A method for designing the mix proportion of hydraulic asphalt concrete suitable for high-altitude and high-intensity frigid zones.

By using modified composite fibers and functional additives, the mix proportions of hydraulic asphalt concrete are optimized, solving the problem of adaptability to multiple extreme environments in high-altitude and high-temperature zones, improving impermeability and mechanical properties, and making it suitable for key components such as dams of high-altitude pumped storage power stations.

CN123106072APending Publication Date: 2026-11-17CHINA THREE GORGES PROJECTS DEV CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611198353.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-07
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing hydraulic asphalt concrete technology lacks systematic solutions for multiple extreme environments, including high altitude, low temperature, large temperature difference, strong ultraviolet radiation, and high seismic loads, and cannot effectively adapt to complex geological conditions.

Method used

Modified composite fibers and functional additives were used, and the proportions of coarse aggregate, fine aggregate, filler and asphalt were optimized through chemical structure design and nanocomposite reinforcement. Combined with L9(33) orthogonal array and field test, hydraulic asphalt concrete suitable for high-altitude and high-intensity areas was prepared.

Benefits of technology

It improves the impermeability, cold resistance and mechanical strength of asphalt concrete, and can maintain the integrity and functionality of the seepage prevention structure under extreme conditions. It is suitable for key parts such as seepage prevention panels, leveling cementing layers and sealing layers of pumped storage power station dams at high altitudes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to the field of asphalt concrete technology, and discloses a hydraulic asphalt concrete suitable for high-altitude and high-intensity seismic zones, along with its mix design method. The hydraulic asphalt concrete comprises the following raw materials in parts by weight: 40-55 parts coarse aggregate, 30-48 parts fine aggregate, 10-15 parts filler, 6.5-8.5 parts asphalt, 0.1-0.5 parts modified composite fiber, and 0.1-0.5 parts functional additives. The modified composite fiber is prepared by pretreating lignin fiber and polypropylene fiber with silane, grafting with maleic anhydride, crosslinking with bisoxazoline, and vacuum composite with nano-montmorillonite. The hydraulic asphalt concrete of this invention exhibits good impermeability, low-temperature resistance, and mechanical strength, making it suitable for projects such as seepage prevention panels for high-altitude pumped storage power stations.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of asphalt concrete technology, specifically to a hydraulic asphalt concrete suitable for high-altitude and high-intensity areas and its mix design method. Background Technology

[0002] Hydraulic asphalt concrete, due to its excellent impermeability, good deformation adaptability, and unique self-healing crack capacity, has become the preferred material for reservoir and dam seepage prevention in complex geological conditions such as weak rock strata, thick overburden, and high-altitude permafrost. These regions generally possess multiple environmental characteristics, including high altitude, strong ultraviolet radiation, extreme low temperatures, large diurnal temperature differences, and high seismic intensity, which place stringent requirements on the material formulation and construction technology of asphalt concrete. Existing hydraulic asphalt concrete technology is mainly designed for single extreme conditions, such as considering low-temperature crack resistance in frigid regions or seismic deformation resistance in high-intensity areas, lacking a systematic material solution for the coupled effects of high altitude, low temperature, large temperature differences, strong ultraviolet radiation, and strong seismic activity. Therefore, there is an urgent need to develop a hydraulic asphalt concrete material that can systematically adapt to multiple extreme environments of high altitude, low temperature, large temperature difference, strong ultraviolet radiation, and high seismic intensity. Summary of the Invention

[0003] (a) Technical problems to be solved

[0004] To address the shortcomings of existing technologies, this invention provides a method for designing the mix proportion of hydraulic asphalt concrete suitable for high-altitude and high-intensity frigid zones.

[0005] (II) Technical Solution

[0006] To achieve the above objectives, the present invention provides the following technical solution:

[0007] In a first aspect, a hydraulic asphalt concrete suitable for high-altitude and high-intensity climate zones comprises the following raw materials in parts by weight:

[0008] 40-55 parts coarse aggregate, 30-48 parts fine aggregate, 10-15 parts filler, 6.5-8.5 parts asphalt, 0.1-0.5 parts modified composite fiber, and 0.1-0.5 parts functional additives;

[0009] The modified composite fiber is prepared by cross-linking pretreated lignin fiber and modified polypropylene fiber with 2,2'-bis(2-oxazoline), and then modifying it with nano-montmorillonite and fatty alcohol polyoxyethylene ether.

[0010] Furthermore, the coarse aggregate is basalt with a particle size of 5~20 mm, a crushing value of ≤26%, and a water absorption rate of ≤2.0%.

[0011] Furthermore, the fine aggregate is manufactured sand; the fineness modulus of the manufactured sand is 2.6~3.0, and the mud content is ≤1.0%.

[0012] Furthermore, the filler is limestone powder with a particle size ≤0.075 mm, a hydrophilicity coefficient <1.0, and a specific surface area ≥300 m² / kg.

[0013] Furthermore, the functional additives include a waterproofing agent and an anti-stripping agent; the waterproofing agent is an organosilicon-based waterproofing agent, and the dosage is 40-60% of the total mass of the functional additives; the anti-stripping agent is an amine-based anti-stripping agent, and the dosage is 40-60% of the total mass of the functional additives.

[0014] Furthermore, the preparation method of the modified composite fiber includes the following steps:

[0015] A1. Immerse 100-120 parts of lignin fiber in 300-500 parts of 3-5% methyltriethoxysilane solution, stir at 60-70℃ for 30-60 min, and cure with nitrogen at 100-120℃ for 40-50 min to obtain pretreated lignin fiber; wash 60-80 parts of polypropylene fiber with 300-500 parts of ethanol-deionized water (volume ratio 1:3) for 20-30 min, immerse in 200-400 parts of 5-8% maleic anhydride acetone solution, soak at 50-60℃ for 30-60 min, and vacuum dry at 70-80℃ for 4-6 h to obtain modified polypropylene fiber;

[0016] A2. Mix 80-100 parts of pretreated lignin fiber and 40-60 parts of modified polypropylene fiber and immerse them in 300-500 parts of 5-8% (w / w) 2,2'-bis(2-oxazoline)acetone solution. Add 0.5-1.2 parts of sodium methoxide and stir at 100-120℃ for 1-2 h under nitrogen protection. Remove the fiber and cure it at 120-130℃ under nitrogen protection for 40-50 min. Use a low-temperature airflow pulverizer to break up the fiber bundle at 30-40℃ and airflow pressure of 0.6-0.8 MPa to obtain cross-linked fiber.

[0017] A3. Add 100-150 parts of cross-linked fiber to 400-600 parts of deionized water, add 5-20 parts of nano-montmorillonite and 1-5 parts of fatty alcohol polyoxyethylene ether, ultrasonically disperse at 300-500 W for 40-50 min, place in a vacuum tank, evacuate to ≤10 Pa, soak for 10-20 min, pressurize at 0.25-0.3 MPa for 30-60 min, and cure under nitrogen protection at 130-140℃ for 40-50 min to obtain modified composite fiber.

[0018] A second aspect of the present invention provides a method for preparing hydraulic asphalt concrete suitable for high-altitude and high-intensity seismic zones, comprising the following steps:

[0019] S1. Place the coarse aggregate, fine aggregate, and filler into the mixing equipment and dry mix for 2-3 minutes.

[0020] S2. Slowly add the asphalt heated to 155~170℃ to the dry material in step S1, and mix at a constant temperature of 140~160℃ for 3~4 minutes.

[0021] S3. The modified composite fiber is evenly sprinkled into the mixing system of step S2 in two batches. After each addition, the mixture is mixed for 1 to 2 minutes. Then, the functional additives are added and the mixture is mixed for another 1 to 2 minutes to obtain the mixture.

[0022] S4. After mixing, immediately discharge the mixture, controlling the discharge temperature to 140~160℃, and compact it using a rolling mill until the compaction degree is ≥96%;

[0023] S5. After molding, allow it to cure naturally for 24-48 hours. During the curing period, avoid rainwater erosion and external impact. Once curing is complete, it can be put into subsequent construction or use.

[0024] A third aspect of the present invention provides a method for designing the mix proportions of hydraulic asphalt concrete suitable for high-altitude and high-intensity frigid zones, comprising the following steps:

[0025] a. Calibrate the properties of the raw materials described in claims 1 to 6 according to the SL / T 501-2025 standard, and determine the discontinuous gradation range of coarse aggregate and fine aggregate;

[0026] b. Using L9(3) 3 An orthogonal array was used to optimize the baseline mix proportion using factors such as the oil-aggregate ratio, gradation index, and filler content.

[0027] c. Adjust the amount of asphalt and the amount of modified composite fiber to enhance the seismic deformation resistance of hydraulic asphalt concrete and adapt it to the needs of use in high-altitude and high-intensity seismic zones.

[0028] d. Verify the suitability of the mix proportion through on-site paving tests, and revise and determine the final construction mix proportion in conjunction with the construction parameters of the preparation method described in claim 7.

[0029] Furthermore, the factor levels for the orthogonal experiment described in step b are set as follows: oil-aggregate ratio 6.5%, 7.5%, 8.5%; gradation index 0.35, 0.38, 0.41; filler content 10%, 12%, 14%.

[0030] (iii) Beneficial technical effects

[0031] This invention provides a hydraulic asphalt concrete suitable for high-altitude and high-intensity cold regions. Through the chemical structure design and nanocomposite reinforcement of modified composite fibers, interfacial strengthening of the chemical bonding layer between the fibers and the asphalt matrix is ​​achieved, enabling the fibers to effectively exert toughening and crack-resistant effects even under extreme low-temperature service conditions. The preparation process of the modified composite fibers involves pretreating lignin fibers with methyltriethoxysilane to introduce active silanol groups, while simultaneously modifying polypropylene fibers with maleic anhydride grafting to introduce anhydride active sites. A stable covalent cross-linked network is then formed between the fibers using 2,2'-bis(2-oxazoline). Nano-montmorillonite is then used in a vacuum pressure impregnation process to fully fill the surface micropores and internal voids of the cross-linked fibers, further enhancing the overall strength of the fibers and their affinity with asphalt. This invention uses range analysis and variance analysis to determine the optimal combination of three key parameters: asphalt-aggregate ratio, gradation index, and filler content, providing a quantitative decision-making basis for engineering applications. This invention effectively improves the impermeability, cold resistance, and mechanical strength of asphalt concrete by adjusting the proportions of coarse aggregate, fine aggregate, filler, asphalt, modified composite fiber, and functional additives. It can maintain the integrity and functionality of the impermeable structure for a long time under low temperature, large temperature difference, strong ultraviolet radiation, and seismic loads, and is suitable for the long-term service requirements of key parts such as the impermeable panel, leveling cementing layer, and sealing layer of high-altitude pumped storage power station dams. Detailed Implementation

[0032] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0033] Unless otherwise specified, all components of the hydraulic asphalt concrete formula of this invention are commercially available.

[0034] All parts used in this invention are parts by weight;

[0035] Lignin fibers are granular lignin fibers with a fiber length ≤ 6 mm;

[0036] The polypropylene fiber is a bundle of monofilament polypropylene fibers, 10 mm in length, 30 μm in diameter, and 0.91 g / cm³. 3 Purchased from Shenzhen Weitenai New Materials Co., Ltd.

[0037] Nano-montmorillonite purity ≥98%, particle size ≤10 μm, specific surface area ≥30 m² 2 / g, purchased from Zhejiang Fenghong New Materials Co., Ltd.;

[0038] The organosilicon waterproofing agent in the functional additives is sodium methylsilicate, which was purchased from Jinan Hualu Chemical Co., Ltd.

[0039] The anti-stripping agent is a polyamide-based asphalt anti-stripping agent, purchased from Lurui Engineering Materials Co., Ltd.

[0040] A type of hydraulic asphalt concrete suitable for high-altitude and high-intensity climate zones comprises the following raw materials in parts by weight:

[0041] 40-55 parts coarse aggregate, 30-48 parts fine aggregate, 10-15 parts filler, 6.5-8.5 parts asphalt, 0.1-0.5 parts modified composite fiber, and 0.1-0.5 parts functional additives.

[0042] The coarse aggregate is basalt with a particle size of 5~20 mm, a crushing value of ≤26%, and a water absorption rate of ≤2.0%.

[0043] The fine aggregate is manufactured sand; the fineness modulus of the manufactured sand is 2.6~3.0 and the mud content is ≤1.0%.

[0044] The filler is limestone powder with a particle size ≤0.075 mm, a hydrophilicity coefficient <1.0, and a specific surface area ≥300 m² / kg.

[0045] The functional additives include a waterproofing agent and an anti-peeling agent; the waterproofing agent is an organosilicon-based waterproofing agent, and the dosage is 40-60% of the total mass of the functional additives; the anti-peeling agent is an amine-based anti-peeling agent, and the dosage is 40-60% of the total mass of the functional additives.

[0046] The method for preparing the modified composite fiber includes the following steps:

[0047] A1. Immerse 100-120 parts of lignin fiber in 300-500 parts of 3-5% methyltriethoxysilane solution, stir at 60-70℃ for 30-60 min, and cure with nitrogen at 100-120℃ for 40-50 min to obtain pretreated lignin fiber; wash 60-80 parts of polypropylene fiber with 300-500 parts of ethanol-deionized water (volume ratio 1:3) for 20-30 min, immerse in 200-400 parts of 5-8% maleic anhydride acetone solution, soak at 50-60℃ for 30-60 min, and vacuum dry at 70-80℃ for 4-6 h to obtain modified polypropylene fiber;

[0048] A2. Mix 80-100 parts of pretreated lignin fiber and 40-60 parts of modified polypropylene fiber and immerse them in 300-500 parts of 5-8% (w / w) 2,2'-bis(2-oxazoline)acetone solution. Add 0.5-1.2 parts of sodium methoxide and stir at 100-120℃ for 1-2 h under nitrogen protection. Remove the fiber and cure it at 120-130℃ under nitrogen protection for 40-50 min. Use a low-temperature airflow pulverizer to break up the fiber bundle at 30-40℃ and airflow pressure of 0.6-0.8 MPa to obtain cross-linked fiber.

[0049] A3. Add 100-150 parts of cross-linked fiber to 400-600 parts of deionized water, add 5-20 parts of nano-montmorillonite and 1-5 parts of fatty alcohol polyoxyethylene ether, ultrasonically disperse at 300-500 W for 40-50 min, place in a vacuum tank, evacuate to ≤10 Pa, soak for 10-20 min, pressurize at 0.25-0.3 MPa for 30-60 min, and cure under nitrogen protection at 130-140℃ for 40-50 min to obtain modified composite fiber.

[0050] A method for preparing hydraulic asphalt concrete suitable for high-altitude and high-intensity seismic zones includes the following steps:

[0051] S1. Place the coarse aggregate, fine aggregate, and filler into the mixing equipment and dry mix for 2-3 minutes.

[0052] S2. Slowly add the asphalt heated to 155~170℃ to the dry material in step S1, and mix at a constant temperature of 140~160℃ for 3~4 minutes.

[0053] S3. The modified composite fiber is evenly sprinkled into the mixing system of step S2 in two batches. After each addition, the mixture is mixed for 1 to 2 minutes. Then, the functional additives are added and the mixture is mixed for another 1 to 2 minutes to obtain the mixture.

[0054] S4. After mixing, immediately discharge the mixture, controlling the discharge temperature to 140~160℃, and compact it using a rolling mill until the compaction degree is ≥96%;

[0055] S5. After molding, allow it to cure naturally for 24-48 hours. During the curing period, avoid rainwater erosion and external impact. Once curing is complete, it can be put into subsequent construction or use.

[0056] A method for mix design of hydraulic asphalt concrete suitable for high-altitude and high-intensity seismic zones includes the following steps:

[0057] a. Calibrate the properties of the raw materials described in claims 1 to 6 according to the SL / T 501-2025 standard, and determine the discontinuous gradation range of coarse aggregate and fine aggregate;

[0058] b. Using L9(3)3 An orthogonal array was used to optimize the baseline mix proportions using factors such as asphalt-aggregate ratios of 6.5%, 7.5%, and 8.5%; gradation indices of 0.35, 0.38, and 0.41; and filler contents of 10%, 12%, and 14%.

[0059] c. Adjust the amount of asphalt and the amount of modified composite fiber to enhance the seismic deformation resistance of hydraulic asphalt concrete and adapt it to the needs of use in high-altitude and high-intensity seismic zones.

[0060] d. Verify the suitability of the mix proportion through on-site paving tests, and revise and determine the final construction mix proportion in conjunction with the construction parameters of the preparation method described in claim 7.

[0061] Orthogonal experimental design: The oil-aggregate ratio (A), gradation index (B), and filler content (C) were selected as the three factors in the orthogonal experiment. Each factor had three levels, and the L9(3) model was used. 3 Orthogonal array.

[0062] Table 1 Orthogonal array

[0063] level A: Oil-stone ratio (%) B: Grading Index C: Filler content (%) 1 6.5 0.35 10 2 7.5 0.38 12 3 8.5 0.41 14

[0064] The remaining parameters are fixed as follows:

[0065] Coarse aggregate: Fine aggregate mass ratio is 50:40, modified composite fiber: 0.3 parts, functional additives: 0.3 parts (organosilicon waterproofing agent 60% + amine anti-stripping agent 40%).

[0066] Example 1: Grain distribution index 0.35

[0067] A method for preparing hydraulic asphalt concrete suitable for high-altitude and high-intensity seismic zones includes the following steps:

[0068] S1. Place 50 parts coarse aggregate, 40 parts fine aggregate, and 10 parts filler into the mixing equipment and dry mix for 2 minutes.

[0069] S2. Slowly add 6.5 parts of asphalt heated to 160℃ to the dry material in step S1, and mix at a constant temperature of 160℃ for 3 minutes.

[0070] S3. Add 0.3 parts of modified composite fiber evenly to the mixing system in step S2 in two batches. Mix for 2 minutes after each addition. Then add 0.3 parts of functional additive and continue mixing for 1 minute to obtain the mixture.

[0071] S4. After mixing, immediately discharge the mixture, controlling the discharge temperature at 160℃, and compact it using a rolling mill until the compaction degree is ≥96%;

[0072] S5. After molding, allow it to cure naturally for 48 hours. During the curing period, avoid rainwater erosion and external impact. Once curing is complete, it can be put into subsequent construction or use.

[0073] Example 2: Grain distribution index 0.38

[0074] A method for preparing hydraulic asphalt concrete suitable for high-altitude and high-intensity seismic zones includes the following steps:

[0075] S1. Place 50 parts coarse aggregate, 40 parts fine aggregate, and 10 parts filler into the mixing equipment and dry mix for 2 minutes.

[0076] S2. Slowly add 7.5 parts of asphalt heated to 160℃ to the dry material in step S1, and mix at a constant temperature of 160℃ for 3 minutes.

[0077] S3. Add 0.3 parts of modified composite fiber evenly to the mixing system in step S2 in two batches. Mix for 2 minutes after each addition. Then add 0.3 parts of functional additive and continue mixing for 1 minute to obtain the mixture.

[0078] S4. After mixing, immediately discharge the mixture, controlling the discharge temperature at 160℃, and compact it using a rolling mill until the compaction degree is ≥96%;

[0079] S5. After molding, allow it to cure naturally for 48 hours. During the curing period, avoid rainwater erosion and external impact. Once curing is complete, it can be put into subsequent construction or use.

[0080] Example 3: Gradation index 0.41

[0081] A method for preparing hydraulic asphalt concrete suitable for high-altitude and high-intensity seismic zones includes the following steps:

[0082] S1. Place 50 parts coarse aggregate, 40 parts fine aggregate, and 10 parts filler into the mixing equipment and dry mix for 2 minutes.

[0083] S2. Slowly add 8.5 parts of asphalt heated to 160℃ to the dry material in step S1, and mix at a constant temperature of 160℃ for 3 minutes.

[0084] S3. Add 0.3 parts of modified composite fiber evenly to the mixing system in step S2 in two batches. Mix for 2 minutes after each addition. Then add 0.3 parts of functional additive and continue mixing for 1 minute to obtain the mixture.

[0085] S4. After mixing, immediately discharge the mixture, controlling the discharge temperature at 160℃, and compact it using a rolling mill until the compaction degree is ≥96%;

[0086] S5. After molding, allow it to cure naturally for 48 hours. During the curing period, avoid rainwater erosion and external impact. Once curing is complete, it can be put into subsequent construction or use.

[0087] Example 4: Gradation index 0.35

[0088] A method for preparing hydraulic asphalt concrete suitable for high-altitude and high-intensity seismic zones includes the following steps:

[0089] S1. Place 50 parts coarse aggregate, 40 parts fine aggregate, and 12 parts filler into the mixing equipment and dry mix for 2 minutes.

[0090] S2. Slowly add 8.5 parts of asphalt heated to 160℃ to the dry material in step S1, and mix at a constant temperature of 160℃ for 3 minutes.

[0091] S3. Add 0.3 parts of modified composite fiber evenly to the mixing system in step S2 in two batches. Mix for 2 minutes after each addition. Then add 0.3 parts of functional additive and continue mixing for 1 minute to obtain the mixture.

[0092] S4. After mixing, immediately discharge the mixture, controlling the discharge temperature at 160℃, and compact it using a rolling mill until the compaction degree is ≥96%;

[0093] S5. After molding, allow it to cure naturally for 48 hours. During the curing period, avoid rainwater erosion and external impact. Once curing is complete, it can be put into subsequent construction or use.

[0094] Example 5: Grain distribution index 0.38

[0095] A method for preparing hydraulic asphalt concrete suitable for high-altitude and high-intensity seismic zones includes the following steps:

[0096] S1. Place 50 parts coarse aggregate, 40 parts fine aggregate, and 12 parts filler into the mixing equipment and dry mix for 2 minutes.

[0097] S2. Slowly add 6.5 parts of asphalt heated to 160℃ to the dry material in step S1, and mix at a constant temperature of 160℃ for 3 minutes.

[0098] S3. Add 0.3 parts of modified composite fiber evenly to the mixing system in step S2 in two batches. Mix for 2 minutes after each addition. Then add 0.3 parts of functional additive and continue mixing for 1 minute to obtain the mixture.

[0099] S4. After mixing, immediately discharge the mixture, controlling the discharge temperature at 160℃, and compact it using a rolling mill until the compaction degree is ≥96%;

[0100] S5. After molding, allow it to cure naturally for 48 hours. During the curing period, avoid rainwater erosion and external impact. Once curing is complete, it can be put into subsequent construction or use.

[0101] Example 6: Gradation index 0.41

[0102] A method for preparing hydraulic asphalt concrete suitable for high-altitude and high-intensity seismic zones includes the following steps:

[0103] S1. Place 50 parts coarse aggregate, 40 parts fine aggregate, and 12 parts filler into the mixing equipment and dry mix for 2 minutes.

[0104] S2. Slowly add 7.5 parts of asphalt heated to 160℃ to the dry material in step S1, and mix at a constant temperature of 160℃ for 3 minutes.

[0105] S3. Add 0.3 parts of modified composite fiber evenly to the mixing system in step S2 in two batches. Mix for 2 minutes after each addition. Then add 0.3 parts of functional additive and continue mixing for 1 minute to obtain the mixture.

[0106] S4. After mixing, immediately discharge the mixture, controlling the discharge temperature at 160℃, and compact it using a rolling mill until the compaction degree is ≥96%;

[0107] S5. After molding, allow it to cure naturally for 48 hours. During the curing period, avoid rainwater erosion and external impact. Once curing is complete, it can be put into subsequent construction or use.

[0108] Example 7: Gradation index 0.35

[0109] A method for preparing hydraulic asphalt concrete suitable for high-altitude and high-intensity seismic zones includes the following steps:

[0110] S1. Place 50 parts coarse aggregate, 40 parts fine aggregate, and 14 parts filler into the mixing equipment and dry mix for 2 minutes.

[0111] S2. Slowly add 7.5 parts of asphalt heated to 160℃ to the dry material in step S1, and mix at a constant temperature of 160℃ for 3 minutes.

[0112] S3. Add 0.3 parts of modified composite fiber evenly to the mixing system in step S2 in two batches. Mix for 2 minutes after each addition. Then add 0.3 parts of functional additive and continue mixing for 1 minute to obtain the mixture.

[0113] S4. After mixing, immediately discharge the mixture, controlling the discharge temperature at 160℃, and compact it using a rolling mill until the compaction degree is ≥96%;

[0114] S5. After molding, allow it to cure naturally for 48 hours. During the curing period, avoid rainwater erosion and external impact. Once curing is complete, it can be put into subsequent construction or use.

[0115] Example 8: Grain distribution index 0.38

[0116] A method for preparing hydraulic asphalt concrete suitable for high-altitude and high-intensity seismic zones includes the following steps:

[0117] S1. Place 50 parts coarse aggregate, 40 parts fine aggregate, and 14 parts filler into the mixing equipment and dry mix for 2 minutes.

[0118] S2. Slowly add 8.5 parts of asphalt heated to 160℃ to the dry material in step S1, and mix at a constant temperature of 160℃ for 3 minutes.

[0119] S3. Add 0.3 parts of modified composite fiber evenly to the mixing system in step S2 in two batches. Mix for 2 minutes after each addition. Then add 0.3 parts of functional additive and continue mixing for 1 minute to obtain the mixture.

[0120] S4. After mixing, immediately discharge the mixture, controlling the discharge temperature at 160℃, and compact it using a rolling mill until the compaction degree is ≥96%;

[0121] S5. After molding, allow it to cure naturally for 48 hours. During the curing period, avoid rainwater erosion and external impact. Once curing is complete, it can be put into subsequent construction or use.

[0122] Example 9: Gradation index 0.41

[0123] A method for preparing hydraulic asphalt concrete suitable for high-altitude and high-intensity seismic zones includes the following steps:

[0124] S1. Place 50 parts coarse aggregate, 40 parts fine aggregate, and 14 parts filler into the mixing equipment and dry mix for 2 minutes.

[0125] S2. Slowly add 6.5 parts of asphalt heated to 160℃ to the dry material in step S1, and mix at a constant temperature of 160℃ for 3 minutes.

[0126] S3. Add 0.3 parts of modified composite fiber evenly to the mixing system in step S2 in two batches. Mix for 2 minutes after each addition. Then add 0.3 parts of functional additive and continue mixing for 1 minute to obtain the mixture.

[0127] S4. After mixing, immediately discharge the mixture, controlling the discharge temperature at 160℃, and compact it using a rolling mill until the compaction degree is ≥96%;

[0128] S5. After molding, allow it to cure naturally for 48 hours. During the curing period, avoid rainwater erosion and external impact. Once curing is complete, it can be put into subsequent construction or use.

[0129] The preparation method of the modified composite fiber includes the following steps (general for Examples 1-9):

[0130] A1. 100 parts of lignin fiber were immersed in 400 parts of 3% methyltriethoxysilane solution, stirred at 60°C for 30 min, and cured under nitrogen at 100°C for 40 min to obtain pretreated lignin fiber; 60 parts of polypropylene fiber were washed with 300 parts of ethanol-deionized water (volume ratio 1:3) for 20 min, immersed in 200 parts of 5% maleic anhydride acetone solution, soaked at 60°C for 60 min, and vacuum dried at 80°C for 4 h to obtain modified polypropylene fiber.

[0131] A2. Mix 80 parts of pretreated lignin fiber and 40 parts of modified polypropylene fiber and immerse them in 500 parts of 5% (w / w) 2,2'-bis(2-oxazoline)acetone solution. Add 0.5 parts of sodium methoxide and stir at 100°C for 2 h under nitrogen protection. Remove the fiber and cure it at 120°C under nitrogen protection for 50 min. Use a low-temperature airflow pulverizer to break up the fiber bundle at 30°C and 0.6 MPa to obtain cross-linked fiber.

[0132] A3. Add 100 parts of cross-linked fiber to 600 parts of deionized water, add 10 parts of nano-montmorillonite and 3 parts of fatty alcohol polyoxyethylene ether, ultrasonically disperse at 400 W for 50 min, place in a vacuum jar, evacuate to ≤10 Pa, soak for 20 min, pressurize at 0.3 MPa for 30 min, and cure under nitrogen protection at 140℃ for 40 min to obtain modified composite fiber.

[0133] Comparative Example 1: No modified composite fiber was added; otherwise, it was the same as Example 5.

[0134] Comparative Example 2: The modified composite fiber was replaced with a mixed fiber prepared by mixing equal masses of lignin fiber and modified polypropylene fiber, and the rest was the same as in Example 5.

[0135] Comparative Example 3: No filler was added, and the rest was the same as in Example 5.

[0136] Performance testing:

[0137] Table 2 Test Items and Methods

[0138] Testing items Test methods Sample size Test conditions density Water weight method φ101.6×63.5 mm Marshall specimen 25℃ Porosity Marshall test φ101.6×63.5 mm Calculation method Permeability coefficient Constant head permeability test φ100×150 mm Water pressure 0.3 MPa Splitting strength Marshall splitting test φ101.6×63.5 mm 15℃, loading rate 50 mm / min Freezing temperature TSRST 40×40×160 mm Cooling rate -10℃ / h Slope flow value Slope flow test φ101.6×63.5 mm 60℃ constant temperature for 48 hours, slope 1:1

[0139] Table 3 Test Results of Examples

[0140] Group <![CDATA[Density g / cm 3 > Porosity % Permeability coefficient cm / s Splitting strength MPa Freezing temperature (°C) Slope flow value (mm) Example 1A1B1C1 2.32 2.1 <![CDATA[5.6×10 -9 ]]> 1.82 -40 0.9 Example 2A2B2C1 2.35 1.6 <![CDATA[4.2×10 -9 ]]> 2.05 -42 1.1 Example 3A3B3C1 2.31 1.8 <![CDATA[4.8×10 -9 ]]> 1.98 -41 1.4 Example 4A3B1C2 2.38 1.3 <![CDATA[3.1×10 -9 ]]> 2.32 -44 1.2 Example 5A1B2C2 2.33 1.9 <![CDATA[5.2×10 -9 ]]> 1.91 -41 0.8 Example 6A2B3C2 2.36 1.5 <![CDATA[3.8×10 -9 ]]> 2.18 -43 1.0 Example 7A2B1C3 2.39 1.4 <![CDATA[3.5×10 -9 ]]> 2.35 -42 1.3 Example 8A3B2C3 2.41 1.2 <![CDATA[2.8×10 -9 ]]> 2.48 -45 1.5 Example 9A1B3C3 2.36 1.7 <![CDATA[4.6×10 -9 ]]> 2.10 -40 0.9

[0141] Table 4 Comparative test results

[0142] Group <![CDATA[Density g / cm 3 > Porosity % Permeability coefficient cm / s Splitting strength MPa Freezing temperature (°C) Slope flow value (mm) Comparative Example 1 2.28 2.6 <![CDATA[1.1×10 -7 ]]> 1.48 -34 1.0 Comparative Example 2 2.31 2.2 <![CDATA[8.5×10 -9 ]]> 1.72 -37 0.9 Comparative Example 3 2.18 4.5 <![CDATA[5.2×10 -6 ]]> 1.52 -32 2.6

[0143] Results analysis:

[0144] 1. Range analysis:

[0145] Table 5. Range Analysis of Freezing Temperature (°C)

[0146] level A oil-stone ratio Grade B matching index C filler content K1 -40.33 -42.00 -41.00 K2 -42.33 -42.67 -42.67 K3 -43.33 -41.33 -42.33 Range R 3.00 1.34 1.67

[0147] The optimal combination is A3B2C2.

[0148] Table 6 Porosity (%) Range Analysis

[0149] level A oil-stone ratio Grade B matching index C filler content K1 1.90 1.60 1.83 K2 1.50 1.57 1.57 K3 1.43 1.67 1.43 Range R 0.47 0.10 0.40

[0150] The optimal combination is A3B2C3.

[0151] Table 7. Range Analysis of Splitting Strength (MPa)

[0152] level A oil-stone ratio Grade B matching index C filler content K1 1.94 2.16 1.95 K2 2.19 2.15 2.14 K3 2.26 2.09 2.31 Range R 0.32 0.07 0.36

[0153] The optimal combination is A3B1C3.

[0154] Table 8 Permeability Coefficient (10) -9 range analysis (cm / s)

[0155] level A oil-stone ratio Grade B matching index C filler content K1 5.13 4.07 4.87 K2 3.83 4.07 4.03 K3 3.57 4.40 3.63 Range R 1.56 0.33 1.24

[0156] The optimal combination is A3B1 / B2C3.

[0157] 2. Analysis of variance

[0158] Substituting the freezing point temperature data into the analysis of variance, the total sum of squared deviations is:

[0159]

[0160] Table 9. Results of Analysis of Variance

[0161] Source of variance Sum of squares SS Degrees of freedom df Mean Square MS F value Significance A oil ratio 14.00 2 7.00 21.0 ** Grade B matching index 2.67 2 1.33 4.0 - C filler content 4.67 2 2.33 7.0 * error 0.67 2 0.33 - - total 22.00 8 - - -

[0162] F 0.05 (2,2)=19.0, F 0.10 (2,2)=9.0. The oil-aggregate ratio has a significant impact, the filler content has a certain impact, and the gradation index has no significant impact. The results are consistent with the range analysis.

[0163] Considering various performance indicators and taking into account the design requirements for frost-break temperature, porosity, splitting tensile strength, and slope flow value, the optimal mix proportion was determined to be Example 8, with the following parameters: asphalt-aggregate ratio: 8.5%, gradation index: 0.38, filler content: 14%, coarse aggregate: 50 parts, fine aggregate: 40 parts, asphalt: 8.5 parts, modified composite fiber: 0.3 parts, and functional additives: 0.3 parts. This mix proportion has a frost-break temperature of -45℃, a porosity of 1.2%, a splitting tensile strength of 2.48 MPa, and a permeability coefficient of 2.8 × 10⁻⁶. -9 The flow rate is cm / s and the slope flow value is 1.5 mm, which fully meets the design requirements of high-altitude and high-intensity zones.

[0164] Comparative Example 1, without the addition of modified composite fibers, had a freeze-break temperature of only -34℃, failing to meet the design requirement of ≤-38℃; however, its permeability coefficient increased to 1.1×10⁻⁶. -7 The splitting strength decreased by 22.5% (cm / s), indicating that the modified composite fiber significantly improved the low-temperature crack resistance and impermeability of asphalt concrete through synergistic toughening and chemical cross-linking.

[0165] Comparative Example 2 used an equal mass of simple mixed fibers to replace the modified composite fibers. The freeze-break temperature was -37℃, and the porosity increased to 2.2%; the permeability increased to 8.5×10⁻⁶. -9 The splitting strength was 9.9% lower than that of Example 5, indicating that the chemical crosslinking and nano-montmorillonite composite process has a significant effect on achieving excellent low-temperature crack resistance.

[0166] Comparative Example 3, without any filler, achieved a freeze-thaw temperature of -32℃, a porosity of 4.5%, and a permeability coefficient that soared to 5.2×10⁻⁶. -6 The values ​​of cm / s, splitting strength of 1.52 MPa, and slope flow value of 2.6 mm indicate that the filler plays a significant role in the seepage prevention performance of hydraulic asphalt concrete in high-altitude and cold regions.

[0167] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A type of hydraulic asphalt concrete suitable for high-altitude and high-intensity seismic zones, characterized in that, Including the following parts by weight of raw materials: 40-55 parts coarse aggregate, 30-48 parts fine aggregate, 10-15 parts filler, 6.5-8.5 parts asphalt, 0.1-0.5 parts modified composite fiber, and 0.1-0.5 parts functional additives; The modified composite fiber is prepared by cross-linking pretreated lignin fiber and modified polypropylene fiber with 2,2'-bis(2-oxazoline), and then modifying it with nano-montmorillonite and fatty alcohol polyoxyethylene ether.

2. The hydraulic asphalt concrete suitable for high-altitude and high-intensity frigid zones according to claim 1, characterized in that, The coarse aggregate is basalt with a particle size of 5~20 mm, a crushing value of ≤26%, and a water absorption rate of ≤2.0%.

3. The hydraulic asphalt concrete suitable for high-altitude and high-intensity frigid zones according to claim 1, characterized in that, The fine aggregate is manufactured sand; the fineness modulus of the manufactured sand is 2.6~3.0 and the mud content is ≤1.0%.

4. The hydraulic asphalt concrete suitable for high-altitude and high-intensity frigid zones according to claim 1, characterized in that, The filler is limestone powder with a particle size ≤0.075 mm, a hydrophilicity coefficient <1.0, and a specific surface area ≥300 m² / kg.

5. The hydraulic asphalt concrete suitable for high-altitude and high-intensity frigid zones according to claim 1, characterized in that, The functional additives include a waterproofing agent and an anti-peeling agent; the waterproofing agent is an organosilicon-based waterproofing agent, and the dosage is 40-60% of the total mass of the functional additives; the anti-peeling agent is an amine-based anti-peeling agent, and the dosage is 40-60% of the total mass of the functional additives.

6. The hydraulic asphalt concrete suitable for high-altitude and high-intensity frigid zones according to claim 1, characterized in that, The method for preparing the modified composite fiber includes the following steps: A1. Immerse 100-120 parts of lignin fiber in 300-500 parts of 3-5% methyltriethoxysilane solution, stir at 60-70℃ for 30-60 min, and cure with nitrogen at 100-120℃ for 40-50 min to obtain pretreated lignin fiber; wash 60-80 parts of polypropylene fiber with 300-500 parts of ethanol-deionized water (volume ratio 1:3) for 20-30 min, immerse in 200-400 parts of 5-8% maleic anhydride acetone solution, soak at 50-60℃ for 30-60 min, and vacuum dry at 70-80℃ for 4-6 h to obtain modified polypropylene fiber; A2. Mix 80-100 parts of pretreated lignin fiber and 40-60 parts of modified polypropylene fiber and immerse them in 300-500 parts of 5-8% (w / w) 2,2'-bis(2-oxazoline)acetone solution. Add 0.5-1.2 parts of sodium methoxide and stir at 100-120℃ for 1-2 h under nitrogen protection. Remove the fiber and cure it at 120-130℃ under nitrogen protection for 40-50 min. Use a low-temperature airflow pulverizer to break up the fiber bundle at 30-40℃ and airflow pressure of 0.6-0.8 MPa to obtain cross-linked fiber. A3. Add 100-150 parts of cross-linked fiber to 400-600 parts of deionized water, add 5-20 parts of nano-montmorillonite and 1-5 parts of fatty alcohol polyoxyethylene ether, ultrasonically disperse at 300-500 W for 40-50 min, place in a vacuum tank, evacuate to ≤10 Pa, soak for 10-20 min, pressurize at 0.25-0.3 MPa for 30-60 min, and cure under nitrogen protection at 130-140℃ for 40-50 min to obtain modified composite fiber.

7. A method for preparing hydraulic asphalt concrete suitable for high-altitude and high-intensity frigid zones according to any one of claims 1 to 6, characterized in that, Includes the following steps: S1. Place the coarse aggregate, fine aggregate, and filler into the mixing equipment and dry mix for 2-3 minutes. S2. Slowly add the asphalt heated to 155~170℃ to the dry material in step S1, and mix at a constant temperature of 140~160℃ for 3~4 minutes. S3. The modified composite fiber is evenly sprinkled into the mixing system of step S2 in two batches. After each addition, the mixture is mixed for 1 to 2 minutes. Then, the functional additives are added and the mixture is mixed for another 1 to 2 minutes to obtain the mixture. S4. After mixing, immediately discharge the mixture, controlling the discharge temperature to 140~160℃, and compact it using a rolling mill until the compaction degree is ≥96%; S5. After molding, allow it to cure naturally for 24-48 hours. During the curing period, avoid rainwater erosion and external impact. Once curing is complete, it can be put into subsequent construction or use.

8. A method for mix design of hydraulic asphalt concrete suitable for high-altitude and high-intensity frigid zones, characterized in that, Includes the following steps: a. Calibrate the properties of the raw materials described in claims 1 to 6 according to the SL / T 501-2025 standard, and determine the discontinuous gradation range of coarse aggregate and fine aggregate; b. Using L9(3) 3 An orthogonal array was used to optimize the baseline mix proportion using factors such as the oil-aggregate ratio, gradation index, and filler content. c. Adjust the amount of asphalt and the amount of modified composite fiber to enhance the seismic deformation resistance of hydraulic asphalt concrete and adapt it to the needs of use in high-altitude and high-intensity seismic zones. d. Verify the suitability of the mix proportion through on-site paving tests, and revise and determine the final construction mix proportion in conjunction with the construction parameters of the preparation method described in claim 7.

9. The method for mix design of hydraulic asphalt concrete suitable for high-altitude and high-intensity frigid zones according to claim 8, characterized in that, The factor levels for the orthogonal experiment described in step b are set as follows: oil-aggregate ratio 6.5%, 7.5%, 8.5%; gradation index 0.35, 0.38, 0.41; filler content 10%, 12%, 14%.