Synergistic Alkali-Activated Functional Gradient Materials for Multiple Solid Wastes and Their Preparation Methods, and Comprehensive Treatment Methods for Layered Backfilling of Gangue Hills

By preparing multi-solid waste synergistic alkali-activated functional gradient materials, the problems of heavy metal pollution, spontaneous combustion risk and structural instability in gangue piles were solved, realizing the multi-risk synergistic treatment of gangue piles, forming a gradient protection system suitable for different spatial locations, and improving the adsorption performance, flame retardant performance and structural seepage prevention performance of the materials.

CN123106089APending Publication Date: 2026-11-17CHINA UNIV OF MINING & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611472442.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies have failed to effectively address the problems of heavy metal pollution, spontaneous combustion risk, and structural instability in coal gangue piles, especially in the treatment of coal gangue piles in different spatial locations, where the requirements for material structure and performance differ and are mutually restrictive.

Method used

By employing a multi-solid-waste synergistic alkali-activated functional gradient material, using solid waste raw materials such as coal gangue, steel slag, and aluminum slag, combined with a low-alkali activator, heavy metal adsorption type, flame retardant and fireproof type, and structural seepage-proof and sealing type materials are prepared. These materials form pore-gel structures suitable for different spatial locations, achieving directional transformation of material functions, and are then used for layered backfilling treatment.

Benefits of technology

It achieves multi-risk collaborative management of coal gangue piles, effectively adsorbs heavy metals, prevents spontaneous combustion, improves structural stability, forms a gradient protection system, reduces permeability and enhances compressive strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106089A_ABST
    Figure CN123106089A_ABST
Patent Text Reader

Abstract

This invention discloses a multi-solid-waste synergistic alkali-activated functional gradient material and its preparation method, as well as a comprehensive treatment method for layered backfilling of gangue piles. The material uses coal gangue as the main silicon-aluminum source, steel slag as the active calcium source, and selectively adds aluminum slag as the aluminum source and foaming component. Modified water glass is used as a low-alkali activator, and sodium dodecyl sulfate as a foam stabilizer. Through synergistic control of the solid-to-water ratio, calcium-to-silicon ratio, silicon-to-aluminum ratio, water glass modulus, and foam stabilizer dosage, heavy metal adsorption materials, flame-retardant and fire-resistant materials, and structural seepage-proof and sealing materials are prepared under the same solid waste raw material system. Based on the above materials, a layered backfill structure is constructed consisting of a base heavy metal adsorption layer, a coal gangue compacted layer, a middle flame-retardant and fire-resistant layer, a coal gangue compacted layer, and a top structural seepage-proof and sealing layer, achieving synergistic treatment of heavy metal leaching pollution, spontaneous combustion risk, and structural instability in gangue piles. This invention has widely available raw materials, a simple process, and is suitable for large-scale engineering treatment of gangue piles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of industrial solid waste resource utilization and mine safety management technology, specifically involving a multi-solid waste synergistic alkali-activated functional gradient material and its preparation method, and a comprehensive management method for layered backfilling of gangue mountains. Background Technology

[0002] Coal gangue is a major industrial solid waste generated during coal mining and washing. In my country, the cumulative stockpile exceeds 7 billion tons, forming approximately 2,600 gangue mountains of varying sizes, occupying over 13,000 hectares, and is still increasing at a rate of about 800 million tons per year. Long-term stockpiling of coal gangue not only occupies vast amounts of land resources but also poses safety and environmental problems such as heavy metal pollution, spontaneous combustion, and structural instability. Among these issues, phosphorus (Pb) is found in the gangue. 2+ Cd 2+ Cr 6+ As 3+ Heavy metal ions can be released and migrate under the leaching effect of rainwater, causing pollution to the surrounding soil and groundwater; the oxidation of sulfides such as pyrite in gangue releases heat and continues to accumulate, which may cause spontaneous combustion of coal gangue and release harmful gases such as SO2 and CO; at the same time, the loose gangue accumulation has high porosity and poor overall stability, which may also cause geological disasters such as landslides and debris flows.

[0003] Currently, the treatment of coal gangue piles mainly employs methods such as compaction and soil covering. Their primary function is to improve surface stability and reduce direct contact between coal gangue and the external environment. However, they still have limitations in addressing issues such as spontaneous combustion within the gangue pile, heavy metal leaching and migration, and seepage control under long-term rainfall conditions. In recent years, alkali-activated cementitious materials have attracted attention in the field of mine solid waste treatment due to their high utilization rate of industrial solid waste and adjustable material composition and performance.

[0004] Existing technologies include solid waste-based functional materials for various applications such as heavy metal adsorption, fire prevention and extinguishing, and grouting reinforcement. For example, steel slag-based adsorption materials use steel slag, silicon, and aluminum as main raw materials, forming a porous structure under the action of foaming agents and foam stabilizers, and are further processed by alkaline hydrothermal treatment to obtain materials for heavy metal ion adsorption in wastewater. This type of technology mainly focuses on material design for heavy metal adsorption in wastewater; its raw material composition, pore structure formation, and hydrothermal treatment process all serve adsorption performance, which needs improvement. Furthermore, it does not address the use of coal gangue as the main silicon and aluminum source, nor does it consider the different functional requirements such as flame retardancy, fire prevention, and structural seepage prevention under layered backfilling conditions of gangue piles. Existing mine fire prevention and extinguishing materials also disclose technical solutions for constructing fire-extinguishing gels using solid raw materials such as steel slag and alkaline activators. These mainly utilize the water retention, covering, and oxygen barrier effects of the gel material to inhibit coal oxidation and heating processes. This type of technology is mainly designed for a single fire prevention and extinguishing function. Furthermore, existing technologies also disclose coal gangue powder-based grouting materials for treating road voids. These materials use coal gangue powder, fly ash, slag powder, and sand as the main solid components and are activated using water glass and alkaline components. They primarily achieve grouting reinforcement of road void areas by improving the grout's workability and its filling, bonding, and structural properties after curing. These materials are mainly aimed at filling road voids and structural reinforcement. Their application purpose and structural design differ from low-permeability sealing under long-term rainfall infiltration conditions at the top of gangue piles, and they do not involve a gradient layered treatment structure that works in conjunction with a base heavy metal adsorption layer and a central flame-retardant fireproof layer.

[0005] It is evident that although existing technologies involve heavy metal adsorption, fire prevention and extinguishing, or coal gangue-based grouting materials, these technologies are mainly designed for single functions or single engineering scenarios, and have not yet solved the problem that different spatial locations of coal gangue piles have different or even mutually restrictive requirements for material structure and performance. Summary of the Invention

[0006] The purpose of this invention is to provide a multi-solid waste synergistic alkali-activated functional gradient material and its preparation method, which can simultaneously solve the problems of heavy metal pollution, spontaneous combustion risk and structural instability.

[0007] Another objective of this invention is to provide a comprehensive treatment method for layered backfilling of waste rock piles, addressing issues such as heavy metal pollution, spontaneous combustion risk, and structural instability during waste rock pile treatment. Through multi-parameter synergistic control within the same solid waste raw material system, the method achieves a directional transformation of material function from adsorption-type to flame-retardant type and then to impermeable type, and combines this with a layered backfilling structure to achieve synergistic treatment of multiple risks associated with waste rock piles.

[0008] To achieve the above objectives, the present invention adopts the following technical solution: A multi-solid waste synergistic alkali-activated functional gradient material includes a heavy metal adsorption material comprising coal gangue, steel slag, aluminum slag, a low-alkali activator, a foam stabilizer, and water. A slurry is prepared by stirring and then solidified to form a heavy metal adsorption layer. The porosity of the heavy metal adsorption layer is 70-90%, and the specific surface area is 110-130 m². 2 / g, Pb 2+ The adsorption capacity is 90-100 mg / g, Cd 2+ The adsorption capacity is 30-40 mg / g; preferably, the porosity of the heavy metal adsorption layer is 80-85%, and the specific surface area is 125-130 m². 2 / g, Pb 2+ The adsorption capacity is 95-100 mg / g, Cd 2+ The adsorption capacity is 35-40 mg / g.

[0009] The heavy metal adsorption layer within this parameter range can ensure the number of effective adsorption pore structures, enabling the material to maintain a large effective specific surface area and heavy metal adsorption capacity while forming a high porosity.

[0010] In one preferred embodiment, the mass ratio of coal gangue, steel slag, and aluminum slag in the heavy metal adsorbent material is 40~70:20~50:1~20, the silicon-aluminum ratio is 3.2~3.5, the calcium-silicon ratio is 0.8~1.0, the solid-water ratio is 1.2~1.3, the water glass modulus is 1.6~1.7, and the foam stabilizer dosage is 0.8%~1.2%; preferably, the mass ratio of coal gangue, steel slag, and aluminum slag is 60~70:20~25:15~20.

[0011] In the aforementioned heavy metal adsorption material, a high silicon-to-aluminum ratio provides a large number of Si-OH and Al-OH active adsorption sites; a low solid-to-water ratio reserves sufficient space for the foaming reaction, and combined with the large amount of hydrogen generated by the reaction of aluminum slag with the alkaline system, as well as the stabilizing effect of SDS foam stabilizer on the bubbles, a mesoporous-macroporous composite structure with uniform pore size distribution and good connectivity is formed, so that the porosity of the system is stably increased to over 80%, providing sufficient channels for rainwater infiltration and rapid diffusion and deep adsorption of heavy metal ions; the strongly alkaline environment of low-modulus water glass promotes the full depolymerization of the silicon-aluminum phase, further increasing the concentration of active groups. Through the triple action of ion exchange, surface chelation and physical adsorption, Pb adsorption is achieved. 2+ Cd 2+ Efficient and stable curing with heavy metal ions. Experimental results show that, compared with Comparative Example 1 without SDS, the porosity of Example 1 increased from 67.8% to 82.5%, and the specific surface area increased from 89.7 m². 2 / g increased to 125.3 m 2 / g, Pb 2+ and Cd2+ The adsorption capacity increased from 72.4 mg / g and 28.6 mg / g to 98.5 mg / g and 39.2 mg / g, respectively, indicating that the combination of SDS stabilization and aluminum slag gas generation and pore formation is conducive to the formation of a porous structure with a large effective specific surface area and improves the heavy metal adsorption performance.

[0012] In one preferred embodiment, the multi-solid waste synergistic alkali-activated functional gradient material further includes a flame-retardant material comprising coal gangue, steel slag, aluminum slag, a low-alkali activator, a foam stabilizer, and water. A slurry is prepared by stirring and then solidified to form a flame-retardant layer. The flame-retardant layer has a porosity of 20-30% and a specific surface area of ​​60-70 m². 2 / g, Pb 2+ The adsorption capacity is 40-50 mg / g, Cd 2+ The adsorption capacity is 10-20 mg / g.

[0013] In one preferred embodiment, the flame-retardant and fireproof material contains coal gangue, steel slag and aluminum slag in a mass ratio of 45-55:30-40:10-20, a silicon-aluminum ratio of 2.8-3.0, a calcium-silicon ratio of 1.2-1.4, a solid-water ratio of 1.7-1.8, a water glass modulus of 1.8, and a foam stabilizer dosage of 0.5%-0.8%. Preferably, the flame-retardant and fireproof layer is disposed on the upper side of the heavy metal adsorption layer.

[0014] In the aforementioned flame-retardant and fire-resistant material, this parameter combination is used to coordinate the formation of the gel structure and high-temperature water retention performance. The combined adjustment of the silica-alumina ratio, calcium-silica ratio, water glass modulus, and foam stabilizer dosage is beneficial for forming a gel skeleton with a certain structural integrity; a moderate solid-water ratio and foam stabilizer dosage are used to regulate the material's pore structure. Under heated conditions, the moisture retained inside the material can dissipate some heat through evaporation, while the gel skeleton provides a foundation for maintaining a certain structural integrity. Experimental results show that this material has a high water retention rate at 12 h and 100℃, providing a performance basis for flame-retardant and fire-resistant functions under layered backfilling conditions in waste rock piles.

[0015] In one preferred embodiment, the multi-solid waste synergistic alkali-activated functional gradient material further includes a structural seepage-proofing and plugging material. This structural seepage-proofing and plugging material comprises coal gangue, steel slag, a low-alkali activator, and water. A slurry is prepared by stirring and then solidified to form the structural seepage-proofing and plugging layer. The porosity of the structural seepage-proofing and plugging layer is 10-20%, and its specific surface area is 20-30 m². 2 / g, Pb 2+ The adsorption capacity is 10-20 mg / g, Cd 2+ The adsorption capacity is 5-10 mg / g.

[0016] In one preferred embodiment, in the structural seepage-proof sealing material, the mass ratio of coal gangue to steel slag is 50-60:40-50, the silicon-aluminum ratio is 3.0-3.2, the calcium-silicon ratio is 1.6-1.8, the solid-water ratio is 1.9-2.1, and the water glass modulus is 1.9-2.0; preferably, the structural seepage-proof sealing layer is disposed on the upper side of the flame-retardant and fireproof layer.

[0017] This layer does not contain aluminum slag or foam stabilizers to avoid the adverse effects of aluminum slag gas generation and pore formation on the formation of a dense, impermeable structure. The high calcium-to-silicon ratio resulting from the high steel slag content promotes the formation of a large amount of CSH gel and calcium-containing crystalline phases, filling the interparticle gaps. Under high solid-to-water ratio conditions, it is beneficial to improve the packing density of coal gangue and steel slag particles, maintaining a low porosity (approximately 10-20%, preferably 14%–16%). High-modulus water glass accelerates the gel condensation reaction, further improving the matrix density. The above parameter combination is beneficial to improving the structural density and compressive strength of the material, while reducing its permeability coefficient. Experimental results show that the 28-day compressive strength of Example 3 reaches 9.2 MPa, and the permeability coefficient is 2.1 × 10⁻⁶. -9 With a flow rate of cm / s, it exhibits good structural seepage prevention performance, which can be used to reduce the infiltration of top precipitation into the interior of the gangue pile, and provide a performance basis for maintaining the structural integrity of the top sealing layer.

[0018] This invention relates to a multi-solid waste synergistic alkali-activated functional gradient material, prepared from all-solid waste raw materials and a low-alkali activator through alkali activation-foaming curing. Different combinations of the all-solid waste raw materials are selected according to functional requirements: the heavy metal adsorption layer and flame-retardant fireproof layer use a ternary composite of coal gangue, steel slag, and aluminum slag; the structural seepage-proof sealing layer uses a binary composite of coal gangue and steel slag. Coal gangue provides the core silicon-aluminum source, forming the basis of the three-dimensional framework of the geopolymer; steel slag is rich in active calcium-silicon phase, supplementing the system with active calcium source, participating in the formation of aluminosilicate gel, and providing a strongly alkaline environment to stimulate the dissolution and polymerization of the active silicon-aluminum phase in the raw coal gangue, while simultaneously generating calcium-containing hydration products to enhance the framework structure; aluminum slag is rich in active alumina and metallic aluminum, supplementing the system's aluminum source and precisely controlling the silicon-aluminum ratio. Metallic aluminum can react with the alkaline system to release H2, achieving mild foaming and completing the dual function of aluminum source supply and foaming pore creation. Modified water glass is used as the low-alkali activator.

[0019] The core of this invention lies in the alkaline activation system using coal gangue, steel slag, and aluminum slag as the main solid waste raw materials. Based on the treatment needs of different spatial locations in the gangue pile, the composition of the raw materials, solid-to-water ratio, calcium-to-silicon ratio, silicon-to-aluminum ratio, water glass modulus, and foam stabilizer dosage are grouped and matched to form differentiated structures suitable for heavy metal adsorption, flame retardancy, and structural seepage prevention and sealing. The key problem solved in the improvement process of this invention is not simply improving a single performance, but rather coordinating the interrelationships between porosity, specific surface area, gel formation, water retention capacity, structural strength, and permeability. Experimental results show that changing only a single parameter is insufficient to obtain a material structure that matches the target function; it is necessary to simultaneously consider the matching relationship between the raw material composition and the solid-to-water ratio, calcium-to-silicon ratio, silicon-to-aluminum ratio, water glass modulus, and foam stabilizer dosage. In this process, metallic aluminum in the aluminum slag participates in gas generation and pore formation under alkaline conditions, while SDS stabilizes the formed bubbles. The solid-to-water ratio affects slurry fluidity, pore formation, and particle packing. The calcium-to-silicon ratio and the silica-to-alumina ratio jointly influence the composition and network structure of calcium-containing gels and aluminosilicate gels. The water glass modulus further affects the dissolution and condensation processes of the silica-alumina phase. Therefore, the above parameters are not independent of each other. This invention combines and regulates the parameters according to the different requirements of different functional layers for the pore-gel structure, rather than simply superimposing the individual effects of each parameter.

[0020] The coordinated regulation mechanism of the five core parameters is as follows: a. Solid-to-water ratio: The solid-to-water ratio is the ratio of the mass of solid raw material to the mass of added deionized water. It mainly regulates the porosity of the system and the content of the reaction medium. A low solid-to-water ratio (1.25) corresponds to a higher amount of added water, which is beneficial to improving the fluidity of the slurry and providing space for gas generation and pore formation; a medium solid-to-water ratio (1.75) is beneficial to coordinating the fluidity of the slurry, gel formation and pore structure; a high solid-to-water ratio (1.9~2.1) corresponds to a lower amount of added water, which is beneficial to reducing the pores formed by free water migration and evaporation during the hardening process and improving the density of the material structure.

[0021] b. Calcium-silicon ratio: mainly regulates the type and quantity of hydration products. Low calcium-silicon ratio (0.8~1.0) promotes the formation of silicon-aluminum active groups; medium calcium-silicon ratio (1.2~1.4) promotes the formation of a large amount of CASH gel; high calcium-silicon ratio (1.6~1.8) promotes the formation of a large amount of calcium-containing crystalline phases such as CSH and Ca(OH)2, significantly improving structural strength and density.

[0022] c. Silicon-to-aluminum ratio: mainly regulates the gel network structure and the number of active sites. A high silicon-to-aluminum ratio (3.2~3.5) provides more Si-OH and Al-OH active adsorption sites; a medium silicon-to-aluminum ratio (2.8~3.0) forms a continuous and dense three-dimensional gel network; no aluminum slag or foam stabilizer is added to the sealing layer to avoid the adverse effects of aluminum slag gas generation and pore formation on the formation of a dense structure.

[0023] d. Water glass modulus: mainly regulates the alkalinity and reaction kinetics of the system. Low modulus (1.6~1.7) water glass is more alkaline, which is conducive to the rapid depolymerization of the silicon-aluminum phase and increases the concentration of active groups; medium modulus (1.8) water glass is conducive to coordinating the depolymerization and condensation processes and promoting the formation of gel structure; high modulus (1.9~2.0) water glass has strong condensation ability, which is conducive to improving the early strength and density of the material.

[0024] e. Foam stabilizer dosage: mainly controls the stability and pore uniformity of the foaming system. The adsorption layer uses a higher dosage (0.8%~1.2%) to form a uniformly connected mesoporous-macroporous composite structure; the flame retardant layer uses a medium dosage (0.5%~0.8%) to form a uniformly distributed micro-closed-pore structure; the sealing layer does not add aluminum slag or foam stabilizer to avoid the adverse effects of aluminum slag gas generation and foam stabilization on the formation of a dense structure.

[0025] Furthermore, higher or lower parameters are not necessarily more advantageous; rather, there exists a suitable matching range corresponding to the target function. For the heavy metal adsorption layer, an appropriate amount of aluminum slag participates in gas generation and pore formation under alkaline conditions, and works in conjunction with the foam stabilization effect of SDS, which is beneficial for forming a porous structure with a large specific surface area and mass transfer channels. When the foam stabilizer is insufficient, the bubbles formed by gas generation are prone to coalescence or escape, resulting in insufficient formation of effective pore structures. As the amount of foam stabilizer continues to increase to the upper part of the scope of this invention, the increase in porosity and adsorption capacity tends to be limited, while the compressive strength of the material decreases. Therefore, a balance needs to be struck between pore formation, specific surface area, and structural strength. For the structural seepage prevention and sealing layer, the pores formed by aluminum slag gas generation are not conducive to the formation of a dense seepage prevention structure. Therefore, this invention eliminates aluminum slag and foam stabilizer in this functional layer and increases the proportion of steel slag, calcium-silicon ratio, solid-water ratio, and water glass modulus. When the steel slag content is too low, insufficient calcium-containing gel formation occurs, resulting in poor structural density. When the steel slag content is too high, the silicon source in the system is relatively insufficient, which may cause an imbalance in the matching of reaction components, leading to a decrease in material strength and an increase in the permeability coefficient. Therefore, this invention determines the composition of each functional layer by using parameter ranges rather than single extreme values.

[0026] Existing experimental data further demonstrate the aforementioned synergistic relationship: In the heavy metal adsorption system, compared to Comparative Example 1 without SDS, the porosity of Example 1 increased from 67.8% to 82.5%, and the specific surface area increased from 89.7 m². 2 / g increased to 125.3m 2 / g, Pb 2+ and Cd 2+The adsorption capacities increased from 72.4 mg / g and 28.6 mg / g to 98.5 mg / g and 39.2 mg / g, respectively. However, Comparative Example 3, which only adjusted the solid-to-water ratio, showed significantly lower porosity, specific surface area, and heavy metal adsorption capacity compared to Example 1. Comparative Example 4 increased the aluminum slag content to 30% (exceeding the upper limit of the 0-20% range for aluminum slag in the adsorption layer of this invention). Although the porosity increased to 84.6%, excessive gas production led to pore structure deterioration, and the specific surface area decreased to 60.8 m². 2 / g, Pb 2+ Cd 2+ The adsorption capacities decreased to 51.6 mg / g and 19.8 mg / g, respectively, indicating that a higher aluminum slag content in the adsorption layer is not necessarily better. These results demonstrate that the gas production from aluminum slag, SDS foam stabilization, and the matching of raw material composition and other parameters collectively affect the pore structure and adsorption performance of the adsorption layer. In the structural seepage-proof sealing system, Example 3, which removed aluminum slag without adding a foam stabilizer, exhibited a 28-day compressive strength of 9.2 MPa and a permeability coefficient of 2.1 × 10⁻⁶. -9 cm / s; Comparative Example 2: In a similar system, the addition of 15% aluminum slag reduced the compressive strength to 7.5 MPa and increased the permeability coefficient to 4.8 × 10⁻⁶. -9 The cm / s indicates that for the sealing layer, suppressing foaming and combining it with a higher calcium-silicon ratio, a higher solid-water ratio, and a higher modulus water glass are beneficial for forming a dense structure. Examples 3-5 further show that the performance is significantly improved when the steel slag content is increased from 40% to 45%, while the compressive strength decreases and the permeability coefficient slightly increases after further increasing it to 50%, indicating that there is a suitable matching range between the steel slag content and the calcium-silicon ratio.

[0027] This invention also discloses a method for preparing the aforementioned multi-solid-waste synergistic alkali-activated functional gradient material, comprising the following steps: a. Preparation of low-alkali activator: Weigh sodium hydroxide and add it to water glass, stir until completely dissolved, let stand to eliminate bubbles, and obtain low-alkali activator, seal and use for later use; b. Raw material pretreatment: The coal gangue, steel slag, and aluminum slag are crushed, ground, and passed through a 150-250 mesh sieve. They are then dried at 100-110℃ for 10-15 hours to remove free moisture, and the pretreated raw materials are sealed for later use. c. Functional proportioning and batching: Weigh the pretreated raw materials and mix them in a mixer for 10-30 minutes to obtain a mixed powder of all solid waste. d. Slurry preparation: Based on the mass of the solid waste mixed powder, take the modified water glass solution obtained in step a, add deionized water, and stir at 300-400 r / min for 0.5-2 min to obtain an activator dispersion; add the solid mixed powder, and continue stirring at 300-400 r / min for 1-10 min to obtain a uniform geopolymer slurry; e. Curing and solidification: Pour the uniform geopolymer slurry to the target location and allow it to cure naturally for 20-30 hours to complete the initial setting and structural shaping. Continue curing until the design strength is reached.

[0028] In one preferred embodiment, the preparation method of the heavy metal adsorption layer and the flame-retardant fireproof layer further includes a foam stabilizing and mixing step: based on the mass of the solid mixed powder, a foam stabilizer is added to the slurry obtained in step d, and stirred at a speed of 300-400 r / min for 0.5-2 min to achieve uniform dispersion of the foam stabilizer, followed by curing.

[0029] The present invention also discloses a comprehensive treatment method for layered backfilling of coal gangue piles, which uses the aforementioned materials and performs layered backfilling from bottom to top according to the following structure: a base heavy metal adsorption layer, a first coal gangue compaction layer, a flame-retardant and fireproof layer, a second coal gangue compaction layer, and a structural seepage prevention and sealing layer.

[0030] The top structure seepage-proof sealing layer is used to reduce the infiltration of rainwater into the gangue pile. The middle flame-retardant and fireproof layer is set between the upper and lower coal gangue compaction layers to improve the high-temperature water retention capacity inside the pile and form a flame-retardant isolation. The base heavy metal adsorption layer is used to adsorb and retain heavy metal ions in the seepage liquid. The functional layers and the coal gangue compaction layer together form a gradient protection system arranged along the seepage direction and the height of the pile.

[0031] In one preferred embodiment, the layered backfilling integrated treatment process specifically includes the following steps: The base of the waste rock pile should be cleaned and leveled, large pieces of waste rock and debris should be removed, and the compaction degree of the base should be ≥90%. Pour a heavy metal adsorption layer with a thickness of 1~1.5m and allow it to cure naturally for 24 hours; Lay a first coal gangue compacted layer with a thickness of 5-8m, compact it in layers, and achieve a compaction degree of ≥93%; Pour a 1-1.5m thick flame-retardant and fireproof layer and allow it to cure naturally for 24 hours. A second layer of compacted coal gangue, 5-8m thick, is laid and compacted in layers, with a compaction degree ≥93%. A 1-1.5m thick structural seepage prevention and sealing layer is poured on top and allowed to cure naturally until it reaches the design strength.

[0032] The challenges of this invention: The base heavy metal adsorption layer needs to have high porosity, large specific surface area, and suitable mass transfer channels to facilitate the infiltrate's entry into the material and full contact with the adsorption sites. The middle flame-retardant and fireproof layer needs to balance high-temperature water retention capacity, thermal insulation performance, and a certain degree of structural integrity. The top structural seepage-proof sealing layer needs to minimize interconnected pores and improve material density, compressive strength, and seepage resistance. Therefore, simply increasing material porosity, while beneficial for heavy metal adsorption, may reduce material strength and seepage resistance; conversely, simply increasing material density may weaken the mass transfer and adsorption capacity of the adsorption layer. The challenge to overcome in the development of this invention is how to synergistically regulate the material composition and key parameters based on the same solid waste raw material system and the treatment needs of different spatial locations in the waste rock pile, so that the material forms differentiated pore-gel structures suitable for heavy metal adsorption, flame retardancy and fireproofing, and structural seepage-proof sealing, and further construct a mutually supportive layered treatment system.

[0033] The principle of this invention: The functionally graded materials prepared in this invention follow a continuous reaction path: alkali-activated dissolution - gel condensation nucleation - gas-induced foaming - foam stabilizer interfacial stabilization - framework coating and foam consolidation - post-curing and shaping. Alkali-activated dissolution stage: Under alkaline conditions, chemical bonds break in the silica-alumina glass phase of coal gangue, the active calcium-silicon phase of steel slag, and the active alumina and metallic aluminum phase (only the adsorption layer and flame-retardant layer) of aluminum slag. The original mineral structure rapidly depolymerizes, releasing [Si(OH)4] and [Al(OH)4]. - Ca 2+ Active monomers; Gel condensation nucleation stage: The active substances such as Si, Al, and Ca dissolved in the system reach local supersaturation, and hydroxyl dehydration condensation occurs between the active monomers to form aluminosilicate oligomers and further generate early gel nuclei; the reaction of metallic aluminum and alkali in the adsorption layer and flame retardant layer produces gas simultaneously, and SDS molecules adsorb on the surface of the bubbles through the interface to form a stable protective film, inhibiting bubble aggregation and floating. In the skeleton-encapsulated solid-foam stage (adsorption layer and flame retardant layer only): the condensation reaction becomes the dominant process, the gel system grows and matures rapidly, the degree of Si-OT (Si / Al) bond polymerization increases rapidly, the system viscosity rises sharply, the bubbles stabilized by SDS are wrapped and fixed by the continuous gel skeleton, completing the bubble-locking invention process, forming a pore structure with continuous pore walls and uniform pore distribution. In the later hardening and shaping stage: the dissolution and condensation reactions gradually slow down, the incompletely reacted intermediate structure continues to transform into a gel skeleton with a high degree of polymerization, free water gradually transforms into bound water and structural water in the gel structure, the system structure becomes denser, and finally a composite skeleton structure with amorphous aluminosilicate gel as the main body and locally calcium-containing hydrated crystal phases for reinforcement is formed.

[0034] Beneficial effects (1) Multi-parameter synergistic regulation. This invention addresses the different requirements of three functions—heavy metal adsorption, flame retardancy and fire prevention, and structural seepage prevention and sealing—on the pore structure and gel density. Based on the same coal gangue-steel slag-aluminum slag solid waste system, the composition of raw materials, solid-water ratio, calcium-silicon ratio, silicon-aluminum ratio, water glass modulus, and foam stabilizer dosage are matched in groups to achieve directional regulation from porous adsorption structure and water-retaining flame-retardant structure to dense seepage prevention structure.

[0035] (2) The raw material composition is matched with the functional structure. For the heavy metal adsorption layer and the flame retardant and fireproof layer, the aluminum metal in the aluminum slag participates in gas production in an alkaline environment, and the pore structure is controlled by the foam stabilizing effect of SDS. For the top structure seepage prevention and sealing layer, the aluminum slag and foam stabilizer are eliminated and the proportion of steel slag and the system densification parameters are increased to avoid the adverse effects of gas production and pore formation on seepage prevention performance, so that the same type of solid waste raw material can form different microstructures according to the engineering functional requirements.

[0036] (3) Forming a spatial gradient protection system. In this invention, the top structural seepage-proof sealing layer, the middle flame-retardant and fireproof layer, and the base heavy metal adsorption layer are respectively arranged at different spatial locations of the gangue pile, forming a gradient treatment structure of top source seepage reduction - middle flame-retardant isolation - base end adsorption, so that different functional materials can play their roles in positions adapted to their performance characteristics. The functional layers are not simply arranged side by side, but form a mutually cooperating gradient protection system according to the treatment needs of different spatial locations of the gangue pile: the top structural seepage-proof sealing layer is used to reduce the infiltration of precipitation into the pile body, reducing the formation of seepage liquid and the impact of the external environment on the pile body from the source; the middle flame-retardant and fireproof layer is arranged between the upper and lower coal gangue compaction layers, providing high temperature water retention and spatial isolation for the control of spontaneous combustion risk inside the pile body; the base heavy metal adsorption layer adsorbs and intercepts the heavy metal-containing leachate that is still migrating downwards. Thus, the three types of functional materials are respectively arranged in spatial locations adapted to their performance characteristics, forming a chain gradient protection system of the invention of top seepage reduction - middle flame-retardant isolation - base adsorption interception.

[0037] (4) It has good solid waste resource utilization and engineering adaptability. The present invention uses industrial solid wastes such as coal gangue, steel slag and aluminum slag as the main cementitious solid raw materials. Each functional layer can adopt similar raw material pretreatment, mixing, casting and curing processes. By adjusting the solid waste ratio and key parameters, different functional materials can be prepared, which is conducive to organizing construction in the same gangue mountain layered backfilling project. Attached Figure Description

[0038] Figure 1This is the xrd phase composition of coal gangue (CG), steel slag (SS), and cementitious material (SCG) in one embodiment of the present invention; wherein, the phases are labeled as: 1-SiO2, 2-Al2O3, 3-Ca2SiO4, 4-Ca3Si2O7, 5-Ca 0.15 Fe 0.85 O4, 6-Ca3SiO5, 7-CaO, 8-CSH gel, 9-CASH gel; Figure 2 Here are schematic diagrams of material samples prepared in one embodiment of the present invention: (a) Porous functional material of Example 1; (b) Dense functional material without aluminum slag (structural seepage prevention and sealing type); Figure 3 This is a schematic diagram of a layered backfill structure for a coal gangue pile in one embodiment of the present invention; wherein, each layer is labeled as follows: ① Base heavy metal adsorption layer (fill thickness 1~1.5m); ② First coal gangue compaction layer (thickness 5~8m); ③ Flame-retardant and fireproof layer (thickness 1~1.5m); ④ Second coal gangue compaction layer (thickness 5~8m); ⑤ Top structure seepage prevention and sealing layer (thickness 1~1.5m); ⑥ Original coal gangue pile base (cleaned, leveled and compacted). The top structure seepage prevention and sealing layer is used to reduce rainwater infiltration, the middle flame-retardant and fireproof layer is used to provide flame-retardant isolation between the upper and lower coal gangue compaction layers, and the base heavy metal adsorption layer is used to intercept heavy metals in the seepage fluid at the end. Detailed Implementation

[0039] The present invention will be further described in detail below with reference to specific embodiments. These embodiments are based on the technical solution of the present invention and provide detailed implementation methods and specific operating procedures; however, the scope of protection of the present invention is not limited to the following embodiments.

[0040] In the following embodiments and comparative examples of the present invention, the coal gangue used was taken from a coal gangue dump in Shaanxi Province, the steel slag was taken from the converter waste slag of Tangshan Iron and Steel Plant, and the aluminum slag was taken from the smelting waste slag of Borun Refractory Materials in Gongyi City (metallic aluminum mass fraction 20%). The commercially available water glass used had a modulus of 2.4. Sodium hydroxide and sodium dodecyl sulfate (SDS) were both analytical grade reagents.

[0041] Example 1 (Heavy Metal Adsorption Material) The preparation method of the heavy metal adsorption type functional gradient material in this embodiment includes the following steps: a. Preparation of low-alkali activator: Weigh 8.8g of sodium hydroxide and add it to 100g of commercially available water glass. Stir until completely dissolved, adjust the water glass modulus to 1.6, let stand for 24 hours to eliminate bubbles, and obtain a modified water glass solution. Seal and store for later use. b. Raw material pretreatment: Coal gangue, steel slag, and aluminum slag are crushed, ground, and sieved through a 200-mesh sieve, then dried in a 105℃ forced-air drying oven for 12 hours to remove free moisture, and sealed for later use; the pretreated coal gangue, steel slag, and aluminum slag are accurately weighed at a mass ratio of 60:25:15, and mixed in a mixer for 10 minutes to obtain a solid waste mixed powder with a silicon-aluminum ratio of 3.3 and a calcium-silicon ratio of 0.9. c. Slurry preparation: Weigh 20g of the solid mixed powder prepared in step b. Based on its mass, take 10% (2.0g) of the modified water glass solution obtained in step a, add 16g of deionized water, the solid-to-water ratio of the system is 1.25, place it in a beaker and stir at 350r / min for 1min to obtain an activator dispersion; add the solid mixed powder, and continue stirring at 350r / min for 5min to obtain a uniform geopolymer slurry; d. Foam stabilization and mixing: Based on 20g of solid mixed powder, add 1.0% (0.2g) of sodium dodecyl sulfate to the above slurry and stir at 350r / min for 1min to achieve uniform dispersion of the foam stabilizer; e. Curing and solidification: Pour the slurry into the mold and cure naturally for 24h to complete the initial setting and structural shaping. Continue curing for 28d to obtain a heavy metal adsorption type functional gradient material.

[0042] Example 2 (Flame-retardant and fireproof material) The only differences between this embodiment and Embodiment 1 are: in step a, the modulus of water glass is adjusted to 1.8; in step b, the ratio of coal gangue: steel slag: aluminum slag is 50:35:15 (mass ratio), the silicon-aluminum ratio of the system is 2.9, and the calcium-silicon ratio is 1.3; in step c, the modified water glass content is 11% (2.2g), 11.4g of deionized water is added, and the solid-water ratio of the system is 1.75; in step d, the foam stabilizer content is 0.6% (0.12g); the remaining raw material ratios and process parameters are the same as in Embodiment 1, resulting in a flame-retardant and fire-resistant functional graded material.

[0043] Example 3 (Structural seepage prevention and sealing material, optimal steel slag content) The only difference between this embodiment and Example 1 is that: in step a, 5.5g of sodium hydroxide is weighed and added to 100g of commercially available water glass, and the water glass modulus is adjusted to 1.9; in step b, aluminum slag is not added, and the ratio of coal gangue to steel slag is 55:45 (mass ratio), the system silicon-aluminum ratio is 3.1, and the calcium-silicon ratio is 1.7; in step c, the modified water glass content is 12% (2.4g), and 10.0g of deionized water is added, and the system solid-water ratio is 2.0; the foam stabilization and mixing process in step d is omitted; the remaining raw material ratios and process parameters are the same as in Example 1, resulting in a structural seepage-proof and sealing functional gradient material.

[0044] Example 4 (40% steel slag admixture in the sealing layer) The only difference between this embodiment and Embodiment 3 is that in step b, the ratio of coal gangue to steel slag is 60:40 (mass ratio), and the calcium-silicon ratio of the system is 1.5; all other process parameters are the same as in Embodiment 3.

[0045] Example 5 (50% steel slag admixture in the sealing layer) The only difference between this embodiment and Embodiment 3 is that in step b, the ratio of coal gangue to steel slag is 50:50 (by mass), and the calcium-silicon ratio of the system is 1.9; all other process parameters are the same as in Embodiment 3.

[0046] Example 6 (Dosage of high-stabilizing foaming agent in the adsorption layer) The only difference between this embodiment and Example 1 is that the amount of foam stabilizer in step d is 1.2% (0.24g); all other process parameters are the same as in Example 1.

[0047] Comparative Example 1 (Comparative Example with No Foam Stabilizer in Adsorption Layer) The only difference between this comparative example and Example 1 is that step d, the stabilizing and mixing process, is omitted; all other process parameters are the same as in Example 1.

[0048] Comparative Example 2 (Comparative Example of Sealing Layer with Aluminum Slag) The only difference between this comparative example and Example 3 is that 15% aluminum slag is added in step b, and the ratio of coal gangue:steel slag:aluminum slag = 40:45:15 (mass ratio); all other process parameters are the same as in Example 3.

[0049] Comparative Example 3 (Comparative Example of Single Solid-to-Water Ratio Adjustment) In this comparative example, the solid-to-water ratio was fixed at 1.75, and only the raw material ratio and water glass modulus were adjusted to prepare heavy metal adsorption materials. The remaining process parameters were the same as in Example 1.

[0050] Comparative Example 4 (Comparative Example with Excessive Aluminum Dross Content in the Adsorption Layer) The preparation method of this comparative example is basically the same as that of Example 1, except that the composition of the solid raw materials for the adsorption layer is adjusted. The mass ratio of coal gangue, steel slag, and aluminum slag is adjusted from 60:25:15 in Example 1 to 40:30:30, increasing the mass proportion of aluminum slag from 15% to 30%. Consequently, the silicon-aluminum ratio of the system decreases to 2.6, which exceeds the parameter range of aluminum slag mass proportion and silicon-aluminum ratio in the heavy metal adsorption material of this invention. Except for the above-mentioned solid raw material composition and the resulting change in silicon-aluminum ratio, the modified water glass modulus, solid-water ratio, foam stabilizer dosage, stirring conditions, and curing conditions are all the same as in Example 1.

[0051] Experimental Results and Analysis Comparison of basic properties of different functional materials The basic performance of each embodiment and comparative sample was tested at 28 days, and the results are shown in Table 1.

[0052] Table 1. Performance test results of different functional materials at 28 days

[0053] Test results show that the samples prepared in Examples 1-3 exhibit differentiated heavy metal adsorption, high-temperature water retention, and structural seepage prevention properties, corresponding to the functional requirements of different locations in the layered backfilling of waste rock piles. Among them, Example 1 has higher porosity, specific surface area, and Pb content. 2+ Cd 2+ Adsorption capacity; Example 2 has a high water retention rate at 12 h and 100℃, which can provide a performance basis for flame retardant and fireproof functions; Example 3 has high compressive strength and low permeability coefficient, showing good structural seepage prevention performance.

[0054] As can be seen from the results of the embodiments and comparative examples, the formation of each functional material of the present invention is not determined by a single parameter alone, but is related to the synergistic matching of raw material composition and multiple process parameters.

[0055] For heavy metal adsorption materials, the raw material composition and other process conditions of Example 1 and Comparative Example 1 are basically the same, the difference being that SDS was not added in Comparative Example 1. The porosity of Example 1 increased from 67.8% in Comparative Example 1 to 82.5%, and the specific surface area increased from 89.7 m². 2 / g increased to 125.3 m 2 / g, Pb 2+ The adsorption capacity increased from 72.4 mg / g to 98.5 mg / g, Cd 2+The adsorption capacity increased from 28.6 mg / g to 39.2 mg / g. The results indicate that in the alkaline-activated system containing aluminum slag, the combination of the SDS foam stabilization process and the aluminum slag gas generation and pore-forming process is beneficial for increasing the effective porosity and specific surface area, thereby improving the heavy metal adsorption performance. Compared with Comparative Example 3, which only underwent single solid-water ratio control, Example 1 showed improved adsorption capacity for Pb. 2+ The adsorption capacity increased from 58.6 mg / g to 98.5 mg / g, Cd 2+ The adsorption capacity increased from 22.4 mg / g to 39.2 mg / g, indicating that relying solely on the adjustment of the solid-water ratio is insufficient to obtain the adsorption-type pore structure required by this invention. It is necessary to combine and match the raw material composition, solid-water ratio, silicon-aluminum ratio, calcium-silicon ratio, water glass modulus, and foam stabilizer dosage.

[0056] For structural seepage-proof sealing materials, compared with Comparative Example 2, Example 3, by eliminating aluminum slag, avoided the adverse effects of aluminum gas generation and pore formation on the dense structure. The material's 28-day compressive strength increased from 7.5 MPa to 9.2 MPa, and the permeability coefficient increased from 4.8 × 10⁻⁶ MPa. -9 cm / s decreased to 2.1 × 10 -9 cm / s. This result further illustrates that the same component produces different effects in different functional layers. The present invention selects whether to introduce aluminum slag and foam stabilizer according to the target structure of different functional layers, rather than mechanically preparing three types of materials using the same raw material composition.

[0057] The results of Comparative Example 4 further demonstrate that a higher porosity in the adsorption layer material is not necessarily more advantageous. Compared to Example 1, Comparative Example 4, by using a higher proportion of aluminum slag and deviating the solid raw material composition and silicon-aluminum ratio from the preferred parameter range of the present invention, resulted in a further increase in material porosity from 82.5% to 84.6%, but the specific surface area decreased from 125.3 m². 2 / g decreased to 60.8 m 2 / g, Pb 2+ The adsorption capacity decreased from 98.5 mg / g to 51.6 mg / g, Cd 2+ The adsorption capacity decreased from 39.2 mg / g to 19.8 mg / g. These results indicate that simply increasing the gas-producing components and improving the total porosity of the material does not guarantee a simultaneous improvement in adsorption performance. A higher proportion of aluminum slag, and the resulting changes in the silica-alumina ratio, gas production process, and pore structure, affect the formation of effective adsorption pore structures. Therefore, it is necessary to synergistically control the composition of coal gangue, steel slag, and aluminum slag, as well as the foam stabilization conditions, to ensure that the material maintains a large effective specific surface area and heavy metal adsorption capacity while achieving a high porosity.

[0058] Effect of different steel slag contents on the performance of the sealing layer To optimize the steel slag content of the sealing layer, the key performance of Examples 3-5 under different steel slag contents was tested for 28 days, and the results are shown in Table 2.

[0059] Table 2. Comparison of sealing layer performance after 28 days with different steel slag admixtures

[0060] Test results show that as the steel slag content increases from 40% to 45%, the porosity of the sealing layer decreases from 17.3% to 15.1%, the compressive strength increases from 7.1 MPa to 9.2 MPa, and the permeability coefficient increases from 6.7 × 10⁻⁶. -9 cm / s decreased to 2.1 × 10 -9 The performance was continuously optimized with a speed of cm / s. When the steel slag content exceeded 45%, the hydration reaction was incomplete due to the relative insufficiency of silicon source in the system, resulting in a decrease in compressive strength and a slight increase in permeability coefficient. Therefore, under the experimental conditions and within the range of steel slag content investigated, a steel slag content of 45% (coal gangue: steel slag = 55:45) showed superior comprehensive performance.

Claims

1. A multi-solid-waste synergistic alkali-activated functional gradient material, characterized in that: The material includes a heavy metal adsorption material comprising coal gangue, steel slag, aluminum slag, a low-alkali activator, a foam stabilizer, and water. A slurry is prepared by stirring and then solidified to form a heavy metal adsorption layer. The porosity of the heavy metal adsorption layer is 70-90%, and the specific surface area is 110-130 m². 2 / g, Pb 2 + The adsorption capacity is 90-100 mg / g, Cd 2+ The adsorption capacity is 30-40 mg / g; preferably, the porosity of the heavy metal adsorption layer is 80-85%, and the specific surface area is 125-130 m². 2 / g, Pb 2+ The adsorption capacity is 95-100 mg / g, Cd 2+ The adsorption capacity is 35-40 mg / g.

2. The multi-solid waste synergistic alkali-activated functional gradient material according to claim 1, characterized in that: In the aforementioned heavy metal adsorbent material, the mass ratio of coal gangue, steel slag, and aluminum slag is 40~70:20~50:1~20, the silicon-aluminum ratio is 3.2~3.5, the calcium-silicon ratio is 0.8~1.0, the solid-water ratio is 1.2~1.3, the water glass modulus is 1.6~1.7, and the foam stabilizer dosage is 0.8%~1.2%; preferably, the mass ratio of coal gangue, steel slag, and aluminum slag is 60~70:20~25:15~20.

3. The multi-solid waste synergistic alkali-activated functional gradient material according to claim 1 or 2, characterized in that: It also includes flame-retardant and fire-resistant materials, which consist of coal gangue, steel slag, aluminum slag, low-alkali activator, foam stabilizer, and water. These materials are mixed to form a slurry, which is then cured to form a flame-retardant and fire-resistant layer. The porosity of this layer is 20-30%, and its specific surface area is 60-70 m². 2 / g, Pb 2+ The adsorption capacity is 40-50 mg / g, Cd 2+ The adsorption capacity is 10-20 mg / g.

4. The multi-solid waste synergistic alkali-activated functional gradient material according to claim 3, characterized in that: In the flame-retardant and fireproof material, the mass ratio of coal gangue, steel slag and aluminum slag is 45-55:30-40:10-20, the silicon-aluminum ratio is 2.8-3.0, the calcium-silicon ratio is 1.2-1.4, the solid-water ratio is 1.7-1.8, the water glass modulus is 1.8, and the foam stabilizer dosage is 0.5%-0.8%; preferably, the flame-retardant and fireproof layer is disposed on the upper side of the heavy metal adsorption layer.

5. The multi-solid waste synergistic alkali-activated functional gradient material according to claim 3 or 4, characterized in that: It also includes structural seepage-proof sealing materials, which consist of coal gangue, steel slag, a low-alkali activator, and water. These materials are mixed to form a slurry, which is then cured to form the structural seepage-proof sealing layer. The porosity of the structural seepage-proof sealing layer is 10-20%, and its specific surface area is 20-30 m². 2 / g, Pb 2+ The adsorption capacity is 10-20 mg / g, Cd 2+ The adsorption capacity is 5-10 mg / g.

6. The multi-solid waste synergistic alkali-activated functional gradient material according to claim 5, characterized in that: In the structural seepage-proof sealing material, the mass ratio of coal gangue to steel slag is 50-60:40-50, the silicon-aluminum ratio is 3.0-3.2, the calcium-silicon ratio is 1.6-1.8, the solid-water ratio is 1.9-2.1, and the water glass modulus is 1.9-2.0; preferably, the structural seepage-proof sealing layer is disposed on the upper side of the flame-retardant and fireproof layer.

7. A method for preparing a multi-solid waste synergistic alkali-activated functional gradient material as described in any one of claims 1-6, characterized in that, Includes the following steps: a. Preparation of low-alkali activator: Weigh sodium hydroxide and add it to water glass, stir until completely dissolved, let stand to eliminate bubbles, and obtain low-alkali activator, seal and use for later use; b. Raw material pretreatment: The coal gangue, steel slag, and aluminum slag are crushed, ground, and passed through a 150-250 mesh sieve. They are then dried at 100-110℃ for 10-15 hours to remove free moisture, and the pretreated raw materials are sealed for later use. c. Functional proportioning and batching: Weigh the pretreated raw materials and mix them in a mixer for 10-30 minutes to obtain a mixed powder of all solid waste. d. Slurry preparation: Based on the mass of the mixed powder of all solid waste, take the modified water glass solution obtained in step a, add deionized water, and stir at a speed of 300-400 r / min for 0.5-2 min to obtain the activator dispersion; Add solid mixed powder and continue stirring at 300-400 r / min for 1-10 min to obtain a uniform geopolymer slurry; e. Curing and solidification: Pour the uniform geopolymer slurry to the target location and allow it to cure naturally for 20-30 hours to complete the initial setting and structural shaping. Continue curing until the design strength is reached.

8. The method according to claim 7, characterized in that, The preparation method of the heavy metal adsorption layer and the flame retardant and fireproof layer also includes a foam stabilizing and mixing step: based on the mass of the solid mixed powder, a foam stabilizer is added to the slurry obtained in step d, and stirred at a speed of 300-400 r / min for 0.5-2 min to achieve uniform dispersion of the foam stabilizer, followed by curing.

9. A comprehensive treatment method for layered backfilling of waste rock piles, characterized in that: Using the material as described in claim 5 or 6, backfilling is carried out in layers from bottom to top according to the following structure: base heavy metal adsorption layer, first coal gangue compaction layer, flame retardant and fireproof layer, second coal gangue compaction layer, and structural seepage prevention and sealing layer. The top structure seepage-proof sealing layer is used to reduce the infiltration of rainwater into the gangue pile. The middle flame-retardant and fireproof layer is set between the upper and lower coal gangue compaction layers to improve the high-temperature water retention capacity inside the pile and form a flame-retardant isolation. The base heavy metal adsorption layer is used to adsorb and retain heavy metal ions in the seepage liquid. The functional layers and the coal gangue compaction layer together form a gradient protection system arranged along the seepage direction and the height of the pile.

10. The method according to claim 9, characterized in that, The layered backfilling comprehensive treatment process specifically includes the following steps: The base of the waste rock pile should be cleaned and leveled, large pieces of waste rock and debris should be removed, and the compaction degree of the base should be ≥90%. Pour a heavy metal adsorption layer with a thickness of 1~1.5m and allow it to cure naturally for 24 hours; Lay a first coal gangue compacted layer with a thickness of 5-8m, compact it in layers, and achieve a compaction degree of ≥93%; Pour a 1-1.5m thick flame-retardant and fireproof layer and allow it to cure naturally for 24 hours. A second layer of compacted coal gangue, 5-8m thick, is laid and compacted in layers, with a compaction degree ≥93%. A 1-1.5m thick structural seepage prevention and sealing layer is poured on top and allowed to cure naturally until it reaches the design strength.