Preparation method of graded pre-mineralization-slow release activation synergistic enhancement industrial solid waste low-carbon grouting material

By employing a graded pre-mineralization-slow-release activation synergistic enhancement method, the conflict between alkali activation and CO2 mineralization processes is resolved, achieving the dual requirements of efficient solid waste alkali activation and stable CO2 mineralization. This enhances the strength and carbon sequestration efficiency of the material, making it suitable for the industrial production of multi-element solid waste low-carbon grouting materials.

CN123106079APending Publication Date: 2026-11-17ZAOZHUANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611303072.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-26
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies for preparing low-carbon cementitious materials present a conflict between alkali activation and CO2 mineralization processes, resulting in excessive surface mineralization, low internal mineralization, and insufficient overall carbon sequestration utilization. This fails to simultaneously meet the dual requirements of efficient solid waste alkali activation and stable CO2 mineralization.

Method used

A graded pre-mineralization-slow-release activation synergistic enhancement method is adopted. Steel slag and blast furnace slag are graded and lightly CO2 pre-mineralized to form a rigid mineralized shell and an active core. Combined with deep mechanical activation of coal gangue and fly ash, a slow-release composite activator is added to carry out three-stage gradient mineralization maintenance, matching the alkali release rate and CO2 mineralization rate to achieve synergistic hydration-mineralization dual-pathway.

Benefits of technology

It significantly improves mineralization depth and uniformity, increases 28-day compressive strength by more than 40%, increases unit carbon sequestration by 20%-50%, significantly improves material volume stability and durability, reduces production costs and energy consumption, and is suitable for high-volume, low-carbon, and environmentally friendly applications of multi-component solid waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106079A_ABST
    Figure CN123106079A_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing a graded pre-mineralization-slow-release activation synergistic enhancement low-carbon grouting material for industrial solid waste, belonging to the technical field of industrial solid waste grouting material preparation. The method includes: firstly, using industrial solid waste coal gangue, fly ash, slag, and steel slag as raw materials, performing graded pretreatment; adding a slow-release composite activator and a water-reducing agent to the obtained pre-mineralized calcium-rich powder and activated silicon-aluminum-rich powder to obtain graded mineralized core-shell aggregate; then adding the graded mineralized core-shell aggregate to a slurry; pouring the resulting slurry into a mold to prepare a specimen; then subjecting the obtained specimen to three-stage gradient CO2 mineralization curing; finally, removing the cured specimen and performing standard curing to a specified age. This invention achieves simultaneous improvement in material performance and carbon sequestration efficiency through the dual-stage synergy of powder pre-mineralization and hardened body mineralization, and the rhythm matching of slow-release activation and mineralization diffusion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of preparation technology of industrial solid waste grouting materials, specifically to a method for preparing a graded pre-mineralization-slow-release activation synergistic enhancement type low-carbon industrial solid waste grouting material. Background Technology

[0002] my country has a massive stockpile of industrial solid waste, with annual production remaining consistently high, and the overall level of resource utilization is low. Large quantities of industrial solid waste, such as coal gangue, fly ash, slag, and steel slag, have been stockpiled for extended periods without adequate resource utilization and proper disposal. This not only wastes land resources but also easily leads to soil, water, and air pollution, posing significant safety risks such as landslides and collapses, creating prominent environmental and safety hazards and seriously threatening regional ecological stability and production safety. Meanwhile, underground engineering projects such as shield tunnels and mine backfilling have huge demands for cementing materials. Traditional cement-based materials have high carbon emission intensity, making it difficult to meet the requirements of low-carbon construction. Utilizing industrial solid waste combined with CO2 mineralization technology to prepare low-carbon cementing materials, achieving the dual benefits of solid waste resource utilization and carbon sequestration, has become an important direction for industry development.

[0003] Existing technologies mainly fall into two categories: The first is the multi-component solid waste alkaline-activated hydration technology, which enhances the hydration activity of solid waste through a combination of mechanical grinding and chemical activation, enabling the synergistic utilization of multiple solid wastes. However, this technology relies solely on a single-path hydration reaction for strength enhancement, resulting in weak later-stage strength growth under high solid waste content, and it lacks CO2 sequestration benefits. Furthermore, the strongly alkaline components react rapidly with CO2 to form a surface passivation layer, making it inherently unsuitable for subsequent mineralization enhancement processes. The second is the stepwise CO2 mineralization technology, primarily targeting single tailings. It employs supercritical stepwise mineralization to enhance powder activity, but this technology is designed for loose powders, relies on high-pressure conditions of 8-10 MPa, has high equipment energy consumption, and a small processing scale. It is only suitable for the pretreatment of high-value powders and cannot be directly adapted to the industrial production of multi-component solid waste grouting materials.

[0004] For multi-element solid waste systems consisting of coal gangue, fly ash, slag, and steel slag, existing technologies employing mechanical-chemical composite activation coupled with CO2 mineralization mostly pursue the highest possible carbon fixation rate and aggregate mechanical strength, tending towards deep mineralization. However, they fail to consider the inherent technical defects—the alkali activation system and the CO2 mineralization pathway are fundamentally in conflict. Alkaline components readily react with CO2 to form a dense passivation layer on the surface, blocking the internal mineralization and hydration processes. Simply optimizing the mineralization parameter gradient cannot fundamentally solve this technical problem. To address this technical problem, those skilled in the art typically employ time-sequential curing and system component buffer modification to mitigate the conflict between the two processes. Time-sequential curing avoids real-time competitive reactions by first completing alkali-activated gelation and then proceeding with carbonization and mineralization, but this can easily lead to excessive surface mineralization, low internal mineralization, and insufficient overall carbon sequestration utilization. Modification by adding calcium- and aluminum-rich minerals for pH buffering has limited buffering capacity and is difficult to adapt to long-term, high-concentration CO2 mineralization conditions. Simply relying on process parameters such as pressure, moisture content, and temperature for control has a narrow adjustment window and cannot fundamentally resolve the inherent game between alkali activation and mineralization.

[0005] In summary, existing technologies mostly focus on macroscopic operating condition control and overall system component optimization, achieving only a performance compromise and failing to simultaneously meet the dual requirements of efficient solid waste alkali activation and stable CO2 mineralization in the same reaction system. Therefore, there is an urgent need to develop a low-carbon cementitious material preparation technology compatible with both alkali activation and mineralization reactions. Summary of the Invention

[0006] The purpose of this invention is to provide a method for preparing a graded pre-mineralization-slow-release activation synergistic enhancement low-carbon grouting material for industrial solid waste. This method involves graded treatment of multi-component solid waste according to its component characteristics. First, calcium-rich solid waste such as steel slag and blast furnace slag undergoes low-pressure CO2 pre-mineralization modification to form functional micro-aggregates with a "rigid mineralized shell + active core." Then, silicon-aluminum-rich solid waste such as coal gangue and fly ash undergoes deep mechanical activation to release active components. After compounding, a weakly alkaline slow-release composite activator is added to prepare the grout. Following initial curing, a three-stage gradient mineralization curing process is performed. Through the dual-stage synergy of powder pre-mineralization and hardened body mineralization, and the rhythm matching of slow-release activation and mineralization diffusion, the material performance and carbon sequestration efficiency are simultaneously improved.

[0007] To achieve the above objectives, the present invention adopts the following technical solution: A method for preparing a graded pre-mineralization-slow-release activation synergistic enhancement low-carbon grouting material for industrial solid waste includes the following steps: a. Using industrial solid waste coal gangue, fly ash, slag, and steel slag as raw materials, the slag and steel slag are graded and lightly CO2 pre-mineralized to obtain pre-mineralized calcium-rich powder. The pre-mineralized calcium-rich powder only forms a continuous carbonate shell on the surface, and its core minerals show no obvious mineralization according to XRD. The coal gangue and fly ash are deeply mechanically activated to release active components, resulting in activated silicon-aluminum-rich powder. A slow-release composite activator and a water-reducing agent are added to the pre-mineralized calcium-rich powder and activated silicon-aluminum-rich powder to obtain graded mineralized core-shell aggregate as a carrier. b. Add the graded mineralized core-shell aggregate to the slurry, pour the resulting slurry into a mold, and obtain the specimen after standard curing and demolding; c. Place the specimens obtained in step b in a sealed mineralization curing device for three-stage gradient CO2 mineralization curing: c1. Permeation and diffusion stage: CO2 concentration 20%~30%, gas pressure 0.05~0.12MPa, temperature 25~35℃, relative humidity 60%~75%, duration 2~3 hours; In this stage, CO2 slowly permeates into the interior of the specimen, and the crystal nuclei introduced by the graded light CO2 pre-mineralization modification start the internal mineralization reaction. Combined with the low alkalinity of the slow-release activator in the early stage, the rapid carbonization and pore blockage of the shell layer are avoided. c2. Main mineralization reaction stage: CO2 concentration 70%~95%, gas pressure 0.15~0.30MPa, temperature 35~50℃, relative humidity 50%~70%, duration 8~20 hours; in this stage, CO2 reacts fully with calcium and magnesium components to generate carbonate precipitates that fill the pores, while the slow-release composite activator gradually releases alkaline components, promoting the synergistic advancement of hydration and mineralization. c3. Stabilization and solidification stage: CO2 concentration 10%~20%, gas pressure 0.02~0.06MPa, temperature 20~25℃, relative humidity 70%~90%, duration 12~20 hours; this stage stabilizes the mineralization reaction, allows the hydration reaction to continue, and makes it difficult for external carbonate ions to enter the core in large quantities; it avoids rapid decompression that could cause the carbonate products to crack, thus ensuring the stability of the structural volume. d. Following step c, after the mineralization curing is completed, the specimens are taken out and subjected to standard curing until the specified age.

[0008] In the preparation method of the above-mentioned graded premineralization-slow-release activation synergistic enhancement industrial solid waste low-carbon grouting material, in step a, the weight ratio of each raw material in the graded mineralized core-shell aggregate is as follows: 25-45 parts of premineralized calcium-rich powder, 55-75 parts of activated silicon-rich aluminum powder, 3-6 parts of slow-release composite activator, and 0.2-0.8 parts of water-reducing agent.

[0009] The above-mentioned method for preparing a graded pre-mineralization-slow-release activation synergistic enhancement industrial solid waste low-carbon grouting material includes 5-15 parts of steel slag and 20-30 parts of blast furnace slag in the pre-mineralized calcium-rich powder; and 20-40 parts of coal gangue and 30-35 parts of fly ash in the activated silicon-aluminum-rich powder.

[0010] The above-mentioned method for preparing a graded pre-mineralization-slow-release activating synergistic enhancement industrial solid waste low-carbon grouting material, in step a, the process conditions for graded light CO2 pre-mineralization modification are as follows: firstly, steel slag is magnetically separated to remove iron, and then it and slag are ground separately to a specific surface area of ​​420-480 m² / kg to obtain calcium-rich mixed powder; finally, the calcium-rich mixed powder is placed in a reactor, and CO2 gas is introduced for intermittent stirring pre-mineralization treatment: CO2 concentration 20%-40%, gas pressure 0.1-0.3 MPa, temperature 30-40℃, relative humidity 70%-80%, treatment time 3-6 hours; after treatment, a porous rigid carbonate shell and nanocrystal nuclei are formed on the surface of the calcium-rich mixed powder, while more than 70 wt% of free calcium oxide in the steel slag is dissolved.

[0011] In the preparation method of the above-mentioned graded premineralization-slow release activation synergistic enhancement industrial solid waste low-carbon grouting material, in step a, during deep mechanical activation: coal gangue is coarsely crushed to a particle size ≤10mm, ground in a ball mill to a specific surface area of ​​450~520m² / kg, and the undersize is obtained by passing through a 0.075mm square hole sieve; fly ash is dried to a moisture content ≤1%, ground to a specific surface area of ​​450~520m² / kg, and the undersize is obtained by passing through a 0.075mm square hole sieve.

[0012] The above-mentioned method for preparing a graded pre-mineralization-slow-release activating synergistic reinforced low-carbon grouting material for industrial solid waste, in step a, the slow-release composite activator includes sodium sulfate, low-modulus modified water glass and stearic acid coated calcium hydroxide, the mass ratio of the three is 3:2:1; the water-reducing agent is a polycarboxylate-based water-reducing agent.

[0013] In the preparation method of the above-mentioned graded premineralization-slow release activation synergistic enhancement industrial solid waste low-carbon grouting material, in step b, when the graded mineralized core-shell aggregate is added to the shield tunnel synchronous grouting material, the weight ratio of each raw material is as follows: 75-90 parts of graded mineralized core-shell aggregate, 10-25 parts of silicate cement, 3-8 parts of bentonite, 0.1-0.3 parts of hydroxypropyl methylcellulose ether anti-dispersant, and 40-60 parts of mixing water.

[0014] In the preparation method of the above-mentioned graded premineralization-slow release activation synergistic enhancement industrial solid waste low-carbon grouting material, in step b, when the graded mineralized core-shell aggregate is added to the coal mine backfill material, the weight ratio of each raw material is as follows: 80-100 parts of graded mineralized core-shell aggregate, 0.1-20 parts of silicate cement, and 35-50 parts of mixing water.

[0015] In the above-mentioned method for preparing a graded pre-mineralization-slow-release activating synergistic enhancement industrial solid waste low-carbon grouting material, in step b, the mold is a cubic mold with a side length of 70.7 mm or 100 mm, or a cylindrical mold with a diameter of 50 mm × a height of 100 mm.

[0016] In the preparation method of the graded pre-mineralization-slow release activation synergistic enhancement industrial solid waste low-carbon grouting material mentioned above, in step b, the material is demolded after curing for 18 to 24 hours at a temperature of 20±2℃ and a relative humidity of ≥ 95%.

[0017] Compared with the prior art, the present invention brings the following beneficial technical effects: (1) This invention resolves the inherent conflict in the alkali-activated CO2 mineralization process, achieving synergistic enhancement through the hydration-mineralization dual pathway. A slow-release composite activator is used to adapt to the CO2 diffusion rate, combined with pre-mineralized nuclei to induce nucleation within the matrix, fundamentally avoiding passivation caused by rapid surface carbonization; the mineralization depth is increased by more than 40%, and the uniformity of mineralization within the matrix is ​​significantly improved. Compared to the unmineralized control group, the 28-day compressive strength of the sample is increased by no less than 40%, and the carbon fixation per unit area of ​​the material can reach 120–160 g CO2 / kg, which is 20%–50% higher than traditional hardened body mineralization technology, effectively achieving the technical effect of synergistic enhancement through the hydration-mineralization dual pathway.

[0018] (2) Pre-mineralization achieves multiple modifications, simultaneously improving volume stability and stability. This invention first performs graded light CO2 pre-mineralization modification on slag and steel slag to obtain pre-mineralized calcium-rich powder; it then performs deep mechanical activation on coal gangue and fly ash to release active components, obtaining activated silicon-aluminum-rich powder; and mixes it with a slow-release composite activator and a water-reducing agent to obtain graded mineralized core-shell aggregate. The process of this invention simultaneously achieves three functions: the digestion of free CaO in steel slag, the introduction of nanocrystalline nuclei, and the construction of a rigid shell: the free CaO digestion rate reaches more than 70%, and the autoclave stability changes from unqualified to qualified; the rigid mineralized particles, as functional micro-aggregates, play a role in skeleton constraint and pore filling, reducing the 28-day drying shrinkage rate by more than 30% and the water immersion strength loss rate by less than 3%, significantly improving the volume stability and durability of the material during long-term service.

[0019] (3) High solid waste content, low carbon and environmentally friendly, with strong adaptability to engineering scenarios. The total solid waste content can reach more than 80%, and the amount of ordinary silicate cement can be reduced to less than 20%. Each ton of material can reduce CO2 emissions by 200-350 kg, which has the dual environmental benefits of solid waste disposal and carbon sequestration. The anti-dispersion and low shrinkage formula optimized for shield tunneling grouting scenarios can be adapted to complex strata such as water-rich sand layers and fractured zones, effectively avoiding engineering problems such as grout dilution and shrinkage cracking, and ensuring the compactness of backfill and long-term water-blocking reinforcement effect.

[0020] (4) The low-pressure process is suitable for industrialization and has outstanding economic benefits. Both powder pre-mineralization and hardened body mineralization adopt low-pressure conditions within 0.3MPa, eliminating the need for supercritical high-pressure equipment, reducing equipment investment by more than 60%, and significantly reducing operating energy consumption; the production process is compatible with existing solid waste grinding and building material preparation production lines, making it easy to scale up and promote, and the overall production cost is 15% to 25% lower than that of similar mineralized materials.

[0021] (5) Systematic innovation of graded treatment system with clear technical barriers. This invention breaks away from the traditional thinking of "optimization of single mineralization link" and constructs a full-link innovation system of "graded premineralization - activation system regulation - maintenance process synergy". It is different from the existing simple ratio optimization or single-step mineralization improvement and has significant beneficial technical effects. Attached Figure Description

[0022] The present invention will be further described below with reference to the accompanying drawings: Figure 1 This is a flowchart illustrating the preparation process of the grouting material of the present invention. Figure 2 This is a time history curve of the three-stage gradient CO2 mineralization maintenance parameters of the present invention; Figure 3 Comparison of compressive strength before and after mineralization 28 days under different solid waste ratios; Figure 4 Comparison of the microstructure of the material before and after mineralization; Figure 5 Radar chart comparing the performance of coal mine filling and shield tunneling grouting products. Detailed Implementation

[0023] This invention proposes a method for preparing a graded pre-mineralization-slow-release activation synergistic enhancement low-carbon grouting material for industrial solid waste. To make the advantages and technical solutions of this invention clearer and more explicit, the invention will be further described below with reference to specific embodiments.

[0024] The CO2 concentration mentioned in this invention refers to the CO2 volume concentration.

[0025] The technical concept of this invention lies in: using industrial solid waste as the main raw material to achieve its resource utilization; preparing graded mineralized core-shell aggregate through pretreatment of industrial solid waste; using the graded mineralized core-shell aggregate as a carrier to construct a synergistic regulatory structure of "particle surface mineralization control and system alkalinity gradient release," thus solving the technical problem of the conflict between the alkali activation system and the CO2 mineralization reaction; the core of the graded mineralized core-shell aggregate is loaded with deeply mechanically activated coal gangue and fly ash, ensuring that the silica-alumina phase of the industrial solid waste is fully depolymerized and forms a cementitious phase; the mineralized shell can block CO2 from directly invading the core; the structural design of the mineralized shell allows for the regulation of the dissolution rate of the slow-release composite activator during the later mineralization process, so that the alkali release rate and the CO2 mineralization rate are dynamically matched, overcoming the defects of traditional slow-release activators that are easily carbonized and broken down, and slow-release failure, and alleviating the reaction conflict between alkali activation and carbon dioxide mineralization. This core-shell aggregate is prepared by modifying industrial solid waste, and the carrier itself is rich in calcium from steel slag and blast furnace slag as the shell, without the need for the addition of other calcium-rich components. This invention eliminates the need for a strict segmented process of alkali activation and curing followed by mineralization and carbonization. It allows for simultaneous alkali activation and CO2 mineralization after molding, simplifying the production process and providing good process compatibility.

[0026] The present invention will be further described in detail below with reference to specific embodiments.

[0027] Example 1: like Figure 1 As shown, a method for preparing a graded pre-mineralization-slow-release activation synergistic enhancement industrial solid waste low-carbon grouting material includes the following steps: Step 1: Graded pretreatment and composite activation of industrial solid waste: Four types of industrial solid waste, namely coal gangue, fly ash, slag and steel slag, are selected as raw materials and divided into two categories according to their component characteristics: calcium-rich solid waste (slag and steel slag) and silicon-aluminum-rich solid waste (coal gangue and fly ash), and differentiated pretreatment is carried out respectively.

[0028] (1) Low-pressure pre-mineralization modification of calcium-rich solid waste: After iron removal by magnetic separation, steel slag and ore slag are ground separately to a specific surface area of ​​420-480 m² / kg, and mixed evenly in proportion to obtain calcium-rich mixed powder; the calcium-rich mixed powder is placed in a low-pressure horizontal mineralization reactor, and CO2 gas is introduced for intermittent stirring pre-mineralization treatment: CO2 volume concentration 20%-40%, gas pressure 0.1-0.3 MPa, temperature 30-40℃, relative humidity 70%-80%, treatment time 3-6 hours; after the pre-mineralization is completed, the material is discharged to obtain pre-mineralized calcium-rich powder. A porous rigid carbonate shell and nanocrystal nuclei are formed on the surface of the powder, while more than 70% of the free CaO in the steel slag is dissolved.

[0029] (2) Deep mechanical activation of silicon-aluminum-rich solid waste: Coal gangue is coarsely crushed by a jaw crusher to a particle size of no more than 10 mm, and then ground by a ball mill to a specific surface area of ​​450-520 m² / kg. After sieving, the powder passing through a 0.075 mm square hole sieve is collected. Fly ash is dried to a moisture content of no more than 1%, ground to a specific surface area of ​​450-520 m² / kg, and the undersize material is collected by passing through a 0.075 mm square hole sieve. The two are mixed evenly in proportion to obtain activated silicon-aluminum-rich powder.

[0030] (3) Mix the two types of pretreated powders evenly according to the following mass proportions to obtain composite solid waste powder. Premineralized calcium-rich powder: 25-45 parts (of which steel slag 5-15 parts and blast furnace slag 20-30 parts) Activated silicon-aluminum-rich powder: 55-75 parts (of which coal gangue 25-40 parts and fly ash 30-35 parts)

[0031] (4) Add a slow-release composite activator and a water-reducing agent to the composite solid waste powder to obtain graded mineralized core-shell aggregate. The weight ratio of each raw material is as follows: 25-45 parts of pre-mineralized calcium-rich powder, 55-75 parts of activated silicon-aluminum-rich powder, 3-6 parts of slow-release composite activator, and 0.2-0.8 parts of water-reducing agent. In the graded mineralized core-shell aggregate, the slow-release composite activator and the water-reducing agent are mixed together as functional powder materials and do not participate in the core-shell structure. The slow-release composite activator plays a role in subsequent steps.

[0032] The slow-release composite activator is composed of sodium sulfate, low-modulus modified water glass, and stearic acid-coated calcium hydroxide in a mass ratio of 3:2:1. The water-reducing agent is a polycarboxylate-based high-efficiency water-reducing agent.

[0033] Step 2: Determine the material ratio according to different engineering scenarios

[0034] (1) The proportion of the shield tunneling synchronous grouting material, by weight: 75-90 parts of graded mineralized core-shell aggregate, 10-25 parts of ordinary Portland cement, 3-8 parts of bentonite, 0.1-0.3 parts of hydroxypropyl methylcellulose ether anti-dispersant, and 40-60 parts of mixing water. Control indicators: grout fluidity 200-280mm, bleeding rate not greater than 1.5%, initial setting time 6-12h, and grout density 1.6-2.1g / cm³.

[0035] (2) Coal mine backfill material mix proportions, by weight: 80-100 parts graded mineralized core-shell aggregate, 0.1-20 parts ordinary Portland cement, and 35-50 parts mixing water. Control indicators: slurry fluidity 180-270 mm, bleeding rate not greater than 2%, and initial setting time 4-10 h.

[0036] Add the measured solid components to a forced mixer and dry mix for 2-3 minutes until homogeneous. Then add the mixing water and continue mixing for 3-5 minutes until the slurry is homogeneous and free of lumps.

[0037] A radar chart comparing the performance of products in two scenarios, coal mine backfilling and tunnel boring machine grouting, is shown below. Figure 5 As shown.

[0038] Step 3: Casting and Initial Curing: Pour the slurry obtained in Step 2 into the mold and vibrate it on a vibrating table for 1-3 minutes to remove air bubbles. The mold is a cube with a side length of 70.7mm or 100mm, or a cylinder with a diameter of 50mm × height of 100mm. After casting, cover with plastic film to prevent moisture evaporation. Curing is carried out for 18-24 hours at a temperature of 20±2℃ and a relative humidity of not less than 95%, after which the specimen is demolded to allow the initial pore skeleton and mechanical strength to be formed.

[0039] Step 4, Gradient Mineralization Curing: Place the demolded specimen in a sealed mineralization curing device and perform CO2 mineralization curing according to the following three-stage gradient regime, forming a two-stage synergy with powder pre-mineralization, such as... Figure 2 As shown.

[0040] The first stage (penetration and diffusion stage): CO2 concentration 20%–30%, gas pressure 0.05–0.12 MPa, temperature 25–35℃, relative humidity 60%–75%, duration 2–3 hours. In this stage, CO2 slowly penetrates into the interior of the specimen, initiating the internal mineralization reaction with the help of crystal nuclei introduced by pre-mineralization. Combined with the low initial alkalinity of the slow-release activator in the system, rapid carbonization and pore blockage on the surface are avoided.

[0041] The second stage (main mineralization reaction stage): CO2 concentration 70%–95%, gas pressure 0.15–0.30 MPa, temperature 35–50℃, relative humidity 50%–70%, duration 8–20 hours. In this stage, CO2 reacts fully with the internal calcium and magnesium components to generate carbonates that fill the pores, while a slow-release activator gradually releases alkaline components, promoting the synergistic advancement of hydration and mineralization.

[0042] The third stage (stabilization and solidification stage): CO2 concentration 10%–20%, gas pressure 0.02–0.06 MPa, temperature 20–25℃, relative humidity 70%–90%, duration 12–20 hours. This stage allows the mineralization reaction to gradually stabilize, while the hydration reaction continues, avoiding rapid depressurization that could cause cracking of the carbonate products and ensuring structural volume stability.

[0043] During the mineralization curing process, CO2 gas is supplied through industrial flue gas purification, cement kiln tail gas recovery, or liquid CO2 gasification. After mineralization curing, the specimens are removed and subjected to standard curing until the specified age. This invention compares the specimens before and after mineralization; the SEM microstructure comparison images of the mineralized specimens are shown below. Figure 4 As shown, from Figure 4 It can be seen that the microstructure of the unmineralized sample is loose, with a large number of continuous pores and weak interfacial areas. After mineralization curing, the internal pores of the sample are filled with a large amount of carbonate crystals generated, and CSH gel and mineralization products grow intertwined, significantly improving the density of the matrix. At the same time, it can be observed that the core-shell interface of the premineralized particles is clear, and the rigid shell is tightly bonded to the hydrated matrix, effectively playing the role of micro-aggregate skeleton constraint.

[0044] Performance testing: The following performance tests were conducted on the specimens after mineralization curing: Compressive strength: The compressive strength at 3d, 7d, and 28d was tested, with the 28d compressive strength being at least 40% higher than that of the unmineralized control group with the same mix ratio; CO2 mineralization carbon fixation: The carbonate content in the specimens was determined by thermogravimetric analysis or acid decomposition, and the CO2 fixation per unit mass of cementitious material was calculated, not less than 120gCO2 / kg; Flowability and bleeding rate: Tested according to the method specified in GB / T 8077; Setting time: Tested according to the method specified in GB / T1346; Volume stability: The 28d drying shrinkage rate was tested, not greater than 0.08% for shield grouting type; Autoclave stability was tested and deemed qualified; Durability: The impermeability grade and the strength loss rate after 28d water immersion were tested; Microstructure and phase analysis: The microstructure and pore filling of the mineralization products were observed using scanning electron microscopy (SEM), and X-ray diffraction was used. X-ray diffraction (XRD) was used to analyze the phase composition of the mineralization products. When the core performance indicators for the corresponding engineering scenario meet the control requirements, the batch of materials is deemed qualified. A bar chart comparing the compressive strength before and after mineralization at 28 days is shown below. Figure 3 As shown, from Figure 3 It can be seen that after CO2 mineralization curing, the 28-day compressive strength of the four solid waste-based formulations (A, B, C, and D) was significantly improved, with an improvement of 82% to 87%, which is much higher than the 9% improvement of the pure cement system in group E. This proves that CO2 mineralization has a more prominent enhancing and synergistic effect on solid waste-based cementitious materials. It also verifies the technical effect of synergistic enhancement of mineralization and hydration under the formulation system of this invention.

[0045] Example 2: The difference from Example 1 is that in step one, the calcium-rich solid waste is not pre-mineralized and modified. Instead, the steel slag is magnetically separated to remove iron and then ground separately with the slag to a specific surface area of ​​420-480 m² / kg. This is then directly mixed with the activated silicon-aluminum-rich powder to obtain composite solid waste powder. The remaining raw material ratios, activator dosages, slurry preparation, and three-stage gradient mineralization and curing system are exactly the same as in Example 1.

[0046] The grouting material prepared in this embodiment has the following performance comparison with that of Example 1: The compressive strength of the unmineralized control group after 28 days was 16.8 MPa, and the compressive strength after 28 days of mineralization curing was 21.8 MPa, with a strength improvement rate of 29.8%; the unit carbon fixation content was 98 g CO2 / kg; the drying shrinkage rate after 28 days was 0.112%; the autoclaving stability was unqualified, and the free CaO in the steel slag was not effectively eliminated; the strength loss rate after 28 days of water immersion was 7.2%.

[0047] The results show that without the powder pre-mineralization step, the hardened body is prone to surface pore blockage, shallow mineralization depth, low carbon fixation, and the steel slag stability hazard cannot be eliminated. The overall performance of the material is significantly worse than that of Example 1 of this invention, proving that graded light pre-mineralization is a necessary step to achieve two-stage synergistic effect.

[0048] Example 3: The difference from Example 1 is that in step one, the calcium-rich mixed powder undergoes deep pre-mineralization modification treatment. The deep mineralization process conditions are: CO2 volume concentration 80%–90%, gas pressure 0.8–1.0 MPa, temperature 50–60℃, relative humidity 70%–80%, and treatment time 12–15 h. After treatment, the overall mineralization degree of the calcium-rich powder is high, the core active components react in large quantities, and the core-shell structure is destroyed. The remaining raw material ratios, activator dosage, slurry preparation, and hardened body mineralization curing regime are exactly the same as in Example 1.

[0049] The grouting material prepared in this embodiment has the following performance comparison with that of Example 1: The compressive strength of the unmineralized control group after 28 days is 15.5 MPa, and the compressive strength after 28 days of mineralization curing is 20.3 MPa, with a strength improvement rate of 31.0%; the unit carbon fixation content is 107 g CO2 / kg; the drying shrinkage rate after 28 days is 0.094%; and the autoclaving stability is qualified.

[0050] The results show that although deep premineralization can dissolve free CaO, the activity of the particle core is greatly lost, the function of "continuous hydration of the active core" is lost, the micro-aggregate effect is weakened, and the final strength and carbon fixation effect are significantly lower than those of the light premineralization scheme of this invention. This proves that the core-shell structure of "light surface mineralization and core activity retention" is the core design to achieve optimal performance.

[0051] Any parts not mentioned in this invention can be achieved by referring to existing technologies.

[0052] Those skilled in the art should recognize that the above embodiments are only used to illustrate this application and are not intended to limit this application. Any appropriate changes and variations made to the above embodiments within the essential spirit and scope of this application fall within the scope of protection claimed in this application.

Claims

1. A preparation method of a hierarchical pre-mineralization-slow-release excitation synergistically enhanced industrial solid waste low-carbon grouting material, characterized in that, The steps are as follows: a. Using industrial solid waste coal gangue, fly ash, slag, and steel slag as raw materials, the slag and steel slag are graded and lightly CO2 pre-mineralized to obtain pre-mineralized calcium-rich powder. The pre-mineralized calcium-rich powder only forms a continuous carbonate shell on the surface, and its core minerals show no obvious mineralization according to XRD. The coal gangue and fly ash are deeply mechanically activated to release active components, resulting in activated silicon-aluminum-rich powder. A slow-release composite activator and a water-reducing agent are added to the pre-mineralized calcium-rich powder and activated silicon-aluminum-rich powder to obtain graded mineralized core-shell aggregate as a carrier. b. Add the graded mineralized core-shell aggregate to the slurry, pour the resulting slurry into a mold, and obtain the specimen after standard curing and demolding; c. Place the specimens obtained in step b in a sealed mineralization curing device for three-stage gradient CO2 mineralization curing: c1. Permeation and diffusion stage: CO2 concentration 20%~30%, gas pressure 0.05~0.12MPa, temperature 25~35℃, relative humidity 60%~75%, duration 2~3 hours; In this stage, CO2 slowly permeates into the interior of the specimen, and the crystal nuclei introduced by the graded light CO2 pre-mineralization modification start the internal mineralization reaction. Combined with the low alkalinity of the slow-release activator in the early stage, the rapid carbonization and pore blockage of the shell layer are avoided. c2. Main mineralization reaction stage: CO2 concentration 70%~95%, gas pressure 0.15~0.30MPa, temperature 35~50℃, relative humidity 50%~70%, duration 8~20 hours; in this stage, CO2 reacts fully with calcium and magnesium components to generate carbonate precipitates that fill the pores, while the slow-release composite activator gradually releases alkaline components, promoting the synergistic advancement of hydration and mineralization. c3. Stabilization and solidification stage: CO2 concentration 10%~20%, gas pressure 0.02~0.06MPa, temperature 20~25℃, relative humidity 70%~90%, duration 12~20 hours; this stage stabilizes the mineralization reaction, allows the hydration reaction to continue, and makes it difficult for external carbonate ions to enter the core in large quantities; it avoids rapid decompression that could cause the carbonate products to crack, thus ensuring the stability of the structural volume. d. Following step c, after the mineralization curing is completed, the specimens are taken out and subjected to standard curing until the specified age.

2. The preparation method of the hierarchical pre-mineralization-slow-release excitation synergistically enhanced industrial solid waste low-carbon grouting material according to claim 1, characterized in that, In step a, the weight proportions of each raw material in the graded mineralized core-shell aggregate are as follows: 25-45 parts of pre-mineralized calcium-rich powder, 55-75 parts of activated silicon-aluminum-rich powder, 3-6 parts of slow-release composite activator, and 0.2-0.8 parts of water-reducing agent.

3. The preparation method of hierarchical pre-mineralization-slow-release excitation synergistically enhanced industrial solid waste low-carbon grouting material according to claim 2, characterized in that: The premineralized calcium-rich powder contains 5-15 parts steel slag and 20-30 parts blast furnace slag; the activated silicon-aluminum-rich powder contains 20-40 parts coal gangue and 30-35 parts fly ash.

4. The preparation method of hierarchical pre-mineralization-slow-release excitation synergistically enhanced industrial solid waste low-carbon grouting material according to claim 1, characterized in that: In step a, the process conditions for graded light CO2 pre-mineralization modification are as follows: First, the steel slag is magnetically separated to remove iron, and then it and the slag are ground separately to a specific surface area of ​​420-480 m² / kg to obtain calcium-rich mixed powder; finally, the calcium-rich mixed powder is placed in a reactor and CO2 gas is introduced for intermittent stirring pre-mineralization treatment: CO2 concentration 20%-40%, gas pressure 0.1-0.3 MPa, temperature 30-40℃, relative humidity 70%-80%, and treatment time 3-6 hours; after treatment, a porous rigid carbonate shell and nanocrystal nuclei are formed on the surface of the calcium-rich mixed powder, while more than 70 wt% of free calcium oxide in the steel slag is dissolved.

5. The preparation method of hierarchical pre-mineralization-slow-release excitation synergistically enhanced industrial solid waste low-carbon grouting material according to claim 1, characterized in that: In step a, during deep mechanical activation: the coal gangue is coarsely crushed to a particle size ≤10mm, then ground in a ball mill to a specific surface area of ​​450~520m² / kg, and the undersize is collected by passing through a 0.075mm square hole sieve; the fly ash is dried to a moisture content ≤1%, ground to a specific surface area of ​​450~520m² / kg, and the undersize is collected by passing through a 0.075mm square hole sieve.

6. The preparation method of hierarchical pre-mineralization-slow-release excitation synergistically enhanced industrial solid waste low-carbon grouting material according to claim 1, characterized in that: In step a, the slow-release composite activator includes sodium sulfate, low-modulus modified water glass, and stearic acid-coated calcium hydroxide, with a mass ratio of 3:2:1; the water-reducing agent is a polycarboxylate-based water-reducing agent.

7. The preparation method of a graded pre-mineralization-slow-release activation synergistic enhancement industrial solid waste low-carbon grouting material according to claim 1, characterized in that: In step b, when the graded mineralized core-shell aggregate is added to the shield tunnel synchronous grouting material, the weight ratio of each raw material is as follows: 75-90 parts of graded mineralized core-shell aggregate, 10-25 parts of silicate cement, 3-8 parts of bentonite, 0.1-0.3 parts of hydroxypropyl methylcellulose ether anti-dispersant, and 40-60 parts of mixing water.

8. The preparation method of a graded pre-mineralization-slow-release activation synergistic enhancement industrial solid waste low-carbon grouting material according to claim 1, characterized in that: In step b, when graded mineralized core-shell aggregate is added to the coal mine backfill material, the weight ratio of each raw material is as follows: 80-100 parts of graded mineralized core-shell aggregate, 0.1-20 parts of silicate cement, and 35-50 parts of mixing water.

9. The preparation method of a graded pre-mineralization-slow-release activation synergistic enhancement industrial solid waste low-carbon grouting material according to claim 1, characterized in that: In step b, the mold is a cube mold with a side length of 70.7 mm or 100 mm, or a cylindrical mold with a diameter of 50 mm and a height of 100 mm.

10. The preparation method of a graded pre-mineralization-slow-release activation synergistic enhancement industrial solid waste low-carbon grouting material according to claim 1, characterized in that: In step b, the product is cured at a temperature of 20±2℃ and a relative humidity of ≥ 95% for 18–24 hours before demolding.