greater than 5% and not greater than 20% is recorded as Grade II; a salting-out area ratio greater than 20% and not greater than 50% is recorded as Grade III; a salting-out area ratio greater than 50% or the presence of surface powdering or peeling is recorded as Grade IV. The highest grade among the five samples in each group is taken as the efflorescence grade for that group. The above grades are the unified comparative evaluation grades used in this test.
[0051] The test results are shown in Tables 1 and 2.
[0052] Table 1. Test results of barium leaching concentration of wall bricks and sulfide content released by acidification of treated barium slag.
[0053] Note: The barium leaching concentration is measured on the wall bricks after curing; the acidification-released sulfide content is measured on the treated barium slag obtained after S3 and before entering S4.
[0054] Table 2. Test results of compressive strength, water absorption and efflorescence performance
[0055] Note: The frost rating is the unified comparative evaluation rating used in this test.
[0056] As shown in Tables 1 and 2, compared with Example 1, the barium leaching concentration and water absorption rate of Comparative Example 1 increased, while the content of sulfides released by acidification and the compressive strength decreased, and the efflorescence grade remained unchanged. This is because Comparative Example 1 did not add sodium thiosulfate pentahydrate, and the industrial calcium peroxide powder could still oxidize some of the sulfides in the barium slag. At the same time, without the addition of sodium thiosulfate pentahydrate, the oxidation capacity of the industrial calcium peroxide powder may be used more for the oxidation of the original sulfides in the barium slag, resulting in a lower content of sulfides released by acidification. However, there was a lack of a reaction pathway for thiosulfate ions to enter the internal pores of the barium slag and form sulfate ions during subsequent oxidation. The migratory barium inside the particles was not sufficiently fixed, leading to an increase in the barium leaching concentration.
[0057] In Comparative Example 2, the barium leaching concentration, acidification-released sulfide content, and water absorption rate increased, while the compressive strength decreased and the efflorescence grade increased from Grade I to Grade II. This is because the industrial calcium peroxide powder first comes into contact with the barium slag, which may cause the oxidation reaction to occur preferentially on the particle surface and pores, which is not conducive to the full migration of the subsequently added sodium thiosulfate pentahydrate aqueous solution into the particle interior, resulting in insufficient fixation of the migratable barium inside the particle and insufficient oxidation treatment of sulfides.
[0058] Compared with Comparative Example 3, the barium leaching concentration, acidification-released sulfide content, and water absorption rate increased, the compressive strength decreased, and the efflorescence grade increased from Grade I to Grade II. This is because the sodium thiosulfate pentahydrate aqueous solution and industrial calcium peroxide powder were added at the same time without static pre-permeation. Some thiosulfate ions may undergo oxidation reaction before fully entering the internal pores of the barium slag, causing the transformation of sulfur-containing species and the precipitation and fixation of barium to be more concentrated on the outside of the particles, thus weakening the fixation effect of pre-permeation treatment on the migratable barium inside the particles.
[0059] In Comparative Example 4, the barium leaching concentration, acidification-released sulfide content, and water absorption rate increased, while the compressive strength decreased and the efflorescence grade increased from Grade I to Grade III. This is because after the cancellation of non-enclosed covering aging and open aging, the industrial calcium peroxide powder did not receive sufficient time for hydrolysis, oxidation reaction, and decomposition of residual active substances, resulting in insufficient treatment of sulfides and migratable barium in the barium slag. At the same time, residual active substances may continue to react during subsequent water addition, pressing, and curing processes, leading to an increase in pores and interconnected pores inside the brick.
[0060] Compared with Comparative Example 5, the barium leaching concentration, acidification-released sulfide content, and water absorption rate increased, the compressive strength decreased, and the efflorescence grade increased from Grade I to Grade IV. This is because no industrial calcium peroxide powder was added, the thiosulfate ions that pre-permeated into the pores of the barium slag were not fully oxidized, and the original sulfides in the barium slag were not fully transformed into forms that are not easily released by acidification. The generation of highly oxidized sulfur-containing species such as sulfate ions was insufficient, which was not conducive to the fixation of barium in the form of insoluble barium-containing phases. At the same time, the soluble sulfur-containing species and sodium salts remaining in the system may migrate to the surface of the brick with water and precipitate, thereby aggravating the efflorescence.
[0061] The above description is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention fall within the protection and disclosure scope of the present invention.
Claims
1. A barium-slag based low leaching wall tile material, characterized in that, It is made by mixing, pressing and curing barium slag, granulated blast furnace slag powder, fly ash, metakaolin, sodium metasilicate pentahydrate and anhydrous sodium carbonate; The mass ratio of the solid feed amount of the barium slag, granulated blast furnace slag powder, fly ash, metakaolin, sodium metasilicate pentahydrate, and anhydrous sodium carbonate is 100:(45-52):(20-24):(7-9):(5.5-7.5):(1.8-2.3). The treated barium slag is obtained by first pre-permeating barium slag raw material with an aqueous solution of sodium thiosulfate pentahydrate, and then oxidizing and aging it with industrial calcium peroxide powder. The mass ratio of the barium slag raw material to sodium thiosulfate pentahydrate is 100:(0.8-1.8) on a dry basis, and the mass ratio of sodium thiosulfate pentahydrate to industrial calcium peroxide powder is 1:(2.5-3.0). The CaO2 content in the industrial calcium peroxide powder is 60-75 wt.%. The amount of solid feed material for the treated barium slag is the sum of the dry basis mass of the barium slag raw material, the mass of sodium thiosulfate pentahydrate, and the mass of industrial calcium peroxide powder added when preparing the treated barium slag. The raw materials for preparing the barium slag-based low-leaching wall brick material do not contain additional silicate cement clinker, cement containing silicate cement clinker, sulfoaluminate cement, dihydrate gypsum, hemihydrate gypsum, or anhydrous gypsum.
2. The barium-slag-based low leaching wall tile material according to claim 1, characterized in that, The granulated blast furnace slag powder is selected from at least one of S95 grade granulated blast furnace slag powder and S105 grade granulated blast furnace slag powder; the fly ash is Class F, Grade II fly ash; the metakaolin contains 50-60 wt.% SiO2, 35-45 wt.% Al2O3, and a total content of 85-98 wt.% SiO2 and Al2O3.
3. The barium-slag-based low leaching wall tile material according to claim 1, wherein, The purity of the sodium metasilicate pentahydrate is not less than 95 wt.%, the purity of the anhydrous sodium carbonate is not less than 98 wt.%, and the D90 of the industrial calcium peroxide powder is not greater than 150 μm.
4. A process for the production of a barium-slag based low leaching wall tile material according to any one of claims 1 to 3, characterized in that, Includes the following steps: S1, the barium slag is cleaned of impurities, crushed and screened, and the moisture content is adjusted to obtain barium slag raw material; S2, dissolve sodium thiosulfate pentahydrate in the first portion of water to obtain the first solution, add the first solution to the barium slag raw material in batches and mix, let stand for pre-permeation treatment to obtain the first mixture; S3, add industrial calcium peroxide powder to the first mixture in batches and mix, carry out non-sealed covering aging, stir and then carry out open aging to obtain treated barium slag; S4, granulated blast furnace slag powder, fly ash, metakaolin, sodium metasilicate pentahydrate and anhydrous sodium carbonate are mixed to obtain a second mixture; S5, the treated barium slag is mixed with the second mixture, a second portion of water is added in batches and mixing is continued to obtain a third mixture; S6, the third mixture is pressed into shape to obtain a brick blank, and the brick blank is subjected to sealed curing, moist heat curing and room temperature curing in sequence to obtain barium slag-based low leaching wall brick material.
5. The method of producing a barium residue based low leaching wall tile material according to claim 4, characterized in that, In S1, the barium slag raw material has a moisture content of 10-15 wt.% and a particle size of no more than 2 mm.
6. The method of producing a barium residue based low leaching wall tile material according to claim 4, characterized in that, In S2, the mass ratio of the barium slag raw material to the total mass of the water and the first portion of water contained in the barium slag raw material, based on dry weight, is 100:(25-35). The temperature of the first portion of water is 20-35℃. The first solution is added in 2-4 portions, and mixed for 3-8 minutes after each addition. After all the solution is added, mixing continues for 10-20 minutes. The settling temperature is 15-35℃ and the settling time is 0.5-2 hours.
7. The method of producing a barium residue based low leaching wall tile material according to claim 4, characterized in that, In S3, the D90 of the industrial calcium peroxide powder is not greater than 150 μm; The industrial calcium peroxide powder is added in 2-4 batches, and mixed for 5-10 minutes after each addition; the non-sealed covered aging temperature is 15-35℃ and the time is 6-18 hours; the open aging temperature is 15-35℃ and the time is 2-8 hours.
8. The method of producing a barium residue based low leaching wall tile material according to claim 4, characterized in that, In S4, the mixing time of the granulated blast furnace slag powder, fly ash, metakaolin, sodium metasilicate pentahydrate and anhydrous sodium carbonate is 3-10 min.
9. The method of producing a barium residue based low leaching wall tile material according to claim 4, characterized in that, In S6, the pressure for pressing is 15-30 MPa.
10. The method of producing a barium residue based low leaching wall tile material according to claim 4, characterized in that, In S6, the temperature for sealing curing is 20-35℃ and the time is 12-36h; the temperature for damp heat curing is 40-65℃ and the relative humidity is not less than 90% for 8-24h; and the temperature for room temperature curing is 20-30℃ and the time is 7-28d.