Cement-based electrolytes and their preparation methods, cement-based energy storage batteries

By modifying the microporous structure of cement-based electrolytes with a ternary composite of potassium hydroxide, potassium phosphite, and polyacrylic acid, the problem of low ionic conductivity of traditional cement-based electrolytes is solved, achieving a balance between efficient ion transport and mechanical properties, making it suitable for diverse applications in building energy storage batteries.

CN123106084APending Publication Date: 2026-11-17CHINA ENERGY GREEN BUILDING MATERIAL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611426952.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-15
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Traditional cement-based electrolytes have low ionic conductivity, resulting in insufficient ion migration rate, low ion transport efficiency inside the battery, and severe interface polarization, which affects the discharge performance and cycle stability of the device and limits the application effect and promotion value of cement-based energy storage devices.

Method used

A ternary composite modification system of potassium hydroxide solution, potassium phosphite solution and polyacrylic acid was used to optimize the micropore structure of cement, construct continuous and interconnected microporous ion transport channels, improve the migration rate of hydroxide ions, and maintain the structural strength and dimensional stability of the cement matrix.

Benefits of technology

It significantly improves the ionic conductivity of cement-based electrolytes, reduces battery internal resistance, reduces polarization loss during charging and discharging, and increases the discharge capacity and energy density of individual cells, while maintaining good mechanical properties and safety, making it suitable for the use of integrated building energy storage components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106084A_ABST
    Figure CN123106084A_ABST
Patent Text Reader

Abstract

This application provides a cement-based electrolyte and its preparation method, as well as a cement-based energy storage battery, relating to the field of electrochemical technology. The raw material components of the cement-based electrolyte provided in this application include reference cement, potassium hydroxide solution, potassium phosphite solution, polyacrylic acid, and deionized water; wherein, based on the mass of the reference cement, the mass percentage content of the potassium hydroxide solution is 10%-20%, the mass percentage content of the potassium phosphite solution is 10%-20%, and the mass percentage content of the polyacrylic acid is 2%-8%. This application effectively improves the ionic conductivity of the cement-based electrolyte by optimizing the raw material compatibility and synergistically enhancing the ion conductivity of the system. The raw materials for this cement-based electrolyte are readily available, the component system is simplified, and the preparation process is simple, making it suitable for applications such as cement-based energy storage batteries and energy storage functional concrete, with excellent prospects for industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of electrochemical technology, and in particular to a cement-based electrolyte and its preparation method, and a cement-based energy storage battery. Background Technology

[0002] With the rapid development of building-integrated energy storage technology, cement-based electrolytes, which combine structural support and energy storage functions, have shown great promise in the field of solid-state building energy storage due to their advantages such as low cost, safety and leak-free operation, and good compatibility with building structures. Currently, the biggest technical bottleneck of traditional cement-based electrolytes is their low ionic conductivity. The dense, disordered porous structure formed by the hydration of the cement matrix greatly limits the ion migration rate, resulting in insufficient ion transport efficiency and severe interface polarization within the battery. Furthermore, insufficient conductivity also leads to poor discharge performance and unsatisfactory cycle stability, hindering the effectiveness and widespread application of cement-based energy storage devices. Therefore, there is an urgent need to develop cement-based electrolytes with high conductivity to effectively improve ion transport capabilities and meet the practical application requirements of building energy storage. Summary of the Invention

[0003] The purpose of this application is to provide a cement-based electrolyte and its preparation method, as well as a cement-based energy storage battery, to effectively improve the content and ion migration efficiency of free conductive ions within the cement solid matrix, thereby increasing the conductivity of the cement-based electrolyte. The specific technical solution is as follows:

[0004] The first aspect of this application provides a cement-based electrolyte, the raw material components of which include: reference cement, potassium hydroxide solution, potassium phosphite solution, polyacrylic acid and water; wherein, based on the mass of the reference cement, the mass percentage of the potassium hydroxide solution is 10%-20%, the mass percentage of the potassium phosphite solution is 10%-20%, and the mass percentage of the polyacrylic acid is 2%-8%.

[0005] In some embodiments of this application, based on the mass of the reference cement, the mass percentage of the potassium hydroxide solution is 12%-18%, the mass percentage of the potassium phosphite solution is 12%-16%, and the mass percentage of the polyacrylic acid is 3%-6%.

[0006] In some embodiments of this application, the concentration of the potassium hydroxide solution is 1.0 mol / L to 2.0 mol / L.

[0007] In some embodiments of this application, the concentration of the potassium phosphite solution is 0.03 mol / L to 0.12 mol / L.

[0008] In some embodiments of this application, the number average molecular weight of the polyacrylic acid is 2000-10000.

[0009] In some embodiments of this application, the particle size of the reference cement is 1μm-74μm.

[0010] In some embodiments of this application, the cured thickness of the cement-based electrolyte is 4mm-12mm.

[0011] The second aspect of this application provides a method for preparing the cement-based electrolyte described in the first aspect of this application, comprising the steps of:

[0012] Weigh out the reference cement powder and dry mix it to remove powder agglomerates;

[0013] Weigh potassium hydroxide solution, potassium phosphite solution and polyacrylic acid, add water and stir to mix well to obtain a transparent and homogeneous modified composite solution;

[0014] The transparent and uniform modified composite liquid is slowly sprayed into the reference cement powder in multiple batches and stirred until the slurry is fine and uniform, without dry powder lumps or free bleeding water.

[0015] The mixed slurry is poured into a molding mold, vibrated to remove air bubbles trapped inside, and then left to stand naturally until initial setting. After curing in a standard curing environment, it is demolded and cured at room temperature until fully hydrated and solidified to obtain cement-based electrolyte.

[0016] In some embodiments of this application, the dry mixing time is 2-3 minutes.

[0017] In some embodiments of this application, the "multiple times" refers to 2 to 3 times; the stirring speed is 80 r / min to 120 r / min; and the stirring time is 3 min to 5 min.

[0018] In some embodiments of this application, the vibration time is 1 min-2 min; the initial setting time is 2 h-4 h; the standard curing environment curing time is 24 h-48 h; and the room temperature curing time is 6 days-8 days.

[0019] A third aspect of this application provides a cement-based energy storage battery, including the cement-based electrolyte described in the first aspect of this application.

[0020] The beneficial effects of this application are:

[0021] (1) Significant improvement in ionic conductivity: The ternary compound modification system of potassium hydroxide + potassium phosphite + polyacrylic acid is adopted to simultaneously optimize the two dimensions of ion supply and pore reconstruction. A large number of continuous and interconnected micropores are generated inside the cement matrix. The micropores are filled with alkaline conductive electrolyte, which greatly improves the migration rate of hydroxide ions. This solves the industry pain points of high pore ratio, high ion transport resistance and low conductivity of traditional cement electrolytes from the root. When applied to energy storage batteries, it can effectively reduce the internal resistance of the battery, reduce the polarization loss of charging and discharging, and improve the discharge capacity and energy density of the single cell.

[0022] (2) Synergistic balance between mechanical and electrochemical properties: This application strictly limits the dosage of each component, solution concentration, polymer molecular weight, raw material particle size and finished product thickness parameters to avoid problems such as matrix loosening and cracking and pore blockage caused by excessive dosage of a single modifier. The modified cement electrolyte retains the excellent compressive load-bearing capacity of the cement substrate and has excellent solid ionic conductivity, perfectly meeting the "load-bearing + energy storage" composite use requirements of building energy storage integrated components.

[0023] (3) Low raw material cost and safe and reliable production: The main raw material of the formula is general standard cement, and potassium hydroxide, potassium phosphite and polyacrylic acid are all bulk chemical raw materials on the market. The procurement channels are wide and the unit price is low. The whole process is formed and cured at room temperature, without the need for complex equipment such as high temperature sintering and high pressure molding, and the production energy consumption is low. The finished product is a solid inorganic structure. The internal electrolyte is firmly adsorbed and locked by micropores. There is no risk of liquid leakage during the whole process. It is flame retardant and explosion resistant. Its safety performance is far superior to that of traditional liquid electrolyte batteries.

[0024] (4) Wide range of application scenarios: The product can be cut and processed into sheet solid electrolytes and assembled into nickel-iron system cement-based energy storage batteries; it can also be directly cast into energy storage concrete wall panels and prefabricated energy storage blocks, and integrated into the walls, basements and floors of buildings to realize the self-generated energy storage and discharge of the building itself. It is suitable for diverse applications such as household photovoltaic energy storage, industrial and commercial park energy storage, and emergency refuge building energy storage, and has a broad space for industrialization.

[0025] Of course, implementing any product or method of this application does not necessarily require achieving all of the advantages described above at the same time. Attached Figure Description

[0026] To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this application. For those skilled in the art, other embodiments can be obtained based on these accompanying drawings.

[0027] Figure 1 A schematic diagram of the cross-sectional microstructure of the cement-based electrolyte provided in this application.

[0028] In the figure, 1-reference cement solid matrix; 2-through microporous ion channel; 3-polyacrylic acid modified coating layer adsorbed on the surface of cement particles; 4-composite alkaline electrolyte (potassium hydroxide + potassium phosphite solution) filled in the micropores. Detailed Implementation

[0029] The technical solutions of this application will be clearly and completely described below with reference to the embodiments and accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. All other embodiments obtained by those skilled in the art based on this application are within the scope of protection of this application.

[0030] To address the technical shortcomings of existing traditional cement-based electrolytes, such as disordered and closed pore structures, low ionic conductivity, and difficulty in simultaneously achieving mechanical and electrical properties, this application provides a cement-based electrolyte with high ionic conductivity. By synergistically optimizing the micropore structure of cement through a ternary composite modification system of potassium hydroxide solution, potassium phosphite solution, and polyacrylic acid, a large number of continuous and interconnected microporous ion transport channels are constructed within the cement solid matrix. This significantly increases the content of internal free conductive ions and ion migration efficiency, while simultaneously ensuring the structural strength and dimensional stability of the cement matrix after curing. This solves the problems of insufficient conductivity, easy cracking, and poor cycle performance of traditional products.

[0031] The first aspect of this application provides a cement-based electrolyte, the raw material components of which include: reference cement, potassium hydroxide solution, potassium phosphite solution, polyacrylic acid and water; wherein, based on the mass of the reference cement, the mass percentage of the potassium hydroxide solution is 10%-20%, the mass percentage of the potassium phosphite solution is 10%-20%, and the mass percentage of the polyacrylic acid is 2%-8%.

[0032] In this application, potassium hydroxide solution serves as the basic alkaline ion source, dissociating to release a large amount of K+ after dissolution. + With OH - Potassium hydroxide fills the pores of cement, creating an alkaline conductive environment that provides sufficient free hydroxide ions, thus establishing a basic ion transport medium. This highly alkaline environment can fine-tune the cement hydration rate, preventing rapid hydration from causing large-scale pore closure. If the amount of potassium hydroxide added is too low, the amount of free conductive ions inside the matrix is ​​insufficient, limiting the improvement in ionic conductivity. Excessive addition, on the other hand, leads to excessive alkali disruption of the cement mineral hydration balance, resulting in loose hydration products, a significant decrease in the overall compressive strength of the electrolyte, and defects such as crumbling, powdering, and cracking.

[0033] In this application, potassium phosphite can precisely regulate the cement hydration kinetic rate, refine the grain size of cement hydration products, reconstruct the original disordered macropores and closed blind pores of cement into dense and interconnected micropores, optimize the pore size distribution, and reduce the proportion of ineffective closed pores. Simultaneously, potassium phosphite can improve the interfacial compatibility between inorganic cement powder and organic polyacrylic acid, promoting the uniform adhesion of organic modifiers to the surface of cement particles and avoiding the problem of localized agglomeration and pore blockage by organic polymers. When the concentration and dosage of potassium phosphite solution exceed the standard, it will severely damage the cement hydration system, resulting in irregular cracks in the matrix; insufficient dosage will result in a weak pore optimization effect and failure to achieve a connected micropore structure.

[0034] In this application, polyacrylic acid, as a water-soluble polymer modifier, uniformly coats the surface of the reference cement particles during the slurry mixing stage, delaying the rapid early hydration of cement and preventing the rapid accumulation of hydration products that block newly formed pores. Polymer segments interspersed among the cement hydration products support the formation of small, interconnected pores, stabilizing the pore structure after curing and preventing micropore collapse and closure during curing. Simultaneously, polyacrylic acid possesses hydrophilic groups, enhancing the liquid retention capacity of the cement matrix and firmly adsorbing and retaining alkaline electrolyte within the microporous channels, ensuring a sufficient ion transport medium over the long term. If the molecular weight of polyacrylic acid is too low, the polymer skeleton will not provide sufficient support and will not be able to stabilize the pore structure; if the molecular weight is too high, the viscosity of the aqueous solution will increase sharply, causing the material to clump together during the mixing stage, blocking the pore channels and conversely reducing ionic conductivity.

[0035] Figure 1 This is a schematic diagram of the cross-sectional microstructure of the cement-based electrolyte provided in this application, wherein 1-a reference cement solid matrix; 2-through-type microporous ion channels; 3-polyacrylic acid modified coating layer adsorbed on the surface of cement particles; 4-composite alkaline electrolyte (potassium hydroxide + potassium phosphite solution) filled in the micropores. As can be clearly seen from the figure, after modification treatment according to this application, the polyacrylic acid modified coating layer 3 uniformly coats the surface of the reference cement solid matrix 1 particles, regulating cement hydration to generate a large number of interconnected through-type microporous ion channels 2. The composite alkaline electrolyte 4 is uniformly filled inside the micropores, forming an uninterrupted ion conduction pathway. Unlike the isolated and closed pore structure inside conventional cement, the cement-based electrolyte provided in this application has a significantly improved pore connectivity, providing a structural basis for efficient ion migration.

[0036] The cement-based electrolyte provided in this application has a clear division of labor among its raw material components, which work synergistically to simultaneously optimize the electrolyte's conductivity from three dimensions: ion source, pore control, and interface modification.

[0037] In some embodiments of this application, based on the mass of the reference cement, the mass percentage of the potassium hydroxide solution is 12%-18%, the mass percentage of the potassium phosphite solution is 12%-16%, and the mass percentage of the polyacrylic acid is 3%-6%.

[0038] In this application, based on the mass of the reference cement, the mass percentage of potassium hydroxide solution can be 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, or a range of any two of these values; the mass percentage of potassium phosphite solution can be 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, or a range of any two of these values; the mass percentage of polyacrylic acid can be 2%, 3%, 4%, 5%, 6%, 7%, 8%, or a range of any two of these values.

[0039] The water used in this application is preferably deionized water. There is no particular limitation on the amount of deionized water used in this application, as long as the purpose of this invention can be achieved. For example, the mass-to-volume ratio of the reference cement to the deionized water is 100g:(5 mL-15 mL); that is, the mass of the reference cement is 100g and the volume of the deionized water is 5 mL-15 mL.

[0040] The mass percentages of potassium hydroxide solution, potassium phosphite solution, and polyacrylic acid in this application are the optimal parameters obtained through multiple sets of comparative experiments. The synergistic effect of each component is maximized, which avoids problems such as matrix cracking, loose structure, and excessive water leakage of electrolyte due to excessive amount of a single component. At the same time, it can give full play to the pore optimization, ion replenishment, and interface improvement of the ternary modified system, and achieve a balanced improvement in both electrochemical conductivity and mechanical properties.

[0041] In some embodiments of this application, the concentration of the potassium hydroxide solution is 1.0 mol / L to 2.0 mol / L. In this application, the concentration of the potassium hydroxide solution can be 1.0 mol / L, 1.1 mol / L, 1.2 mol / L, 1.3 mol / L, 1.4 mol / L, 1.5 mol / L, 1.6 mol / L, 1.7 mol / L, 1.8 mol / L, 1.9 mol / L, 2.0 mol / L, or a range of any two of these values. When the concentration of the potassium hydroxide solution in this application is below 1.0 mol / L, the number of OH⁻ ions per unit volume of solution is low, making it impossible to construct a high-concentration alkaline conductive environment in the cement pores. When the concentration of the potassium hydroxide solution is above 2.0 mol / L, the strong alkaline corrosiveness is too strong, continuously corroding the cement clinker, damaging the hydration and hardening system, and significantly reducing the electrolyte mechanical strength after molding.

[0042] In some embodiments of this application, the concentration of the potassium phosphite solution is 0.03 mol / L to 0.12 mol / L. In this application, the concentration of the potassium phosphite solution can be 0.03 mol / L, 0.04 mol / L, 0.05 mol / L, 0.06 mol / L, 0.07 mol / L, 0.08 mol / L, 0.09 mol / L, 0.10 mol / L, 0.11 mol / L, 0.12 mol / L, or a range of any two of these values. When the concentration of the potassium phosphite solution used in this application is controlled within the above range, potassium phosphite can gently regulate the hydration rate, which is beneficial for precisely refining the pore structure. If the concentration is too low, the pore refinement modification effect is insufficient; if the concentration is too high, the strongly reducing potassium phosphite reacts violently with the cement hydration products, generating bubbles inside the matrix and forming irregular large voids, thus deteriorating the overall performance.

[0043] In some embodiments of this application, the number-average molecular weight of the polyacrylic acid is 2000-10000. In this application, the number-average molecular weight of the polyacrylic acid can be 2000, 2500, 3000, 3500, 4000, 4500, 5000, 5500, 6000, 6500, 7000, 7500, 8000, 8500, 9000, 9500, 10000, or a range of any two of these values. In this application, when the number-average molecular weight of the polyacrylic acid is below 2000, the polymer chain length is insufficient, resulting in poor film formation, poor skeletal support, and difficulty in delaying cement hydration; when the number-average molecular weight is above 10000, the water solubility of the polyacrylic acid deteriorates, the solution viscosity increases sharply, and the material agglomerates and clumps during stirring, clogging newly formed micropores and significantly reducing ion conduction efficiency.

[0044] In some embodiments of this application, the particle size of the reference cement is 1μm-74μm. The reference cement used in this application is the national standard P·I reference cement, and the particle size is controlled within 1μm-74μm by sieving (using a 200-mesh sieve). Within this particle size range, the cement particle gradation is continuous and the mixing is uniform, resulting in controllable matrix density after molding. If the proportion of large particles is too low, shrinkage cracks are likely to occur in the matrix; if the proportion of fine powder is too high, the hydration rate is too fast, and the internal pores are prone to closure.

[0045] In some embodiments of this application, the finished thickness of the cement-based electrolyte after casting and curing is 4mm-12mm. In this application, the finished thickness of the cement-based electrolyte after casting and curing can be 4mm, 5mm, 6mm, 7mm, 8mm, 9mm, 10mm, 11mm, 12mm, or any combination of two of these values. In this application, when the thickness of the cement-based electrolyte is less than 4mm, the electrolyte structure is insufficient, its mechanical load-bearing capacity does not meet the standards for building components, and it is prone to breakage under stress during battery assembly; when the thickness is greater than 12mm, the migration path of ions inside the electrolyte is too long, the ohmic internal resistance increases, and the discharge performance of the device decreases.

[0046] The second aspect of this application provides a method for preparing the cement-based electrolyte described in the first aspect of this application, comprising the steps of:

[0047] S1: Weigh the reference cement powder and dry mix it to remove powder agglomerates;

[0048] S2: Weigh potassium hydroxide solution, potassium phosphite solution and polyacrylic acid, add water and stir to mix well to obtain a transparent and uniform modified composite liquid;

[0049] S3: The transparent and uniform modified composite liquid is slowly sprayed into the reference cement powder in multiple batches and stirred until the slurry is fine and uniform, without dry powder lumps or free bleeding water.

[0050] S4: Pour the mixed slurry into the molding mold, vibrate to eliminate air bubbles trapped inside the slurry, and let it stand naturally until it initially sets; after curing in a standard curing environment, demold and continue to cure at room temperature until it is fully hydrated and solidified to obtain cement-based electrolyte.

[0051] This application does not impose any particular restrictions on the equipment used for dry mixing in S1, as long as it can achieve the purpose of this invention. For example, a reference cement powder with a particle size of 1μm-74μm after sieving can be selected and put into a vertical mixing device for dry mixing to remove powder agglomerates.

[0052] In this application, in S4, the standard curing environment refers to a temperature of 23±2℃ and a relative humidity of 60%-70%; normal temperature curing refers to a temperature of 23±5℃ and a relative humidity of ≥60%.

[0053] The method for preparing the cement-based electrolyte provided in this application is simple and can be mass-produced.

[0054] In some embodiments of this application, in S1, the dry mixing time is 2-3 minutes.

[0055] In some embodiments of this application, in S3, the "multiple times" refers to 2-3 times; the stirring speed is 80 r / min-120 r / min, and the stirring time is 3 min-5 min. In this application, the stirring speed can be 80 r / min, 85 r / min, 90 r / min, 95 r / min, 100 r / min, 105 r / min, 110 r / min, 115 r / min, 120 r / min, or a range consisting of any two of these values.

[0056] In some embodiments of this application, in step S4, the vibration time is 1-2 minutes; the initial setting time is 2-4 hours; the standard curing environment curing time is 24-48 hours; and the room temperature curing time is 6-8 days. In this application, the initial setting time can be 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, or a range consisting of any two of these values.

[0057] A third aspect of this application provides a cement-based energy storage battery, including the cement-based electrolyte described in the first aspect of this application. The cement-based energy storage battery provided by this application has the cement-based electrolyte described in the first aspect of this application assembled between its positive and negative electrodes, enabling it to replace traditional liquid electrolytes and achieve the preparation of all-solid-state cement energy storage cells. The cement-based electrolyte described in this application can be used in lightweight, ultra-thin cement-based energy storage devices and small energy storage patch concrete.

[0058] The cement-based electrolyte raw material formula parameters used in this application are controllable, the raw material procurement is convenient, the production process is simple, and it can be mass-produced on a large scale. It is suitable for the preparation of various products such as cement-based solid-state batteries and precast concrete panels with energy storage functions.

[0059] Example

[0060] The embodiments and comparative examples provided below illustrate the implementation of this application in more detail. Various tests and evaluations were conducted according to the methods described below. Furthermore, unless otherwise specified, "parts" and "%" are quality standards.

[0061] The reference cement used in the following examples and comparative examples is P·I42.5 reference cement.

[0062] Test methods and equipment:

[0063] Conductivity test: Electrochemical impedance spectroscopy was performed using an electrochemical workstation at room temperature (25±5℃) with a frequency of 100kHz-0.1Hz, an initial voltage of 0V, and a current of 100mA. The equivalent ohmic resistance R0 was extracted from the electrochemical impedance spectroscopy, and the electrolyte ionic conductivity was calculated using the formula σ=L / (S·R0), where σ is the ionic conductivity, L is the electrolyte thickness, S is the test cross-sectional area, and R0 is the equivalent ohmic resistance.

[0064] 7-day curing compressive strength test: Referring to GB / T50081 standard, using the same raw material formula and curing process as in the examples and comparative examples, 100mm×100mm×100mm cubic specimens were prepared for compressive strength testing. After curing, the specimens were removed, surface moisture was wiped off, and debris was cleaned from the bearing surface. The specimen was then placed centered on the pressure plate of the pressure testing machine, and a uniform loading rate of 1.0 MPa per second was applied, recording the failure load. The compressive strength was calculated using the formula: multiplying the 100mm specimen by a size correction factor of 0.95. The average of the three test values ​​(excluding the extreme values) was taken as the 7-day compressive strength result.

[0065] Example 1

[0066] S1: Raw material pretreatment: Weigh 100g of reference cement powder with a particle size of 1μm-74μm after sieving, put it into a vertical mixing device and dry mix for 2 minutes to remove powder agglomerates.

[0067] S2: Preparation of modified mixture: Weigh 15g of potassium hydroxide solution (concentration 1.0mol / L), 15g of potassium phosphite solution (concentration 0.07mol / L) and 2g of polyacrylic acid (number average molecular weight 2000), add 10mL of deionized water and stir at room temperature to obtain a transparent and uniform modified composite solution.

[0068] S3: Wet material mixing: The transparent and uniform modified composite liquid is slowly sprayed into the reference cement powder in 3 portions, and the mixing equipment is used to stir at low speed (100r / min) for 4 minutes until the slurry is fine and uniform, without dry powder lumps and free bleeding water.

[0069] S4: Casting, molding and curing: Pour the mixed slurry into the mold, vibrate it on a vibrating table for 2 minutes to eliminate air bubbles trapped inside the slurry, and let it stand naturally at room temperature until initial setting (3h); move it to a standard curing environment (temperature 23℃, relative humidity 65%) for curing for 36h, then demold it and continue to cure at room temperature for 7 days until complete hydration and solidification, to obtain a finished cement-based electrolyte with a thickness of 4mm.

[0070] Example 2-Example 22

[0071] Except for adjusting the relevant parameters according to Table 1, everything else is the same as in Example 1.

[0072] Comparative Examples 1-6

[0073] Except for adjusting the relevant parameters according to Table 1, everything else is the same as in Example 1.

[0074] Comparative Example 7

[0075] S1: Raw material pretreatment: Weigh 100g of reference cement powder with a particle size of 1μm-74μm after sieving, put it into a vertical mixing device and dry mix for 2 minutes to remove powder agglomerates.

[0076] S2: Add 50mL of deionized water (without any modifying reagents) to the reference cement powder and stir at room temperature until well mixed. Pour the mixed slurry into the molding mold and vibrate it on a vibrating table for 2 minutes to eliminate air bubbles trapped inside the slurry. Let it stand naturally at room temperature until initial setting (3h). Move it to a standard curing environment (temperature 23℃, relative humidity 65%) and cure for 36h before demolding. Continue to cure at room temperature for 7 days until complete hydration and solidification, to obtain a finished cement-based electrolyte with a thickness of 8mm.

[0077] Table 1

[0078] Note: " / " indicates that it does not exist.

[0079] The cement-based electrolytes obtained in each embodiment and comparative example were tested using the above-described conductivity and compressive strength test methods. The test results are shown in Table 2 below.

[0080] Table 2

[0081] As can be seen from the above results, the cement-based electrolyte prepared by the preparation method provided in Examples 1 to 22 of this application has good ionic conductivity at room temperature and 7-day standard curing compressive strength. However, in Comparative Examples 1 and 2, the amount of potassium hydroxide solution added was not controlled within the range of this application, resulting in a significant decrease in ionic conductivity and 7-day standard curing compressive strength. In Comparative Examples 3 and 4, the amount of potassium phosphite solution added was not controlled within the range of this application, resulting in a significant decrease in ionic conductivity and 7-day standard curing compressive strength. In Comparative Examples 5 and 6, the amount of polyacrylic acid added was not controlled within the range of this application, resulting in a significant decrease in ionic conductivity and 7-day standard curing compressive strength. In Comparative Example 7, no modifying reagent was added, and the micropore connectivity was significantly reduced, resulting in a significant decrease in ionic conductivity and 7-day standard curing compressive strength.

[0082] The above description is only a preferred embodiment of this application and is not intended to limit this application. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the scope of protection of this application.

Claims

1. A cement-based electrolyte, characterized in that, The raw material components include: reference cement, potassium hydroxide solution, potassium phosphite solution, polyacrylic acid, and water; Wherein, based on the mass of the reference cement, the mass percentage of the potassium hydroxide solution is 10%-20%, the mass percentage of the potassium phosphite solution is 10%-20%, and the mass percentage of the polyacrylic acid is 2%-8%.

2. The cement-based electrolyte according to claim 1, characterized in that, Based on the mass of the reference cement, the mass percentage of the potassium hydroxide solution is 12%-18%, the mass percentage of the potassium phosphite solution is 12%-16%, and the mass percentage of the polyacrylic acid is 3%-6%.

3. The cement-based electrolyte according to claim 1, characterized in that, The concentration of the potassium hydroxide solution is 1.0 mol / L to 2.0 mol / L.

4. The cement-based electrolyte according to claim 1, characterized in that, The concentration of the potassium phosphite solution is 0.03 mol / L to 0.12 mol / L.

5. The cement-based electrolyte according to claim 1, characterized in that, The number average molecular weight of the polyacrylic acid is 2000-10000.

6. The cement-based electrolyte according to claim 1, characterized in that, The particle size of the reference cement is 1μm-74μm.

7. The cement-based electrolyte according to any one of claims 1-6, characterized in that, The cured thickness of the cement-based electrolyte is 4mm-12mm.

8. A method for preparing a cement-based electrolyte according to any one of claims 1-7, characterized in that, Including the following steps: Weigh out the reference cement powder and dry mix it to remove powder agglomerates; Weigh potassium hydroxide solution, potassium phosphite solution and polyacrylic acid, add water and stir to mix well to obtain a transparent and homogeneous modified composite solution; The transparent and uniform modified composite liquid is slowly sprayed into the reference cement powder in multiple batches and stirred until the slurry is fine and uniform, without dry powder lumps or free bleeding water. The mixed slurry is poured into a molding mold, vibrated to remove air bubbles trapped inside, and then left to stand naturally until initial setting. After curing in a standard curing environment, it is demolded and cured at room temperature until fully hydrated and solidified to obtain cement-based electrolyte.

9. The preparation method according to claim 8, characterized in that, The dry mixing time is 2-3 minutes; The number of times is 2 to 3; the stirring speed is 80 r / min to 120 r / min; and the stirring time is 3 min to 5 min. The vibration time is 1-2 minutes; the initial setting time is 2-4 hours; the standard curing environment curing time is 24-48 hours; and the room temperature curing time is 6-8 days.

10. A cement-based energy storage battery, characterized in that, Includes the cement-based electrolyte according to any one of claims 1-7.