A high-strength fiber-reinforced ceramic matrix composite rod and its preparation method

By adding lanthanum-niobium dual-doped boron carbon nitride and onion carbon modified continuous carbon fibers to the ceramic matrix, the problems of insufficient interfacial bonding strength and matrix sintering activity of ceramic matrix composites were solved, and ceramic matrix composite rods with high density, high strength and high toughness were realized.

CN123106239APending Publication Date: 2026-11-17NORTHWESTERN POLYTECHNICAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611543722.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-08
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing ceramic matrix composites suffer from problems such as difficulty in controlling interfacial bonding strength and limited matrix sintering activity, resulting in insufficient mechanical properties and toughness of the materials.

Method used

By adding lanthanum-niobium dual-doped boron carbon nitride and onion carbon modified continuous carbon fibers to a ceramic matrix, high-strength fiber-reinforced ceramic matrix composite rods are prepared by improving the interfacial bonding state and enhancing the sintering activity of the matrix.

Benefits of technology

It significantly improves the sintering density and mechanical properties of composite materials, enhances the bonding strength between fibers and the matrix, and improves the flexural strength and fracture toughness of the materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106239A_ABST
    Figure CN123106239A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of ceramic matrix composite technology, specifically relating to a high-strength fiber-reinforced ceramic matrix composite rod and its preparation method. The preparation method includes the following steps: adding zirconium diboride, silicon carbide, lanthanum-niobium dual-doped boron carbonitride, and phenolic resin to ethanol, and wet-milling to obtain a mixed slurry; impregnating onion-carbon modified continuous carbon fibers into the mixed slurry, followed by winding, spreading, and air-drying to obtain mixed fiber sheets; cutting the mixed fiber sheets and placing them into a mold, hot-pressing and sintering under an inert gas atmosphere, and cooling to obtain the ceramic matrix composite rod. This invention improves the comprehensive performance of the composite material by adding lanthanum-niobium dual-doped boron carbonitride and onion-carbon modified continuous carbon fibers to the ceramic matrix, resulting in ceramic matrix composite rods with excellent flexural strength and fracture toughness, exhibiting a synergistic improvement effect of high density, high strength, and high toughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of ceramic matrix composite technology, specifically relating to a high-strength fiber-reinforced ceramic matrix composite rod and its preparation method. Background Technology

[0002] Ceramic matrix composites (CMCs) possess excellent properties such as high temperature resistance, high specific strength, high specific modulus, and low density. In particular, continuous fiber reinforced CMCs, with their core advantages of lightweight, high temperature resistance, and ablation resistance, have shown broad application prospects in the fields of hot-end components of aero-engines (such as combustion chambers and turbine blades), thermal protection systems of spacecraft, and high-temperature structural components such as scramjet engines.

[0003] However, this material faces two major technical bottlenecks in practical applications. On the one hand, the smooth and chemically inert surface of carbon fibers results in poor wettability with the ceramic matrix, making it difficult to precisely control the interfacial bonding strength. Excessive interfacial bonding leads to brittle fracture in the composite material, failing to effectively utilize the toughening effect of the fibers; conversely, insufficient interfacial bonding hinders effective load transfer, both significantly weakening the material's mechanical properties. To improve interfacial bonding, researchers have attempted to introduce coatings such as pyrolytic carbon and SiC onto the carbon fiber surface using chemical vapor deposition (CVD). However, this process is complex and costly, and the thermal expansion mismatch between the coating and the fiber can easily induce residual stress. Furthermore, a single coating has limited ability to control the interfacial microstructure. On the other hand, ultra-high temperature ceramic matrices, represented by zirconium diboride-silicon carbide (ZrB2-SiC), have limited sintering activity and are not easy to generate high-density composite materials. The low density seriously impairs the strength, toughness, and thermal shock resistance of the materials. In order to improve the sintering properties of the matrix, a third phase is often added to ZrB2-SiC to promote densification. However, while existing added phases improve sintering activity, they often fail to simultaneously improve the strength and toughness of the materials, and the problem of high porosity has not been effectively solved.

[0004] Therefore, there is an urgent need to develop a composite rod and its preparation method that can effectively optimize the fiber-matrix interface state and synergistically improve the sintering activity and mechanical properties of the matrix. Summary of the Invention

[0005] To overcome the shortcomings of existing technologies, the present invention aims to provide a high-strength fiber-reinforced ceramic matrix composite rod and its preparation method. By adding lanthanum-niobium dual-doped boron carbonitride and onion-carbon modified continuous carbon fibers to the ceramic matrix, the comprehensive performance of the composite material is improved, resulting in a ceramic matrix composite rod with excellent flexural strength and fracture toughness, exhibiting a synergistic improvement effect of high density, high strength, and high toughness.

[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows: The first aspect of this invention provides a method for preparing a high-strength fiber-reinforced ceramic matrix composite rod, comprising the following steps: (1) Zirconium diboride, silicon carbide, lanthanum-niobium dual-doped boron carbonitride and phenolic resin were added to ethanol and wet ball milled to obtain a mixed slurry; (2) Onion carbon modified continuous carbon fiber is added to the mixed slurry for impregnation, and after winding, spreading and air drying, a mixed fiber sheet is obtained; (3) After cutting the mixed fiber sheets, they are placed into a mold, hot-pressed and sintered in an inert gas atmosphere, and then cooled to obtain ceramic matrix composite rods.

[0007] Furthermore, the lanthanum-niobium dual-doped boron carbonitride titanium is prepared by the following steps: Metatitanic acid, lanthanum chloride, niobium ammonium oxalate, boric acid and glucose were added to water and mixed evenly. After drying, the mixture was first calcined under an argon atmosphere and then sintered under a nitrogen atmosphere to obtain lanthanum-niobium double-doped boron carbon nitride.

[0008] Furthermore, the ratio of metatitanic acid, lanthanum chloride, niobium ammonium oxalate, boric acid, glucose and water is 100 g : (0.8-2.6) g : (5.7-11.4) g : (13-14) g : (12-13.5) g : (300-400) mL.

[0009] Furthermore, the calcination temperature is 300-400 ℃ and the time is 1-1.5 h; the sintering temperature is 1200-1400 ℃ and the time is 1.5-2.5 h.

[0010] Further, the onion-modified carbon continuous carbon fiber described in step (2) is prepared by the following steps: (a) The catalyst, curing agent, phenolic resin and ethanol are mixed evenly, and then acid-treated continuous carbon fibers are added. After impregnation, drying and curing, resin-coated continuous carbon fibers are obtained. (b) In an inert gas atmosphere, resin-coated continuous carbon fibers are calcined, cooled, and then immersed in acid to obtain onion carbon modified continuous carbon fibers.

[0011] Further, the method for preparing the acid-treated continuous carbon fiber in step (a) is as follows: add the continuous carbon fiber to a nitric acid solution with a concentration of 10-12 mol / L and soak it at 50-70 ℃ for 5-8 h to obtain the continuous carbon fiber; the ratio of the continuous carbon fiber to the nitric acid solution is 1 g: 8-10 mL.

[0012] Further, in step (a), the catalyst is ferric nitrate, and the curing agent is hexamethylenetetramine; the ratio of the amount of phenolic resin, acid-treated continuous carbon fiber, curing agent, catalyst, and ethanol is 1 g: (2-2.5) g: (0.05-0.1) g: (0.06-0.08) g: (10-12) mL; the impregnation time is 6-12 h; and the curing temperature is 120-150 ℃, and the time is 0.5-1 h.

[0013] Further, in step (b), the calcination temperature is 950-1050 ℃ and the time is 3-5 h; the acid solution is a 0.5-1 mol / L dilute hydrochloric acid solution; the soaking time is 10-15 h; and the ratio of the amount of resin-coated continuous carbon fiber to the amount of acid solution is 1 g: 10-12 mL.

[0014] Further, in step (1), the ratio of zirconium diboride, silicon carbide, lanthanum-niobium dual-doped boron carbonitride, phenolic resin and ethanol is 10 g: (2-3) g: (0.3-0.7) g: (0.19-0.41) g: (16-20) mL; in step (2), the mass ratio of the mixed slurry and onion carbon modified continuous carbon fiber is 1: (0.03-0.04); in step (3), the hot pressing sintering pressure is 20-25 MPa, the temperature is 1700-1800 ℃, and the time is 0.8-1.2 h.

[0015] A second aspect of the present invention provides a high-strength fiber-reinforced ceramic matrix composite rod prepared by the above-described preparation method.

[0016] The beneficial technical effects of this invention are as follows: 1. This invention significantly improves the sintering density and mechanical properties of composite materials by adding lanthanum and niobium-doped titanium boron carbon nitride to a ceramic matrix. Titanium boron carbon nitride has a face-centered cubic structure and possesses high strength and hardness. As an additive phase in ceramic materials, it can effectively improve the mechanical properties of the material. The dual-element doping of lanthanum and niobium can create lattice distortion, further enhancing the mechanical properties. Moreover, lanthanum doping can adsorb and purify impurities, reducing interfacial impurity segregation, while niobium doping can improve high-temperature stability. Together, these two factors enhance the surface activity of the titanium boron carbon nitride particles, improve the lattice fit between the particles and the ceramic matrix, improve the sintering activity of the material, and increase the sintering density.

[0017] 2. This invention uses onion-carbon coated and modified continuous carbon fibers as reinforcement, significantly improving the strength and fracture toughness of the composite material. Continuous carbon fibers have excellent toughening and reinforcing effects, while onion-carbon has a multi-layered nano-graphite structure. Coating the fiber surface can form tiny protrusions that serve as a transition layer between the carbon fibers and the ceramic matrix, optimizing the bonding state between the fibers and the matrix. Through multiple mechanisms such as crack deflection, fiber pull-out, and interlaminar slip, the strength and toughness of the composite material are further improved. Attached Figure Description

[0018] Figure 1 X-ray diffraction (XRD) patterns of lanthanum-niobium double-doped boron carbonitride and boron carbonitride prepared in Example 1 of this invention. Figure 2 This is a scanning electron microscope image of the onion-carbon modified continuous carbon fiber prepared in Example 4 of the present invention. Detailed Implementation

[0019] The following is a further detailed description of the present invention in conjunction with specific preferred embodiments, and it should not be construed that the specific implementation of the present invention is limited to these descriptions. For those skilled in the art, various simple deductions or substitutions can be made without departing from the concept of the present invention, and all such modifications and substitutions should be considered within the scope of protection of the present invention. Specific conditions not specified in the embodiments are performed according to conventional conditions or conditions recommended by the manufacturer. Unless otherwise specified, all reagents or instruments used are conventional products obtained through commercial channels.

[0020] (a) Preparation example Preparation Example 1 Preparation Example 1 provides a lanthanum-niobium dual-doped boron carbonitride titanium, which is prepared by the following steps: According to the ratio of metatitanic acid, lanthanum chloride, niobium ammonium oxalate, boric acid, glucose and water of 100 g: 1.5 g: 9 g: 14 g: 13 g: 350 mL, metatitanic acid, lanthanum chloride, niobium ammonium oxalate, boric acid and glucose were added to water and stirred thoroughly until uniformly mixed. After drying, a powder was obtained. The powder was transferred to a tube furnace and calcined at 350 °C for 1.2 h under an argon atmosphere, and then sintered at 1300 °C for 2 h under a nitrogen atmosphere. After cooling, lanthanum-niobium double-doped boron carbonitride titanium was obtained.

[0021] Preparation Example 2 Preparation Example 2 provides a lanthanum-niobium dual-doped boron carbonitride titanium, prepared by the following steps: According to the ratio of metatitanic acid, lanthanum chloride, niobium ammonium oxalate, boric acid, glucose and water of 100 g: 0.8 g: 5.7 g: 13 g: 12 g: 300 mL, metatitanic acid, lanthanum chloride, niobium ammonium oxalate, boric acid and glucose were added to water and stirred thoroughly until uniformly mixed. After drying, a powder was obtained. The powder was transferred to a tube furnace and calcined at 300 °C for 1.5 h under an argon atmosphere, and then sintered at 1200 °C for 2.5 h under a nitrogen atmosphere. After cooling, lanthanum-niobium double-doped boron carbonitride titanium was obtained.

[0022] Preparation Example 3 Preparation Example 3 provides a lanthanum-niobium dual-doped boron carbonitride titanium, prepared by the following steps: According to the ratio of metatitanic acid, lanthanum chloride, niobium ammonium oxalate, boric acid, glucose and water of 100 g: 2.6 g: 11.4 g: 14 g: 13.5 g: 400 mL, metatitanic acid, lanthanum chloride, niobium ammonium oxalate, boric acid and glucose were added to water and stirred thoroughly until uniformly mixed. After drying, a powder was obtained. The powder was transferred to a tube furnace and calcined at 400 °C for 1 h under an argon atmosphere, and then sintered at 1400 °C for 1.5 h under a nitrogen atmosphere. After cooling, lanthanum-niobium double-doped boron carbonitride titanium was obtained.

[0023] Preparation Example 4 Preparation Example 4 provides an onion-carbon modified continuous carbon fiber, which is prepared by the following steps: (a) Continuous carbon fibers were added to 11 mol / L nitric acid solution at a ratio of 1 g: 9 mL, and soaked at 60 °C for 6 h. After filtration, washing, and drying, acid-treated continuous carbon fibers were obtained. Ferric nitrate, hexamethylenetetramine, ferric nitrate, and ethanol were mixed evenly at a ratio of 1 g: 2.2 g: 0.08 g: 0.07 g: 11 mL. Then, acid-treated continuous carbon fibers were added and impregnated for 9 h. After evaporating the solvent and drying, the mixture was cured at 140 °C for 0.8 h to obtain resin-coated continuous carbon fibers. (b) Under an argon atmosphere, resin-coated continuous carbon fibers were calcined at 1000 °C for 4 h. After cooling, the resin-coated continuous carbon fibers and dilute hydrochloric acid solution were soaked in 0.8 mol / L dilute hydrochloric acid solution for 12 h at a ratio of 1 g: 11 mL. After filtration, washing and drying, onion carbon modified continuous carbon fibers were obtained.

[0024] Preparation Example 5 Preparation Example 5 provides an onion-carbon modified continuous carbon fiber, which is prepared by the following steps: (a) Continuous carbon fibers were added to a 10 mol / L nitric acid solution at a ratio of 1 g: 8 mL, and soaked at 50 °C for 8 h. After filtration, washing, and drying, acid-treated continuous carbon fibers were obtained. Phenolic resin, acid-treated continuous carbon fibers, hexamethylenetetramine, ferric nitrate, and ethanol were mixed evenly at a ratio of 1 g: 2 g: 0.05 g: 0.06 g: 10 mL. Then, acid-treated continuous carbon fibers were added and impregnated for 6 h. After evaporating the solvent and drying, the mixture was cured at 120 °C for 1 h to obtain resin-coated continuous carbon fibers. (b) Under an argon atmosphere, the resin-coated continuous carbon fiber was calcined at 950 °C for 5 h. After cooling, it was soaked in 0.5 mol / L dilute hydrochloric acid solution for 15 h according to the ratio of resin-coated continuous carbon fiber to dilute hydrochloric acid solution of 1 g: 10 mL. After filtration, washing and drying, onion carbon modified continuous carbon fiber was obtained.

[0025] Preparation Example 6 Preparation Example 6 provides an onion-carbon modified continuous carbon fiber, which is prepared by the following steps: (a) Continuous carbon fibers were added to a 12 mol / L nitric acid solution at a ratio of 1 g: 10 mL, and soaked at 70 °C for 5 h. After filtration, washing, and drying, acid-treated continuous carbon fibers were obtained. Ferric nitrate, hexamethylenetetramine, ferric nitrate, and ethanol were mixed evenly at a ratio of 1 g: 2.5 g: 0.1 g: 0.08 g: 12 mL. Then, acid-treated continuous carbon fibers were added and impregnated for 12 h. After evaporating the solvent and drying, the mixture was cured at 150 °C for 0.5 h to obtain resin-coated continuous carbon fibers. (b) Under an argon atmosphere, the resin-coated continuous carbon fiber was calcined at 1050 °C for 3 h. After cooling, it was soaked in 1 mol / L dilute hydrochloric acid solution for 10 h according to the ratio of resin-coated continuous carbon fiber to dilute hydrochloric acid solution of 1 g: 12 mL. After filtration, washing and drying, onion carbon modified continuous carbon fiber was obtained.

[0026] (II) Implementation Examples

[0027] Example 1 Example 1 provides a method for preparing a high-strength fiber-reinforced ceramic matrix composite rod, comprising the following steps: (1) According to the ratio of zirconium diboride, silicon carbide, lanthanum-niobium double-doped boron carbonitride, phenolic resin and ethanol, zirconium diboride, silicon carbide, lanthanum-niobium double-doped boron carbonitride and phenolic resin in Preparation Example 1, zirconium diboride, silicon carbide, lanthanum-niobium double-doped boron carbonitride and phenolic resin in Preparation Example 1 and ethanol were added to ethanol and wet ball milled for 8 h to obtain a mixed slurry. (2) According to the mass ratio of mixed slurry and onion carbon modified continuous carbon fiber of 1:0.03, the onion carbon modified continuous carbon fiber of Preparation Example 4 was added to the mixed slurry for impregnation, and then wound onto the surface by a rotating roller. After spreading and air drying, mixed fiber sheets were obtained. (3) After cutting the mixed fiber sheets and stacking them in a cross shape, they are placed into a mold, vacuumed, filled with argon, and hot-pressed and sintered for 1 h at 24 MPa and 1800 ℃. After cooling in the furnace, ceramic matrix composite rods are obtained.

[0028] This embodiment also provides a high-strength fiber-reinforced ceramic matrix composite rod prepared by the above method.

[0029] Example 2 Example 2 provides a method for preparing a high-strength fiber-reinforced ceramic matrix composite rod, comprising the following steps: (1) According to the ratio of zirconium diboride, silicon carbide, lanthanum-niobium double-doped boron carbonitride, phenolic resin and ethanol, zirconium diboride, silicon carbide, lanthanum-niobium double-doped boron carbonitride and phenolic resin in preparation Example 2 and ethanol, zirconium diboride, silicon carbide, lanthanum-niobium double-doped boron carbonitride and phenolic resin in preparation Example 2 and ethanol were added to ethanol and wet ball milled for 5 h to obtain a mixed slurry. (2) According to the mass ratio of mixed slurry and onion carbon modified continuous carbon fiber of 1:0.03, the onion carbon modified continuous carbon fiber of Preparation Example 5 was added to the mixed slurry for impregnation, and then wound onto the surface by a rotating roller. After spreading and air drying, mixed fiber sheets were obtained. (3) After cutting the mixed fiber sheets and stacking them in a cross shape, they are placed into a mold, vacuumed, filled with argon, and hot-pressed and sintered at 20 MPa and 1700 ℃ for 1.2 h. After cooling in the furnace, ceramic matrix composite rods are obtained.

[0030] This embodiment also provides a high-strength fiber-reinforced ceramic matrix composite rod prepared by the above method.

[0031] Example 3 Example 3 provides a method for preparing a high-strength fiber-reinforced ceramic matrix composite rod, comprising the following steps: (1) According to the ratio of zirconium diboride, silicon carbide, lanthanum-niobium double-doped boron carbonitride, phenolic resin and ethanol, zirconium diboride, silicon carbide, lanthanum-niobium double-doped boron carbonitride and phenolic resin in preparation Example 3 and ethanol, zirconium diboride, silicon carbide, lanthanum-niobium double-doped boron carbonitride and phenolic resin in preparation Example 3 and ethanol were added to ethanol and wet ball milled for 10 h to obtain a mixed slurry. (2) According to the mass ratio of mixed slurry and onion carbon modified continuous carbon fiber of 1:0.04, the onion carbon modified continuous carbon fiber of Preparation Example 6 was added to the mixed slurry for impregnation, and then wound onto the surface by a rotating roller. After spreading and air drying, mixed fiber sheets were obtained. (3) After cutting the mixed fiber sheets and stacking them in a cross shape, they are placed into a mold and vacuumed. Argon gas is then introduced and hot-pressed for 0.8 h at 25 MPa and 1800 ℃. After cooling in the furnace, ceramic matrix composite rods are obtained.

[0032] This embodiment also provides a high-strength fiber-reinforced ceramic matrix composite rod prepared by the above method.

[0033] (III) Comparative Example Comparative Example 1 Comparative Example 1 is basically the same as Example 1, except that the onion carbon modified continuous carbon fiber in Example 1 is replaced with continuous carbon fiber.

[0034] Comparative Example 2 Comparative Example 2 is basically the same as Example 1, except that the lanthanum-niobium double-doped boron carbonitride in Example 1 is replaced with boron carbonitride.

[0035] Comparative Example 3 Comparative Example 3 is basically the same as Example 1, except that the lanthanum-niobium double-doped boron carbonitride in Example 1 is replaced with a mixture of boron carbonitride, lanthanum oxide and niobium oxide, wherein the mass ratio of boron carbonitride, lanthanum oxide and niobium oxide is 100:1.88:3.44.

[0036] (iv) Test Examples Test Example 1 Figure 1 The XRD patterns of lanthanum-niobium double-doped boron carbonitride and boron carbonitride prepared in Example 1 of this invention are shown below. Figure 1 As can be seen from the data, the diffraction peaks of lanthanum-niobium double-doped boron carbonitride titanium match well with the face-centered cubic structure, and the peak positions are slightly shifted, confirming that lanthanum and niobium have been successfully dissolved and lattice distortion has been introduced; at the same time, no impurity phase peaks appear in the spectrum, indicating that a single solid solution has been formed.

[0037] Figure 2The image shows a scanning electron microscope (SEM) image of the onion-carbon modified continuous carbon fiber prepared in Example 4 of this invention. As can be seen from the image, the carbon fiber surface is uniformly coated with an onion-carbon layer, exhibiting a rough morphology and accompanied by a large number of micro-protrusions, which is beneficial to enhancing the interfacial bonding between the fiber and the ceramic matrix.

[0038] Test Example 2 The ceramic-based composite rods prepared in Examples 1-3 and Comparative Examples 1-3 were subjected to the following performance tests.

[0039] Density test: The bulk density of each sample was tested in accordance with GB / T 25995-2010 "Test Method for Density and Apparent Porosity of Fine Ceramics", and the relative density was calculated (based on theoretical density).

[0040] Bending strength test: The bending strength of each specimen was tested in accordance with GB / T 6569-2006 "Test Method for Bending Strength of Fine Ceramics".

[0041] Fracture toughness test: The fracture toughness of each specimen was tested in accordance with GB / T 23806-2025 "Test method for fracture toughness of fine ceramics - single-sided pre-cracked beam (SEPB) method".

[0042] The test results are shown in Table 1.

[0043] Table 1. Test results of density, flexural strength and fracture toughness of each embodiment and comparative example.

[0044] As shown in Table 1, the ceramic-based composite rods prepared in Examples 1-3 of the present invention have excellent bending strength and fracture toughness, exhibiting a synergistic improvement effect of high density, high strength and high toughness.

[0045] Compared to Example 1, Comparative Example 1 used ordinary continuous carbon fibers without coating treatment, which showed a decrease in density, but also a significant reduction in flexural strength and fracture toughness. This indicates that the interfacial bonding between the uncoated carbon fibers and the ceramic matrix is ​​poor, and the toughening mechanisms such as fiber pull-out and crack deflection cannot be effectively utilized. Although the impact on the overall density is relatively limited, the weak interface directly leads to a sharp deterioration in the material's strength and toughness.

[0046] Compared to Example 1, Comparative Example 2, using undoped boron carbonitride, exhibited a sharp decrease in density, with the lowest flexural strength and fracture toughness. This indicates that the dual doping of lanthanum and niobium can induce lattice distortion, enhancing the surface activity of the boron carbonitride particles. This significantly improves the lattice fit between the particles and the ceramic matrix, as well as the sintering activity of the material, effectively promoting the densification process and substantially increasing density. Simultaneously, lanthanum doping can adsorb and purify interfacial impurities, reducing interfacial segregation, while niobium doping helps improve high-temperature stability. The synergistic effect of both enhances the overall mechanical properties of the material.

[0047] Compared to Example 1, Comparative Example 3, which replaced lanthanum-niobium dual-doped boron carbonitride with a mechanical mixture of boron carbonitride, lanthanum oxide, and niobium oxide, showed improved density, flexural strength, and fracture toughness compared to Comparative Example 2, but was still significantly lower than Example 1. This indicates that the key to achieving lattice distortion and improving sintering activity lies in the doping of lanthanum and niobium into the boron carbonitride lattice to form a solid solution, rather than simply mixing as independent oxides. Directly mixed oxides cannot produce lattice distortion, and oxide particles tend to agglomerate at grain boundaries, hindering particle rearrangement and densification processes, resulting in limited improvement in density and mechanical properties.

[0048] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them. The basic principles and main features of the present invention have been described above with specific implementation schemes. Based on the present invention, some modifications or substitutions can be made, but these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of protection claimed by the present invention.

Claims

1. A method for preparing a high-strength fiber-reinforced ceramic matrix composite rod, characterized in that, Includes the following steps: (1) Zirconium diboride, silicon carbide, lanthanum-niobium dual-doped boron carbonitride and phenolic resin were added to ethanol and wet ball milled to obtain a mixed slurry; (2) Onion carbon modified continuous carbon fiber is added to the mixed slurry for impregnation, and after winding, spreading and air drying, a mixed fiber sheet is obtained; (3) After cutting the mixed fiber sheets, they are placed into a mold, hot-pressed and sintered in an inert gas atmosphere, and then cooled to obtain ceramic matrix composite rods.

2. The method for preparing high-strength fiber-reinforced ceramic matrix composite rods according to claim 1, characterized in that, The lanthanum-niobium dual-doped boron carbonitride titanium dioxide was prepared by the following steps: Metatitanic acid, lanthanum chloride, niobium ammonium oxalate, boric acid and glucose were added to water and mixed evenly. After drying, the mixture was first calcined under an argon atmosphere and then sintered under a nitrogen atmosphere to obtain lanthanum-niobium double-doped boron carbon nitride.

3. The method for preparing the high-strength fiber-reinforced ceramic matrix composite rod according to claim 2, characterized in that, The ratio of metatitanic acid, lanthanum chloride, niobium ammonium oxalate, boric acid, glucose and water is 100 g : (0.8-2.6) g : (5.7-11.4) g : (13-14) g : (12-13.5) g : (300-400) mL.

4. The method for preparing the high-strength fiber-reinforced ceramic matrix composite rod according to claim 2, characterized in that, The calcination temperature is 300-400 ℃ and the time is 1-1.5 h; the sintering temperature is 1200-1400 ℃ and the time is 1.5-2.5 h.

5. The method for preparing high-strength fiber-reinforced ceramic matrix composite rods according to claim 1, characterized in that, The onion-modified carbon continuous carbon fiber described in step (2) is prepared by the following steps: (a) The catalyst, curing agent, phenolic resin and ethanol are mixed evenly, and then acid-treated continuous carbon fibers are added. After impregnation, drying and curing, resin-coated continuous carbon fibers are obtained. (b) In an inert gas atmosphere, resin-coated continuous carbon fibers are calcined, cooled, and then immersed in acid to obtain onion carbon modified continuous carbon fibers.

6. The method for preparing the high-strength fiber-reinforced ceramic matrix composite rod according to claim 5, characterized in that, The method for preparing the acid-treated continuous carbon fiber in step (a) is as follows: add the continuous carbon fiber to a nitric acid solution with a concentration of 10-12 mol / L and soak it at 50-70 ℃ for 5-8 h to obtain the carbon fiber; the ratio of the continuous carbon fiber to the nitric acid solution is 1g:8-10mL.

7. The method for preparing the high-strength fiber-reinforced ceramic matrix composite rod according to claim 5, characterized in that, The catalyst in step (a) is ferric nitrate, and the curing agent is hexamethylenetetramine; the ratio of phenolic resin, acid-treated continuous carbon fiber, curing agent, catalyst and ethanol is 1 g: (2-2.5) g: (0.05-0.1) g: (0.06-0.08) g: (10-12) mL; the impregnation time is 6-12 h; the curing temperature is 120-150 ℃, and the time is 0.5-1 h.

8. The method for preparing the high-strength fiber-reinforced ceramic matrix composite rod according to claim 5, characterized in that, The calcination temperature in step (b) is 950-1050 ℃ and the time is 3-5 h; the acid solution is a 0.5-1 mol / L dilute hydrochloric acid solution; the soaking time is 10-15 h; the ratio of the amount of resin-coated continuous carbon fiber to the amount of acid solution is 1 g: 10-12 mL.

9. The method for preparing the high-strength fiber-reinforced ceramic matrix composite rod according to claim 1, characterized in that, In step (1), the ratio of zirconium diboride, silicon carbide, lanthanum-niobium dual-doped boron carbonitride, phenolic resin and ethanol is 10g:(2-3)g:(0.3-0.7)g:(0.19-0.41)g:(16-20)mL; in step (2), the mass ratio of the mixed slurry and onion carbon modified continuous carbon fiber is 1:(0.03-0.04); in step (3), the hot pressing sintering pressure is 20-25 MPa, the temperature is 1700-1800 ℃, and the time is 0.8-1.2 h.

10. A high-strength fiber-reinforced ceramic matrix composite rod, characterized in that, It is prepared by the preparation method described in any one of claims 1-9.