A nano-CO2 bubble water filling material and its preparation method
By introducing nano-CO2 bubble water, rheology modifiers, and targeted activating additives into the filling material of coal mine goaf, the difficulties in rheological control and stability of existing materials under high-concentration pulping and transportation conditions have been solved, thereby improving the fluidity and structural stability of the slurry and promoting the resource utilization of solid waste and low-carbon development.
Patent Information
- Application Number
- CN202610981785.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-02
- Publication Date
- 2026-11-17
AI Technical Summary
Existing coal mine goaf filling materials suffer from problems such as difficulty in rheological control, insufficient stability of particle systems, easy bleeding and segregation, difficulty in balancing early structure establishment and later filling stability, and low degree of solid waste resource utilization and CO2 synergistic utilization under high-concentration slurry preparation and transportation conditions.
The composite gelling system is introduced in the form of nano-CO2 bubble water, combined with rheology modifiers and targeted activating additives to regulate the interaction between particles, ion balance and structure establishment rate, promote the formation of nano-calcium carbonate, and improve the fluidity, flow retention and anti-segregation ability of the slurry.
It achieves a unified improvement in the fluidity, stability, and early structure building capabilities of the filling slurry, while taking into account the needs of high-value utilization of multi-source solid waste and low-carbon preparation, and improves the continuity, uniformity, and safety of the goaf filling process.
Smart Images

Figure CN123106136A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of high-value utilization of solid waste and mine backfilling and reinforcement technology, specifically involving a nano CO2 bubble water backfill material and its preparation method. Background Technology
[0002] During coal mining, as coal resources are continuously extracted, the area of underground goafs expands, easily triggering a series of geological and engineering problems such as overburden movement, surface subsidence, and roadway instability. In severe cases, these problems can even affect mine safety and the stability of surface structures. Therefore, using backfilling technology to treat goafs is an important means to control stratum deformation, improve resource recovery rates, and ensure safe and green coal mining. Compared with traditional caving methods, goaf backfilling technology has advantages such as mitigating surface subsidence, improving the stress state of surrounding rock, reducing environmental disturbance, and promoting the resource utilization of solid waste, and has become an important development direction for modern green coal mining.
[0003] Existing coal mine goaf backfill materials are mainly composed of cement, fly ash, slag, and coal gangue, which are prepared as high-concentration slurries and transported to the goaf for backfilling. However, goaf backfilling conditions place high demands on material performance: on the one hand, the slurry should possess good fluidity, pumpability, and flow retention capacity during preparation and transportation to meet the needs of high-concentration, long-distance transportation; on the other hand, after entering the goaf, the slurry should have good resistance to bleeding and segregation, particle system stability, and rapid early structure building ability to ensure uniformity, compactness, and later-stage stability during the backfilling process. Existing backfill material systems often struggle to simultaneously meet these multiple requirements, frequently exhibiting problems such as narrow rheological control windows, easy bleeding and segregation of the slurry, significant particle settling, and insufficient early structure building, thus limiting their engineering application effectiveness under complex goaf conditions.
[0004] Meanwhile, industrial solid wastes such as steel slag, blast furnace slag, fluorogypsum, and coal gangue are produced in large quantities, face high storage pressure, and impose a heavy environmental burden. Utilizing these wastes for high-value applications in mine backfill material preparation is a crucial pathway to achieving solid waste resource utilization and low-carbon development in mining. Existing research indicates that constructing composite cementitious systems using steel slag, blast furnace slag, and gypsum-based materials has the potential to replace some traditional cementitious materials, reduce costs, and improve resource utilization. However, multi-source solid waste systems are complex in composition and diverse in reaction pathways, often accompanied by problems such as insufficient activity, unstable particle interface behavior, and significant fluctuations in rheological properties. Especially under conditions of high solid phase concentration and complex ionic environments, the system's fluidity maintenance, structural evolution, and early stability become even more difficult to precisely control.
[0005] Furthermore, with the continuous advancement of the "dual carbon" goal, the resource utilization of CO2 has gradually become an important research direction in the field of cementitious materials. Existing research shows that CO2 participation in the reaction of cementitious systems helps induce the formation of carbonate phases and plays a regulatory role in the early structural evolution of the system. However, the direct introduction of CO2 often suffers from problems such as low mass transfer efficiency, poor dispersion uniformity, and difficulty in precisely controlling the reaction process. It can also easily cause excessively rapid local carbonation, a sudden increase in slurry viscosity, enhanced particle flocculation, and decreased flow retention, which is not conducive to the stable preparation and transportation of high-concentration filling slurries. At the same time, when CO2 is directly introduced, its nucleation process and the reaction efficiency of generating nano-calcium carbonate are difficult to fully realize, limiting the synergistic effect of CO2 in the filling material system. To address the above problems, this invention proposes a method for introducing CO2 into the filling system in the form of nano-bubble water. Compared with the direct introduction of CO2, this method can improve the dispersibility and stability of CO2 in the liquid phase and provide a milder and more controllable reaction environment for its participation in the early nucleation reaction of the slurry. Based on this, the present invention further alleviates the rheological instability problem that may occur after the introduction of CO2 bubble water by introducing a rheology regulator; and improves the CO2 nucleation rate and the reaction utilization efficiency of nano-calcium carbonate by introducing a targeted activating admixture, thereby achieving a synergistic improvement in slurry fluidity, structural stability and early reaction activity. Summary of the Invention
[0006] This invention aims to address the challenges of rheological control, insufficient particle system stability, easy bleeding and segregation, and difficulty in balancing early structure establishment and later filling stability in existing coal mine goaf backfill materials under high-concentration slurry preparation and transportation conditions, as well as the low degree of solid waste resource utilization and CO2 synergistic utilization. It proposes a method for preparing CO2 bubble water backfill material for coal mine goafs. This method constructs a composite cementitious system using steel slag powder, slag powder, and fluorogypsum. CO2 is introduced into the slurry in the form of nano-bubble water, utilizing its nucleation effect to promote the formation of nano-calcium carbonate and regulate the early reactions and microstructure evolution of the system. To address the problems of accelerated viscosity increase, enhanced flocculation, and decreased flowability after the introduction of nano-CO2 bubble water, this invention further introduces a rheology modifier composed of calcium lactate and potassium sodium tartrate to regulate interparticle interactions, ion balance, and structure establishment rate, thereby improving the slurry's fluidity, flowability, and anti-segregation ability. Building upon this foundation, a targeted activating additive composed of N,N,N',N'-tetrahydroxyethylethylenediamine and nitrilotriacetic acid was introduced to enhance the dissolution and migration of active components, increase the CO2 nucleation rate, and promote the efficient reaction utilization of nano-calcium carbonate and the formation of gelling products. This resulted in a unified improvement in the fluidity, stability, and early structure-building ability of the filling slurry, while simultaneously meeting the needs for high-value utilization of multi-source solid waste and low-carbon preparation.
[0007] The objective of this invention can be achieved through the following technical solutions:
[0008] A method for preparing a nano-CO2 bubble water filling material includes the following steps:
[0009] (1) Steel slag powder, slag powder, fluorogypsum, rheology modifier and targeted activator are added to a ball mill for grinding and premixing to obtain a uniformly mixed composite powder material;
[0010] (2) Add nano CO2 bubble water and continuously graded coal gangue aggregate to the composite powder material obtained in step (1). First, stir for 1 to 5 minutes at a stirring speed of 200 to 300 r / min, and then continue stirring for 1 to 5 minutes at a stirring speed of 400 to 600 r / min to obtain CO2 bubble water filling slurry for filling coal mine goaf.
[0011] In the technical solution of this invention, the steel slag powder is a by-product of steelmaking in an alkaline oxidation furnace, and after grinding, its specific surface area is 350-450 m². 2 / kg; the slag powder is granulated blast furnace slag, a by-product of blast furnace ironmaking, which, after grinding, has a specific surface area of 550–650 m². 2 / kg; the fluorinated gypsum is a by-product of fluorine-containing industrial processes, and after grinding, its specific surface area is 400-500 m² / kg. 2 / kg.
[0012] In the technical solution of the present invention, the coal gangue aggregate is a continuous graded aggregate obtained by crushing and screening coal gangue, and its particle size range is 0.05 to 5 mm.
[0013] In the technical solution of this invention, the components and dosages in the composite powder material are as follows:
[0014] 5-20 parts by weight of steel slag powder;
[0015] 60-90 parts by weight of slag powder;
[0016] 5-20 parts by weight of fluorinated gypsum;
[0017] Rheology modifier 0.01~5 parts by weight;
[0018] Targeted activating admixture 0.01~2 parts by weight;
[0019] Preferred:
[0020] 5-15 parts by weight of steel slag powder;
[0021] 70-90 parts by weight of slag powder;
[0022] 5-15 parts by weight of fluorinated gypsum;
[0023] Rheology modifier 0.01~1 parts by weight;
[0024] Targeted activating admixture 0.01~0.1 parts by weight.
[0025] In the technical solution of the present invention, the rheology modifier is composed of calcium lactate and potassium sodium tartrate, and the mass ratio of calcium lactate to potassium sodium tartrate is 0.01~3:0.01~2; preferably, the mass ratio of calcium lactate to potassium sodium tartrate is 0.1~2:0.01~0.1.
[0026] In the technical solution of this invention, the targeted activating admixture is composed of N,N,N',N'-tetrahydroxyethylethylenediamine and aminotriacetic acid, and the mass ratio of N,N,N',N'-tetrahydroxyethylethylenediamine to aminotriacetic acid is 0.01~1:0.01~0.5.
[0027] In the technical solution of this invention, the mass ratio of composite powder material to nano CO2 bubble water is 1~3:1~3, and the mass concentration of CO2 in the nano CO2 bubble water is 0.01%~2.0%; the mass ratio of composite powder material to coal gangue aggregate is 1:2~3.
[0028] A nano-CO2 bubble water filling material, wherein the filling material is prepared by the above-described preparation method.
[0029] In the technical solution of this invention, the nano-CO2 bubble water filling material is applied in the field of mine filling and reinforcement.
[0030] The beneficial effects of this invention are as follows:
[0031] (1) This invention innovatively introduces CO2 into the coal mine goaf filling system in the form of nanobubble water. Compared with traditional mixing water, nanoscale CO2 bubbles not only improve the dispersibility and retention capacity of CO2 in the liquid phase, but also promote the growth of Ca in the local microenvironment. 2+ Rapid coupling reactions with carbonate species induce preferential nucleation and precipitation of nano-calcium carbonate. The generated nano-calcium carbonate can serve as a highly active heterogeneous nucleation site, effectively reducing the nucleation barrier for the precipitation of cementitious products, promoting the directional evolution of the early microstructure of the system, and thus benefiting the early structural construction and strength development of the filling slurry.
[0032] (2) Based on this, the present invention further introduces a rheology modifier composed of calcium lactate and sodium potassium tartrate to precisely regulate the rheological behavior of the slurry after the introduction of CO2 bubble water. After the introduction of CO2, the surface charge distribution, ion migration behavior, and local flocculation state of particles in the slurry are more prone to change, usually manifested as accelerated viscosity growth, intensified particle agglomeration, decreased flow retention, and insufficient static stability. The rheology modifier used in the present invention can regulate the calcium lactate and sodium potassium tartrate to regulate the rheological behavior of the slurry.2+ By balancing release and complexation, optimizing the adsorption state on particle surfaces, and delaying the sudden establishment of non-uniform structures, the system effectively alleviates early abnormal thickening and local flocculation problems in slurries, enabling the slurry to maintain good fluidity under shear stress and possess strong structure retention capabilities under static conditions. This significantly improves the slurry's fluidity retention, resistance to bleeding and segregation, and transport stability, better meeting the engineering requirements for high-concentration, long-distance transport and uniform filling in coal mine goaf areas.
[0033] (3) Based on rheological regulation, this invention further introduces a targeted activating admixture composed of N,N,N',N'-tetrahydroxyethylethylenediamine and nitrilotriacetic acid to further enhance the CO2 nucleation process and the utilization efficiency of nano-calcium carbonate reaction. The targeted activating admixture can enhance the dissolution, migration and interfacial reaction processes of active calcium source and potential active aluminum-silicon components in the system, and increase the reaction rate of CO2 participating in the initial nucleation. At the same time, the targeted activating admixture can also promote the coupling between nano-calcium carbonate and subsequent gelation reaction, so that it can give full play to the heterogeneous nucleation, interfacial regulation and microstructure refinement, thereby accelerating the formation of gelation products, promoting early skeleton network overlap, and improving the structural integrity and stability of the filled slurry after hardening.
[0034] (4) Based on the above synergistic effects, the CO2 bubble water filling slurry prepared by this invention has good fluidity, flow retention, structural stability, and filling adaptability. It can effectively reduce the risks of bleeding, settling, and uneven filling of high-concentration filling slurry during transportation and stacking, and improve the continuity, uniformity, and safety of the goaf filling process. At the same time, this invention makes full use of various industrial solid wastes such as steel slag, slag, fluorogypsum, and coal gangue, realizing the synergistic high-value utilization of multi-source solid waste in mine filling materials; and by introducing CO2 into the filling system in the form of nano-bubble water, it expands the application of CO2 in cementing materials and mine filling fields. Therefore, this invention has significant engineering application value, resource and environmental benefits, and low-carbon value. Attached Figure Description
[0035] Figure 1 Mechanical properties of CO2 bubble water filling slurry. Detailed Implementation
[0036] To further illustrate the technical means and effects of this invention, the following description, in conjunction with embodiments and accompanying drawings, provides a further explanation of the invention. It is understood that the specific embodiments described herein are merely illustrative of the invention and not intended to limit it.
[0037] All powders used in the embodiments and comparative examples are materials whose specific surface areas were obtained by grinding.
[0038] The coal gangue aggregate is a continuously graded aggregate obtained by crushing and screening coal gangue, with a particle size range of 0.05 to 5 mm.
[0039] Example 1
[0040] (1) Weigh out the specific surface area of 450 m² according to the mass fraction. 2 10 parts by weight of steel slag powder per kg, with a specific surface area of 650 m² 2 / kg of slag powder, 80 parts by weight, with a specific surface area of 500 m² 2 10 parts by weight of fluorogypsum, 0.5 parts by weight of calcium lactate, 0.01 parts by weight of potassium sodium tartrate, 0.05 parts by weight of N,N,N',N'-tetrahydroxyethylethylenediamine, and 0.01 parts by weight of nitric acid triacetic acid were added to a ball mill for grinding and premixing. The ball milling time was 10 min, resulting in 100 parts by weight of a uniformly mixed composite powder material.
[0041] (2) Add 100 parts by mass of nano CO2 bubble water with a CO2 concentration of 0.5% and 250 parts by mass of continuously graded coal gangue aggregate to the composite powder material obtained in step (1). First, stir for 2 minutes at a stirring speed of 250 r / min, and then continue stirring for 2 minutes at a stirring speed of 500 r / min to obtain CO2 bubble water filling slurry for filling coal mine goaf.
[0042] Example 2
[0043] The raw materials and testing methods used in this embodiment are the same as those in Example 1.
[0044] The steps for preparing CO2 bubble water filling slurry in this embodiment differ from those in Example 1 in that, in step (1), 15 parts by weight of steel slag powder, 70 parts by weight of slag powder, and 15 parts by weight of fluorogypsum are weighed.
[0045] Example 3
[0046] The raw materials and testing methods used in this embodiment are the same as those in Example 1.
[0047] The steps for preparing CO2 bubble water filling slurry in this embodiment differ from those in Example 1 in that, in step (1), the amount of calcium lactate is 1.0 parts by mass and the amount of potassium sodium tartrate is 0.05 parts by mass.
[0048] Example 4
[0049] The raw materials and testing methods used in this embodiment are the same as those in Example 3.
[0050] The difference between the steps for preparing the CO2 bubble water filling slurry in this embodiment and those in Example 3 is that, in step (1), the specific surface area of the steel slag powder is 450 m². 2 / kg, the specific surface area of slag powder is 550 m² 2 / kg, the specific surface area of fluorogypsum is 400m². 2 / kg.
[0051] Example 5
[0052] The raw materials and testing methods used in this embodiment are the same as those in Example 4.
[0053] The difference between the steps for preparing CO2 bubble water filling slurry in this embodiment and those in embodiment 4 is that, in step (2), the concentration of CO2 in the nano CO2 bubble water is 1.0%.
[0054] Example 6
[0055] The raw materials and testing methods used in this embodiment are the same as those in Example 4.
[0056] The difference between the steps for preparing CO2 bubble water filling slurry in this embodiment and those in embodiment 4 is that, in step (2), the concentration of CO2 in the nano CO2 bubble water is 1.5%.
[0057] Example 7
[0058] The raw materials and testing methods used in this embodiment are the same as those in Example 4.
[0059] The difference between the steps for preparing CO2 bubble water filling slurry in this embodiment and those in embodiment 4 is that, in step (2), the concentration of CO2 in the nano CO2 bubble water is 2.0%.
[0060] Example 8
[0061] The raw materials and testing methods used in this embodiment are the same as those in Example 7.
[0062] The difference between the steps for preparing CO2 bubble water filling slurry in this embodiment and those in Example 7 is that in step (1), the amount of N,N,N',N'-tetrahydroxyethylethylenediamine is 0.10 parts by mass and the amount of nitric acid triacetic acid is 0.03 parts by mass.
[0063] Example 9
[0064] The raw materials and testing methods used in this embodiment are the same as those in Example 7.
[0065] The steps for preparing CO2 bubble water filling slurry in this embodiment differ from those in Example 7 in that, in step (1), the amount of N,N,N',N'-tetrahydroxyethyl ethylenediamine is 0.50 parts by mass and the amount of nitric acid triacetic acid is 0.20 parts by mass.
[0066] Example 10
[0067] The raw materials and testing methods used in this embodiment are the same as those in Example 9.
[0068] The steps for preparing CO2 bubble water filling slurry in this embodiment differ from those in Example 9 in that, in step (1), the amount of calcium lactate is 2.0 parts by mass and the amount of potassium sodium tartrate is 0.5 parts by mass.
[0069] Comparative Example 1
[0070] The raw materials and test methods used in this comparative example are the same as those in Example 1.
[0071] The difference between this comparative example and Example 1 is that, in step (2), nano CO2 bubble water with a CO2 concentration of 0.5% is not added, but ordinary water of equal mass is used as mixing water. The composition, amount and preparation process of the other raw materials are the same as those in Example 1.
[0072] Comparative Example 2
[0073] The raw materials and test methods used in this comparative example are the same as those in Example 1.
[0074] The difference between this comparative example and Example 1 is that N,N,N',N'-tetrahydroxyethylethylenediamine is not added in step (1).
[0075] Comparative Example 3
[0076] The raw materials and test methods used in this comparative example are the same as those in Example 1.
[0077] The difference between this comparative example and Example 1 is that nitroglycerin is not added in step (1).
[0078] Comparative Example 4
[0079] The raw materials and test methods used in this comparative example are the same as those in Example 1.
[0080] The difference between this comparative example and Example 1 is that calcium lactate is not added in step (1).
[0081] Comparative Example 5
[0082] The raw materials and test methods used in this comparative example are the same as those in Example 1.
[0083] The difference between this comparative example and Example 1 is that potassium sodium tartrate is not added in step (1).
[0084] The flowability and setting time of CO2 bubble water filling slurries prepared in some embodiments and comparative examples are shown in Table 1. The results show that the initial flowability of each embodiment is generally in the range of 255~270 mm, while that of the comparative example is 241~260 mm. This indicates that the system of the present invention can maintain good initial flowability while maintaining a high solid content, basically meeting the requirements of filling slurry for slurry preparation and pumpability. Compared with comparative example 4, the initial flowability of each embodiment is generally higher. For example, the initial flowability of Example 1 and Example 2 are 265 mm and 260 mm, respectively, which are significantly higher than the 241 mm of comparative example 4. This indicates that after the introduction of the rheology modifier, the non-uniform flocculation between slurry particles is effectively alleviated and the dispersion state of the system is improved. Similarly, when only the targeted activating admixture is added to comparative example 5, the initial flowability is only 243 mm, which is lower than that of comparative example 1, indicating that CO2 bubble water is not conducive to maintaining the initial flowability of the slurry; while when the rheology modifier and the targeted activating admixture work synergistically, they can promote the reaction while maintaining a reasonable flow window.
[0085] Regarding setting time, the initial setting time of each embodiment was 500-590 min, and the final setting time was 630-750 min; while the initial setting times of Comparative Examples 1, 2, and 4 were 640 min, 660 min, and 620 min, respectively, and the final setting times were 810 min, 820 min, and 790 min, respectively. It is evident that the system of this invention exhibits a faster structure establishment speed and a shorter hardening cycle. Specifically, Comparative Example 1 did not add CO2 bubble water, but its initial and final setting times were still significantly longer. Comparative Example 2, with only a rheology modifier added, further extended the initial and final setting times to 660 min and 820 min, respectively, indicating that in the absence of targeted activation, the rheology modifier primarily inhibits ion release and sudden structure establishment, exhibiting a certain retarding effect. Comparative Example 4, with only a targeted activation admixture added, shortened the initial setting time to 620 min, indicating that the targeted activation admixture can indeed promote early reactions and structure formation in the system; however, due to the lack of a rheology modifier, the slurry fluidity was poor, and the system's homogeneity and stability were insufficient. In comparison, the embodiments exhibited superior coagulation control effects. For example, the initial coagulation times of Examples 8 and 9 were shortened to 510 min and 500 min, respectively, and the final coagulation times were 650 min and 630 min, respectively. This indicates that at higher CO2 concentrations, the combination of appropriate amounts of rheology modifiers and higher doses of targeted activating additives can significantly improve the early reaction rate and framework construction efficiency of the system.
[0086] The mechanical properties of CO2 bubble water filling slurry prepared in some embodiments and comparative examples are as follows: Figure 1 As shown, the 7-day strength of the embodiments was 2.79–3.31 MPa, and the 28-day strength was 4.70–5.21 MPa. The embodiments of the present invention showed significantly better early and late strengths than the comparative examples. Among them, Example 9 exhibited the best overall performance, achieving a 7-day strength of 3.31 MPa and a 28-day strength of 5.21 MPa, indicating that under conditions of higher CO2 concentration and higher targeted activation additive dosage, the CO2 nucleation effect and the utilization efficiency of nano-calcium carbonate were more fully utilized, promoting the formation of gelation products and the hardening framework. Compared to Example 7, Examples 8 and 9 showed significantly improved 7-day and 28-day strengths, further demonstrating that the targeted activation additive significantly promoted the release of active calcium sources, initial nucleation, and subsequent reaction coupling. The results of the comparative examples are also very telling. In Comparative Example 1, after replacing CO2 sparkling water with ordinary mixing water, although a functional additive was used, CO2 sparkling water was not added. The strength at 7 days was only 2.02 MPa, and at 28 days it was 4.21 MPa, indicating that simply introducing a functional additive cannot fully translate into a strength advantage. In Comparative Example 2, without the addition of N,N,N',N'-tetrahydroxyethylethylenediamine, the strength at 28 days actually decreased to 3.83 MPa, indicating that rheological optimization alone cannot bring about structural enhancement, and may even weaken strength development due to insufficient reaction propagation. In Comparative Example 4, without the addition of nitrilotriacetic acid, the flowability reached 241 mm, indicating that the absence of a rheology modifier leads to deterioration in flowability.
[0087] Table 1. Flowability and setting time of CO2 bubble water filling slurry
[0088] sample Initial flowability / mm Initial setting time / min Final setting time / min Example 1 265 590 750 Example 2 260 570 740 Example 3 268 580 740 Example 4 270 530 680 Example 5 266 520 690 Example 6 262 540 680 Example 7 260 550 670 Example 8 257 510 650 Example 9 255 500 630 Example 10 265 520 640 Comparative Example 1 245 640 810 Comparative Example 2 258 660 820 Comparative Example 3 253 600 740 Comparative Example 4 241 620 790 Comparative Example 5 243 620 770
Claims
1. A method for preparing a nano-CO2 bubble water filling material, characterized in that, Includes the following steps: (1) Steel slag powder, slag powder, fluorogypsum, rheology modifier and targeted activator are added to a ball mill for grinding and premixing to obtain a uniformly mixed composite powder material; (2) Add nano CO2 bubble water and continuously graded coal gangue aggregate to the composite powder material obtained in step (1). First, stir for 1 to 5 minutes at a stirring speed of 200 to 300 r / min, and then continue stirring for 1 to 5 minutes at a stirring speed of 400 to 600 r / min to obtain CO2 bubble water filling slurry for filling coal mine goaf.
2. The preparation method according to claim 1, characterized in that, The steel slag powder is a byproduct of steelmaking in an alkaline oxidation furnace. After grinding, its specific surface area is 350–450 m². 2 / kg; the slag powder is granulated blast furnace slag, a by-product of blast furnace ironmaking, which, after grinding, has a specific surface area of 550–650 m². 2 / kg; the fluorinated gypsum is a by-product of fluorine-containing industrial processes, and after grinding, its specific surface area is 400-500 m² / kg. 2 / kg.
3. The preparation method according to claim 1, characterized in that, The coal gangue aggregate is a continuously graded aggregate obtained by crushing and screening coal gangue, with a particle size range of 0.05 to 5 mm.
4. The preparation method according to claim 1, characterized in that, The components and dosages in the composite powder material are as follows: 5-20 parts by weight of steel slag powder; 60-90 parts by weight of slag powder; 5-20 parts by weight of fluorinated gypsum; Rheology modifier 0.01~5 parts by weight; Targeted activating admixture 0.01~2 parts by weight; Preferred: 5-15 parts by weight of steel slag powder; 70-90 parts by weight of slag powder; 5-15 parts by weight of fluorinated gypsum; Rheology modifier 0.01~1 parts by weight; Targeted activating admixture 0.01~0.1 parts by weight.
5. The preparation method according to claim 1, characterized in that, The rheology modifier is composed of calcium lactate and potassium sodium tartrate, with a mass ratio of calcium lactate to potassium sodium tartrate of 0.01~3:0.01~2; preferably, the mass ratio of calcium lactate to potassium sodium tartrate is 0.1~2:0.01~0.
1.
6. The preparation method according to claim 1, characterized in that, The targeted activating admixture is composed of N,N,N',N'-tetrahydroxyethylethylenediamine and aminotriacetic acid, with a mass ratio of N,N,N',N'-tetrahydroxyethylethylenediamine to aminotriacetic acid of 0.01~1:0.01~0.
5.
7. The preparation method according to claim 1, characterized in that, The mass ratio of composite powder material to nano-CO2 bubble water is 1~3:1~3, and the mass concentration of CO2 in the nano-CO2 bubble water is 0.01%~2.0%; the mass ratio of composite powder material to coal gangue aggregate is 1:2~3.
8. A nano-CO2 bubble water filling material, characterized in that, The filling material is prepared by the preparation method described in any one of claims 1 to 7.
9. The application of the nano-CO2 bubble water filling material according to claim 8 in the field of mine filling and reinforcement.