A water-activated precast mortar pad and its preparation method

By combining cementitious materials, lightweight aggregates, and water-soluble binders with a hot-pressing process to prepare water-activated precast mortar mats, the problem of precast dry mortar panels being unable to be activated by water in existing technologies has been solved. This results in lightweight, high-strength water-activated precast mortar mats that do not reduce mechanical properties and are suitable for prefabricated thin-layer masonry.

CN123106077APending Publication Date: 2026-11-17CHINA CONSTR EIGHT ENG DIV CORP LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611213141.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-11
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing precast dry mortar slabs cannot be activated by water. Conventional water-soluble binders will participate in the cement hydration reaction, reducing the long-term mechanical strength of the mortar. Furthermore, the dry-formed products made from them lack toughness and are prone to powdering and cracking during transportation and stacking, making it difficult to meet the needs of prefabricated thin-layer masonry.

Method used

Water-activated precast mortar pads are prepared by using cementitious materials, lightweight closed-cell and open-cell aggregates, water absorbents and water-soluble binders through a hot-pressing process. The water-soluble binder dissolves rapidly upon contact with water, only delaying cement hydration without reducing the long-term mechanical properties of the mortar. Combined with a sheet-like grid support matrix, integrated molding is achieved.

Benefits of technology

Water-activated precast mortar pads are rapidly activated upon contact with water, maintaining long-term mechanical properties. They are lightweight, high-strength, easy to produce, suitable for large-scale application, reduce dust pollution, and are compatible with prefabricated thin-layer masonry projects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106077A_ABST
    Figure CN123106077A_ABST
Patent Text Reader

Abstract

This invention provides a water-activated precast mortar pad, comprising a sheet-like mesh support matrix and the following raw materials in parts by weight: 70-80 parts of cementitious material, 10-20 parts of lightweight closed-cell aggregate, 2-6 parts of lightweight open-cell aggregate, 0.2-1 parts of water-absorbing agent, and 5-15 parts of water-soluble binder. The water-soluble binder has a melting point below 200°C and completely melts and dissolves within 180 seconds after being wetted by water. The water-activated precast mortar pad is prepared by the following method: the above raw materials are mixed evenly to obtain a dry-mix premix; half of the dry-mix premix is ​​laid flat in a molding mold and leveled, then the sheet-like mesh support matrix is ​​laid flat, and then the remaining dry-mix premix is ​​laid flat and leveled; hot-pressed molding is performed, and the mixture is naturally cooled to room temperature. After the water-soluble binder has completely solidified, the pad is demolded. Related preparation methods are also provided. The water-activated precast mortar pad of this invention has water-activated properties, does not damage the long-term mechanical properties of the mortar, is lightweight and high-strength, is easy to produce, and has low production costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the technical field of precast mortar products and prefabricated masonry materials, and particularly to the technical field of water-activated precast mortar pads, specifically a water-activated precast mortar pad and its preparation method. Background Technology

[0002] Building construction refers to the production activities during the implementation phase of an engineering project. It is the process of building various types of structures, or the process of turning the lines on design drawings into a physical object at a designated location. It includes foundation construction, main structure construction, roofing construction, and decoration construction.

[0003] Traditional masonry construction involves mixing mortar with water on-site, which generates a lot of dust and wastewater. The mixed mortar also has problems such as short initial setting time and inability to be stored for a long time. High-precision prefabricated blocks require thin mortar joints, and the thickness control of manually mixed mortar is poor. Construction is extremely difficult in restricted conditions such as near water or in confined spaces.

[0004] Most existing precast dry mortar panels on the market use insoluble organic adhesives, which cannot be activated by water after molding. They can only be used as decorative panels and cannot replace masonry mortar. Conventional water-soluble binders have two major drawbacks: first, some binders participate in the cement hydration reaction, significantly reducing the long-term mechanical strength of the mortar; second, dry-formed products made from them lack toughness and are prone to powdering and cracking during transportation and storage. At the same time, the existing system lacks a matching water-absorbing and toughening system suitable for aggregates, and there is no complete process for integrated low-temperature hot pressing molding with fiber mesh interlayer, making it difficult to meet the usage requirements of prefabricated thin-layer masonry.

[0005] Therefore, it is desirable to provide a water-activated precast mortar pad that has water-activated properties, does not damage the long-term mechanical properties of the mortar, is lightweight and high-strength, is easy to produce, and has low production costs. Summary of the Invention

[0006] In order to overcome the shortcomings of the prior art, one object of the present invention is to provide a water-activated precast mortar pad, which has water-activated properties, does not damage the long-term mechanical properties of mortar, is lightweight and high-strength, is easy to produce, has low production cost, and is suitable for large-scale promotion and application.

[0007] Another objective of this invention is to provide a method for preparing water-activated precast mortar pads, which is ingeniously designed, easy to prepare, and low in cost. The water-activated precast mortar pads produced have water-activated properties and do not damage the long-term mechanical properties of the mortar, making them suitable for large-scale application.

[0008] To achieve the above objectives, in a first aspect of the present invention, a water-activated precast mortar pad is provided, comprising the following raw materials in parts by weight: 70-80 parts of cementitious material, characterized in that the water-activated precast mortar pad further comprises a sheet-like mesh support matrix and the following raw materials in parts by weight: 10-20 parts of lightweight closed-cell aggregate, 2-6 parts of lightweight open-cell aggregate, 0.2-1 part of water absorbent, and 5-15 parts of water-soluble binder, wherein the water-soluble binder has a melting point below 200°C and completely melts and dissolves within 180 seconds after being wetted by water, and the water-activated precast mortar pad is prepared by the following method:

[0009] The cementitious material, the lightweight closed-cell aggregate, the lightweight open-cell aggregate, the water absorbent and the water-soluble binder are mixed evenly to obtain a dry-mix premix.

[0010] Half the mass of the dry premix material is laid flat in the molding mold and leveled. Then, the sheet mesh support base is laid flat on the half mass of the dry premix material. The remaining dry premix material is then laid flat on the sheet mesh support base and scraped flat.

[0011] The material is hot-pressed using a hot-pressing process. After hot pressing, it is naturally cooled to room temperature, and then demolded after the water-soluble adhesive has completely solidified.

[0012] Preferably, the cementitious material is cement.

[0013] Preferably, the lightweight closed-cell aggregate is expanded glass.

[0014] Preferably, the lightweight open-cell aggregate is expanded perlite.

[0015] Preferably, the absorbent is selected from at least one of 0.5 mm short wood fibers, 2 mm lignocellulose and 0.3 mm polypropylene short fibers.

[0016] Preferably, the water-soluble binder is selected from at least one of sorbitol, urea, magnesium acetate, and polyethylene glycol.

[0017] Preferably, the sheet-like mesh support substrate is a glass fiber mesh cloth, and the mesh aperture of the glass fiber mesh cloth is 4mm~6mm.

[0018] Preferably, the thickness of the water-activated precast mortar pad is 2mm to 10mm.

[0019] In a second aspect of the present invention, a method for preparing the above-mentioned water-activated precast mortar pad is provided, characterized by comprising the following steps:

[0020] S1: Mix the cementitious material, the lightweight closed-cell aggregate, the lightweight open-cell aggregate, the water absorbent and the water-soluble binder evenly to obtain a dry-mix premix;

[0021] S2: Spread half the mass of the dry premix into the molding die and level it. Then spread the sheet mesh support base on the half mass of the dry premix and spread the remaining dry premix on the sheet mesh support base and scrape it flat.

[0022] S3: Hot-pressed molding using a hot-pressing process;

[0023] S4: After hot pressing, allow the material to cool naturally to room temperature. Once the water-soluble binder has completely solidified, demold the material to obtain the water-activated precast mortar pad.

[0024] Preferably, in step S3, the temperature of the hot pressing process is 80℃~140℃, the pressure of the hot pressing process is 1.5MPa~2.0MPa, and the time of the hot pressing process is 10min~15min.

[0025] The main beneficial effects of this invention are:

[0026] 1. The water-activated precast mortar pad of the present invention comprises a sheet-like mesh support matrix and the following raw materials in parts by weight: 70-80 parts of cementitious material, 10-20 parts of lightweight closed-cell aggregate, 2-6 parts of lightweight open-cell aggregate, 0.2-1 part of water-absorbing agent, and 5-15 parts of water-soluble binder. The water-soluble binder has a melting point below 200°C and completely melts and dissolves within 180 seconds after being wetted by water. The water-activated precast mortar pad is prepared by the following method: mixing cementitious material, lightweight closed-cell aggregate, lightweight open-cell aggregate, water-absorbing agent, and water-soluble binder... The binder is mixed evenly to obtain a dry premix. Half the mass of the dry premix is ​​spread and leveled in the molding mold. Then, a sheet-like grid support substrate is spread on the half mass of the dry premix. The remaining dry premix is ​​spread on the sheet-like grid support substrate and leveled. The mold is formed by hot pressing. After hot pressing, it is naturally cooled to room temperature. After the water-soluble binder has completely solidified, it is demolded. Therefore, it has water-activated properties, does not damage the long-term mechanical properties of mortar, is lightweight and high-strength, is easy to produce, has low production cost, and is suitable for large-scale promotion and application.

[0027] 2. The preparation method of the water-activated precast mortar pad of the present invention includes the following steps: S1: Mixing cementitious materials, lightweight closed-cell aggregates, lightweight open-cell aggregates, water absorbents and water-soluble binders evenly to obtain dry-mix premix; S2: Spreading half the mass of the dry-mix premix into the molding mold and leveling it, then spreading a sheet-like grid support substrate on the half mass of the dry-mix premix, and then spreading the remaining dry-mix premix on the sheet-like grid support substrate and scraping it level; S3: Hot-pressing molding using a hot-pressing process; S4: After hot pressing, naturally cooling to room temperature, and demolding after the water-soluble binder has completely solidified to obtain the water-activated precast mortar pad. Therefore, its design is ingenious, its preparation is simple, and its preparation cost is low. The produced water-activated precast mortar pad has water-activated properties and does not damage the long-term mechanical properties of the mortar, making it suitable for large-scale promotion and application.

[0028] These and other objects, features and advantages of the present invention will be fully realized by the following detailed description and claims, and may be achieved by the means, methods and combinations thereof specifically pointed out in the appended claims. Attached Figure Description

[0029] Figure 1 This is a schematic flowchart of the preparation method of the water-activated precast mortar pad of the present invention. Detailed Implementation

[0030] To address the issues of existing precast dry mortar panels failing to activate upon contact with water, and the fact that conventional water-soluble binders partially participate in the cement hydration reaction, significantly reducing the long-term mechanical strength of the mortar, and resulting in dry-formed products with insufficient toughness, prone to powdering and cracking during transport and storage, the inventors, through extensive research, discovered that using a cementitious material as the matrix, compounding it with two types of lightweight aggregates—lightweight closed-cell aggregates and lightweight open-cell aggregates—reduces its weight. A water-absorbing agent is added to achieve water retention and toughening, supplemented by hot-pressing with a water-soluble binder. The water-soluble binder melts upon heating, bonding the central sheet-like mesh support matrix and the mortar on both sides. Upon contact with water, it dissolves rapidly, only delaying early cement hydration without reducing the later strength of the mortar. Water-activated precast mortar pads soften quickly when exposed to water, restoring the mortar's workability. This invention is suitable for applications in dry powder mortar masonry scenarios.

[0031] This invention first provides a water-activated precast mortar pad, comprising a sheet-like mesh support matrix and the following raw materials in parts by weight: 70-80 parts of cementitious material, 10-20 parts of lightweight closed-cell aggregate, 2-6 parts of lightweight open-cell aggregate, 0.2-1 part of water-absorbing agent, and 5-15 parts of water-soluble binder. The water-soluble binder has a melting point below 200°C and completely dissolves within 180 seconds after being wetted by water. The water-activated precast mortar pad is prepared by the following method:

[0032] The cementitious material, the lightweight closed-cell aggregate, the lightweight open-cell aggregate, the water absorbent and the water-soluble binder are mixed evenly to obtain a dry-mix premix.

[0033] Half the mass of the dry premix material is laid flat in the molding mold and leveled. Then, the sheet mesh support base is laid flat on the half mass of the dry premix material. The remaining dry premix material is then laid flat on the sheet mesh support base and scraped flat.

[0034] The material is hot-pressed using a hot-pressing process. After hot pressing, it is naturally cooled to room temperature, and then demolded after the water-soluble adhesive has completely solidified.

[0035] The cementing material can be any suitable cementing material, preferably cement.

[0036] The lightweight closed-cell aggregate can be any suitable lightweight closed-cell aggregate, preferably expanded glass.

[0037] The lightweight open-cell aggregate can be any suitable lightweight open-cell aggregate, preferably expanded perlite.

[0038] The absorbent can be any suitable absorbent, preferably selected from at least one of 0.5 mm short wood fibers, 2 mm lignocellulose and 0.3 mm polypropylene short fibers.

[0039] The water-soluble binder can be any suitable water-soluble binder, preferably selected from at least one of sorbitol, urea, magnesium acetate, and polyethylene glycol. The water-soluble binder has a melting point below 200°C, completely dissolves within 180 seconds after being wetted by water, and only delays cement hydration without participating in the cement hydration reaction, thus not reducing the compressive strength or bond strength of the mortar in the later stages of curing.

[0040] The sheet-like mesh support substrate can be any suitable sheet-like mesh support substrate. Preferably, the sheet-like mesh support substrate is a glass fiber mesh cloth with a mesh aperture of 4mm to 6mm. The sheet-like mesh support substrate is laid in the middle of the dry-mix premix, and a hot-pressed molten water-soluble binder penetrates through the mesh pores, combining the dry-mix premix and the sheet-like mesh support substrate into a whole.

[0041] The thickness of the water-activated precast mortar pad can be determined as needed. Preferably, the thickness of the water-activated precast mortar pad is 2mm to 10mm. After being fully soaked in water, the water-activated precast mortar pad softens completely within 3 minutes, restoring the normal mixing and construction performance of the mortar, and can be directly used in various masonry scenarios.

[0042] The present invention also provides a method for preparing the above-mentioned water-activated precast mortar pad, comprising the following steps:

[0043] S1: Mix the cementitious material, the lightweight closed-cell aggregate, the lightweight open-cell aggregate, the water absorbent and the water-soluble binder evenly to obtain a dry-mix premix;

[0044] S2: Spread half the mass of the dry premix into the molding die and level it. Then spread the sheet mesh support base on the half mass of the dry premix and spread the remaining dry premix on the sheet mesh support base and scrape it flat.

[0045] S3: Hot-pressed molding using a hot-pressing process;

[0046] The water-soluble binder is heated and melted to form a continuous bonding phase, thereby achieving integrated composite of dry-mix premix and sheet-like mesh support matrix;

[0047] S4: After hot pressing, allow the material to cool naturally to room temperature. Once the water-soluble binder has completely solidified, demold the material to obtain the water-activated precast mortar pad.

[0048] In step S3, the temperature, pressure, and time of the hot pressing process can be determined as needed. Preferably, in step S3, the temperature of the hot pressing process is 80℃~140℃, the pressure of the hot pressing process is 1.5MPa~2.0MPa, and the time of the hot pressing process is 10min~15min.

[0049] To better understand the technical content of this invention, the following embodiments are provided for detailed explanation.

[0050] Example 1

[0051] The raw materials for water-activated precast mortar pads, by weight, are: 70 parts cement, 10 parts expanded glass, 2 parts expanded perlite, 0.2 parts 0.5mm short wood fiber, and 5 parts sorbitol;

[0052] The sheet-like mesh support substrate is a glass fiber mesh with a 4mm aperture.

[0053] Preparation method of water-activated precast mortar pad:

[0054] S1: Add all raw materials to the mixing equipment according to the proportion and mix evenly to obtain dry premix;

[0055] S2: Spread half the mass of dry premix material into the molding mold and level it, spread sheet mesh to support the substrate, then spread the remaining dry premix material and scrape it level.

[0056] S3: Hot pressing process is used for hot pressing molding. The hot pressing temperature is 80℃, the pressure is 2.0MPa, and the heat and pressure are maintained for 12 minutes. Sorbitol melts to form a continuous binder phase. The dry-mixed premix is ​​combined with the glass fiber mesh cloth.

[0057] S4: Allow to cool naturally to room temperature. Once the water-soluble binder has completely solidified, demold to obtain a 2mm dry water-activated precast mortar pad.

[0058] Example 2

[0059] The raw materials for water-activated precast mortar pads, by weight, are: 75 parts cement, 15 parts expanded glass, 4 parts expanded perlite, 0.6 parts 2mm wood cellulose, and 10 parts sorbitol.

[0060] The sheet-like mesh support substrate is a glass fiber mesh with a 5mm aperture.

[0061] Preparation method of water-activated precast mortar pad:

[0062] S1: Add all raw materials to the mixing equipment according to the proportion and mix evenly to obtain dry premix;

[0063] S2: Spread half the mass of dry premix material into the molding mold and level it, spread sheet mesh to support the substrate, then spread the remaining dry premix material and scrape it level.

[0064] S3: Hot pressing process is used for hot pressing molding. The hot pressing temperature is 120℃ and the pressure is 1.5MPa. The heat and pressure are maintained for 15 minutes. Sorbitol melts to form a continuous binder phase. The dry-mixed premix is ​​combined with the glass fiber mesh cloth.

[0065] S4: Allow to cool naturally to room temperature. Once the water-soluble binder has completely solidified, demold to obtain a 3mm dry water-activated precast mortar pad.

[0066] Example 3

[0067] The raw materials for water-activated precast mortar pads, by weight, are: 80 parts cement, 20 parts expanded glass, 6 parts expanded perlite, 1 part 0.3mm polypropylene short fiber, and 15 parts polyethylene glycol.

[0068] The sheet-like mesh support substrate is a glass fiber mesh with a 6mm aperture.

[0069] Preparation method of water-activated precast mortar pad:

[0070] S1: Add all raw materials to the mixing equipment according to the proportion and mix evenly to obtain dry premix;

[0071] S2: Spread half the mass of dry premix material into the molding mold and level it, spread sheet mesh to support the substrate, then spread the remaining dry premix material and scrape it level.

[0072] S3: Hot pressing process is used for hot pressing molding. The hot pressing temperature is 140℃ and the pressure is 1.5MPa. The heat and pressure are maintained for 10 minutes. Polyethylene glycol melts to form a continuous bonding phase. The dry-mixed premix is ​​combined with the glass fiber mesh.

[0073] S4: Allow to cool naturally to room temperature. Once the water-soluble binder has completely solidified, demold to obtain a 5mm dry water-activated precast mortar pad.

[0074] Example 4

[0075] The raw materials for water-activated precast mortar pads, by weight, are: 73 parts cement, 13 parts expanded glass, 3 parts expanded perlite, 0.4 parts 0.5mm short wood fibers, and 8 parts water-soluble binder of urea and magnesium acetate (urea: magnesium acetate = 3:2).

[0076] The sheet-like mesh support substrate is a glass fiber mesh with a 5mm aperture.

[0077] Preparation method of water-activated precast mortar pad:

[0078] S1: Add all raw materials to the mixing equipment according to the proportion and mix evenly to obtain dry premix;

[0079] S2: Spread half the mass of dry premix material into the molding mold and level it, spread sheet mesh to support the substrate, then spread the remaining dry premix material and scrape it level.

[0080] S3: Hot pressing process is adopted for hot pressing molding. The hot pressing temperature is 110℃, the pressure is 1.8MPa, and the heat and pressure are maintained for 14 minutes. Water-soluble binder is compounded to form a continuous bonding phase. The dry-mixed premix is ​​combined with glass fiber mesh cloth.

[0081] S4: Allow to cool naturally to room temperature, and demold after the compounded water-soluble binder has completely solidified to obtain a 10mm dry water-activated precast mortar pad.

[0082] Example 5

[0083] The raw materials for water-activated precast mortar pads, by weight, are: 78 parts cement, 18 parts expanded glass, 5 parts expanded perlite, 0.8 parts 0.3mm polypropylene short fibers, and 12 parts water-soluble binder of sorbitol and polyethylene glycol (sorbitol: polyethylene glycol = 2:1).

[0084] The sheet-like mesh support substrate is a glass fiber mesh with a 6mm aperture.

[0085] Preparation method of water-activated precast mortar pad:

[0086] S1: Add all raw materials to the mixing equipment according to the proportion and mix evenly to obtain dry premix;

[0087] S2: Spread half the mass of dry premix material into the molding mold and level it, spread sheet mesh to support the substrate, then spread the remaining dry premix material and scrape it level.

[0088] S3: Hot pressing process is adopted for hot pressing molding. The hot pressing temperature is 130℃, the pressure is 2.0MPa, and the heat and pressure are maintained for 13 minutes. The compound water-soluble binder is melted to form a continuous bonding phase. The dry-mixed premix is ​​combined with the glass fiber mesh cloth.

[0089] S4: Allow to cool naturally to room temperature, and demold after the compounded water-soluble binder has completely solidified to obtain a 6mm dry water-activated precast mortar pad.

[0090] Comparative Example 1

[0091] The binder consists of 10 parts maltitol, and the remaining raw materials, proportions, and molding process are consistent with those in Example 2.

[0092] Although maltitol can be hot-pressed and melted, its molecular chains are longer and its crystals are denser. The binder phase formed after melting and cooling has poor toughness, resulting in low dry flexural strength of the mortar pad and easy powdering during transportation and stacking. Due to its own solubility and dense crystalline layer, the binder takes up to 240 seconds to completely dissolve after being wetted with water. The mortar pad is activated slowly and will interfere with the normal hydration reaction of cement, resulting in a significant decrease in strength.

[0093] Comparative Example 2

[0094] The binder used was 15 parts mannitol, and the remaining raw materials, proportions, and molding process were consistent with those in Example 2.

[0095] Mannitol can be hot-pressed, but the material has poor water solubility and hard and brittle crystal phase after curing. The dry flexural strength of the mortar pad is insufficient and it is prone to cracking. Water has difficulty penetrating the dense mannitol crystal layer, and the time for the binder to completely dissolve is as high as 275 seconds. The on-site activation efficiency is poor, and it also inhibits cement hydration and reduces the mechanical properties of the mortar.

[0096] Comparative Example 3

[0097] No water-absorbing agent was added, and all other raw materials, proportions, and molding processes remained the same as in Example 2.

[0098] Without a three-dimensional toughened water-retaining network constructed with absorbent fibers, the strength of the mortar pad is reduced, the dry blank is brittle, and it is very easy to fall off and crack during stacking and transportation; the uniformity of water diffusion during watering activation is poor, and local water shortage areas are prone to appear. After the masonry is formed, the mortar joints are prone to dry shrinkage cracks, and the mechanical properties are significantly reduced in the end.

[0099] Comparative Example 4

[0100] The sheet-like mesh support substrate is not set, and all other raw materials, proportions, and molding processes are consistent with those in Example 2.

[0101] The lack of a sheet-like mesh supporting the matrix results in weak interlayer bonding after hot pressing, reduced dry flexural strength, and easy delamination and fracture under bending stress; the uniformity of the forming thickness is difficult to guarantee, and the long-term mechanical stability of the hardened body is insufficient.

[0102] Performance Test Examples

[0103] The relevant performance of the above embodiments and comparative examples was tested according to the following test methods:

[0104] According to JGJ / T 70-2009 "Standard for Test Methods of Basic Performance of Building Mortar", the various properties of water-activated precast mortar pads were determined. The activation and dissolution time was observed visually. When the sample has no hard, dry core layer and can be uniformly plastically deformed by light finger pressure, the mortar pad is considered to be fully activated. The test results are summarized in Table 1 below.

[0105] Table 1 Test results of main performance indicators of water-activated precast mortar pads

[0106] According to the data in Table 1, the water-activated precast mortar pads prepared in Examples 1-5 of the present invention have good performance. Example 2 has the best performance and excellent toughness, and there is no phenomenon of slag falling or damage during transportation and stacking.

[0107] As shown in Table 1, the dry flexural strength of each embodiment can reach 0.70~0.95MPa, with excellent dry toughness, and is not prone to slagging or cracking during stacking and transportation. Comparative Examples 1-4 have lower dry flexural strength, greater brittleness in the dry blanks, and a higher risk of breakage during storage and transportation. Regarding activation performance, the binder dissolution time in the embodiments of this invention is controlled within 130~172s, resulting in uniform activation without localized shrinkage cracks. The maltitol binder in Comparative Example 1 dissolves in 240s, and the mannitol binder in Comparative Example 2 dissolves in 275s, both significantly exceeding the activation time limit, leading to low activation efficiency during on-site construction. In terms of long-term mechanical properties, the 3-day and 28-day bonding and compressive strengths of all embodiments are significantly better than the four comparative examples, proving that the synergistic effect of the compounded water-soluble binder, water absorbent, and sheet-like mesh support matrix of this invention achieves rapid activation upon contact with water without interfering with the later hydration of cement, resulting in stable long-term mechanical properties of the mortar. Example 2 exhibits the best overall performance and is the preferred formulation of this invention.

[0108] Therefore, in response to the problems that existing precast dry mortar panels cannot be activated by water, and that conventional water-soluble binders partially participate in the cement hydration reaction, significantly reducing the long-term mechanical strength of the mortar, and that dry-formed products made from it have insufficient toughness and are prone to powdering and cracking during transportation and stacking, this invention discloses a water-activated precast mortar pad, which, by weight, includes 70-80 parts of cementitious material, 10-20 parts of lightweight closed-cell aggregate, 2-6 parts of lightweight open-cell aggregate, 0.2-1 part of water absorbent, and 5-15 parts of water-soluble binder; the water-soluble binder is selected from one or more of sorbitol, urea, magnesium acetate, and polyethylene glycol, with a melting point below 200℃, and after hot pressing and melting, it binds the mortar particles to the sheet-like mesh support matrix sandwiched in the middle, and uses a low-temperature hot pressing process of 80-140℃ to integrally form a dry mortar pad with a thickness of 2-10mm. This water-soluble binder dissolves rapidly within 180 seconds of contact with water, only delaying the early hydration of cement without participating in the hydration reaction, and will not weaken the later mechanical strength of the mortar; the dry mortar pad has good dry toughness and is not easy to fall off, and it completely softens and restores the mortar's workability within 3 minutes of immersion in water, with no dust pollution during on-site construction, suitable for prefabricated thin-layer masonry projects, and the production process is simple and can be mass-produced with conventional equipment.

[0109] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0110] 1. The use of expanded glass and expanded perlite composite lightweight aggregate significantly reduces the self-weight of the mortar pad and improves the thermal insulation and sound insulation performance of the wall; a three-dimensional network structure is formed by water-absorbing agent, which toughens and prevents slagging when dry, and locks in water and resists cracking after activation.

[0111] 2. The water-soluble binder has a melting point below 200℃ and can be melted and molded at a low temperature of 80~140℃, resulting in low production energy consumption. It dissolves quickly in water and completely melts within 180 seconds after being soaked in water, only delaying the early hydration of cement and not damaging the long-term mechanical properties of mortar.

[0112] 3. The sandwich-type sheet-like grid support base is integrally hot-pressed and formed, and the mortar particles can penetrate the grid to form an interlocking structure, resulting in higher overall structural strength of the mortar pad;

[0113] 4. Water-activated precast mortar pads are transported without leakage or on-site mixing dust, demonstrating significant advantages in green construction.

[0114] 5. The raw materials are common and readily available. The entire preparation process only requires ordinary mixing equipment and hot pressing molds, which can easily achieve industrial mass production. It has excellent storage stability and is suitable for various masonry projects such as aerated concrete blocks, concrete bricks, and prefabricated wall panels.

[0115] This invention uses a low-temperature hot-melt, water-soluble binder that dissolves quickly in water, combined with two lightweight aggregates and a water absorbent, sandwiched with a sheet-like grid supporting the substrate and hot-pressed into a dry mortar pad. The dry pad can be activated into masonry mortar by sprinkling water on site. It has the advantages of green construction, lightweight and high strength, convenient construction, and stable mechanical properties, and has high engineering promotion value.

[0116] In summary, the water-activated precast mortar pad of the present invention has water-activated properties, does not damage the long-term mechanical properties of mortar, is lightweight and high-strength, is easy to produce, has low production cost, and is suitable for large-scale promotion and application.

[0117] Therefore, it is evident that the objective of this invention has been fully and effectively achieved. The function and structural principles of this invention have been demonstrated and explained in the embodiments. Any modifications can be made to the implementation methods without departing from these principles. Therefore, this invention includes all modified embodiments based on the spirit and scope of the claims.

Claims

1. A water-activated precast mortar pad, comprising the following raw materials in parts by weight: 70-80 parts of cementitious material, characterized in that, The water-activated precast mortar pad further includes a sheet-like mesh support matrix and the following raw materials in parts by weight: 10-20 parts lightweight closed-cell aggregate, 2-6 parts lightweight open-cell aggregate, 0.2-1 part water absorbent, and 5-15 parts water-soluble binder. The water-soluble binder has a melting point below 200°C and completely melts and dissolves within 180 seconds after being wetted by water. The water-activated precast mortar pad is prepared by the following method: The cementitious material, the lightweight closed-cell aggregate, the lightweight open-cell aggregate, the water absorbent and the water-soluble binder are mixed evenly to obtain a dry-mix premix. Half the mass of the dry premix material is laid flat in the molding mold and leveled. Then, the sheet mesh support base is laid flat on the half mass of the dry premix material. The remaining dry premix material is then laid flat on the sheet mesh support base and scraped flat. The material is hot-pressed using a hot-pressing process. After hot pressing, it is naturally cooled to room temperature, and then demolded after the water-soluble adhesive has completely solidified.

2. The water-activated precast mortar pad as described in claim 1, characterized in that, The cementing material is cement.

3. The water-activated precast mortar pad as described in claim 1, characterized in that, The lightweight closed-cell aggregate is expanded glass.

4. The water-activated precast mortar pad as described in claim 1, characterized in that, The lightweight, open-cell aggregate is expanded perlite.

5. The water-activated precast mortar pad as described in claim 1, characterized in that, The absorbent is selected from at least one of 0.5 mm short wood fibers, 2 mm wood cellulose and 0.3 mm polypropylene short fibers.

6. The water-activated precast mortar pad as described in claim 1, characterized in that, The water-soluble binder is selected from at least one of sorbitol, urea, magnesium acetate, and polyethylene glycol.

7. The water-activated precast mortar pad as described in claim 1, characterized in that, The sheet-like mesh support substrate is a glass fiber mesh cloth, and the mesh aperture of the glass fiber mesh cloth is 4mm~6mm.

8. The water-activated precast mortar pad as described in claim 1, characterized in that, The thickness of the water-activated precast mortar pad is 2mm to 10mm.

9. A method for preparing a water-activated precast mortar pad as described in claim 1, characterized in that, Includes the following steps: S1: Mix the cementitious material, the lightweight closed-cell aggregate, the lightweight open-cell aggregate, the water absorbent and the water-soluble binder evenly to obtain a dry-mix premix; S2: Spread half the mass of the dry premix into the molding die and level it. Then spread the sheet mesh support base on the half mass of the dry premix and spread the remaining dry premix on the sheet mesh support base and scrape it flat. S3: Hot-pressed molding using a hot-pressing process; S4: After hot pressing, allow the material to cool naturally to room temperature. Once the water-soluble binder has completely solidified, demold the material to obtain the water-activated precast mortar pad.

10. The method for preparing water-activated precast mortar pads as described in claim 9, characterized in that, In step S3, the temperature of the hot pressing process is 80℃~140℃, the pressure of the hot pressing process is 1.5MPa~2.0MPa, and the time of the hot pressing process is 10min~15min.