Methods and applications for preparing high-purity bis(4-hydroxymethylcyclohexylmethyl) terephthalate from PET
By combining MXene-metal salt composite catalysts with precipitation, acid washing, and solvent purification steps, the problem of separating high-purity BHCT monomers from waste PET was solved, enabling the preparation of high-purity BHCT monomers and improving the design and performance of polyester materials.
Patent Information
- Application Number
- CN202611276540.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-21
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies make it difficult to efficiently separate and purify high-purity bis(4-hydroxymethylcyclohexylmethyl) terephthalate (BHCT) monomer directly from waste PET, which limits its application in the structural design and performance improvement of polyester materials.
High-purity BHCT monomers were prepared by reacting MXene-metal salt composite catalysts with PET material and 1,4-cyclohexanediethanol under inert gas purging, followed by precipitation, acid washing, and solvent purification steps.
The BHCT monomer obtained by this method has a purity of no less than 95%, a BHET content of no more than 3%, and a metal residue of no more than 20 ppm, making it suitable as a high-quality monomer raw material for the synthesis of polyesters or copolyesters.
Smart Images

Figure CN123106416A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of polyester chemical recycling and polyester monomer preparation technology, specifically relating to a method and application for preparing high-purity bis(4-hydroxymethylcyclohexylmethyl) terephthalate from PET. Background Technology
[0002] In the chemical recycling of polyester, waste polyester, after depolymerization, can either be used directly as a mixed raw material in subsequent polycondensation, or it can be separated and purified to participate in polymerization again in the form of monomers with well-defined structures. The former process is shorter, but the system often contains oligomers, transesterification products with different end groups, thermal degradation byproducts, and catalyst and processing aid residues. These may continue to cause side reactions during subsequent melt polycondensation or reprocessing, increasing the uncertainty in the control of the composition, color, and performance of the recycled polyester. In contrast, converting waste polyester into monomers with low impurity content and measurable usability is more conducive to the composition design and quality control of subsequent polymerization. Dihydroxy terephthalates, represented by bis(hydroxyethyl) terephthalate (BHET), are typical intermediates in the monomer recycling and repolymerization of PET.
[0003] Building upon this, replacing ethylene glycol (EG) with 1,4-cyclohexanediethanol (CHDM), which has a higher boiling point and stronger nucleophilicity, can improve reaction efficiency while yielding a high-value monomer, bis(4-hydroxymethylcyclohexylmethyl) terephthalate (BHCT), suitable for the preparation of PETG, PCTG, and other novel polyesters. This monomeric structural unit disrupts the regular stacking of polyester segments, reducing crystallization tendency and thus facilitating the acquisition of copolyester materials with high transparency and good toughness. Simultaneously, the introduction of the cyclohexane alicyclic structure also helps improve the material's heat resistance, dimensional stability, and thermo-oxidative processing stability, reducing the tendency to generate degradation byproducts during thermal processing (S. Richard Turner, Encyclopedia of Polymer Science and Technology, Wiley, 2001). Furthermore, BHCT compounds have a low melting point, are highly operable, and can undergo transesterification or polycondensation reactions with various glycols, diacids, or ester monomers. Because the ester bonds formed between terephthalic acid and CHDM in BHCT are relatively stable and not easily destroyed under appropriate reaction conditions, their structural units are more likely to be preserved in subsequent copolymerization processes. If it undergoes transesterification with relatively highly reactive ester bonds or monomers, it is beneficial to construct special copolyesters containing repeating BHCT units, thus endowing the material with special properties, such as a higher glass transition temperature, excellent dimensional stability, and low haze.
[0004] Existing technologies include methods for converting waste PET into PETG or PCTG copolyesters. For example, patent CN115490839B uses a mixed alcohol system composed of EG and CHDM to alcoholyze waste PET, and directly uses the resulting mixture of BHET, BHCT, and their oligomers for subsequent polycondensation. Since EG and CHDM participate in both alcoholysis and transesterification, the resulting system typically contains BHET, BHCT, mixed end-group oligomers, and oligomers with different degrees of polymerization, making it more suitable as a mixed raw material for further polycondensation than for the separation and preparation of a single BHCT monomer. Patent CN114853991A first converts waste PET into DMT and purifies it, then adds an EG / CHDM mixed alcohol for transesterification and further polycondensation. This type of route is based on small-molecule raw materials with well-defined composition and high reactivity purified after waste PET depolymerization, and does not involve the direct alcoholysis reaction of waste PET and CHDM, nor does it obtain high-purity BHCT monomer. It is evident that existing technologies can only convert waste PET into polyester materials such as PETG / PCTG. The common approach is to convert waste PET into mixed raw materials that can continue to polycondense. However, the problem of directly converting waste PET and separating high-purity BHCT monomers has not yet been solved, which limits the design of new polyester structures.
[0005] Using CHDM directly as an external alcoholysis agent is a reaction design that more closely approximates the target BHCT structure. Compared to the EG / CHDM mixed alcoholysis system, reducing the introduction of external EG helps to decrease the tendency for BHET and EG end-group byproducts to form. However, directly using CHDM does not necessarily yield high-purity BHCT. During the alcoholysis of PET and CHDM, EG is still released in situ, and the generated EG can continue to participate in competitive transesterification, forming BHET or oligomers containing EG end groups. Simultaneously, BHCT itself contains hydroxymethyl end groups, which may continue to undergo transesterification or condensation under high temperature and in the presence of a catalyst, generating oligomers containing BHCT structural units. These factors mean that direct CHDM alcoholysis not only requires the breaking of the PET backbone but also the control of EG competitive reactions, BHCT oligomerization, and subsequent product purification. Summary of the Invention
[0006] The main objective of this invention is to provide a method for preparing high-purity bis(4-hydroxymethylcyclohexylmethyl) terephthalate from PET, thereby overcoming the shortcomings of the prior art.
[0007] Another object of the present invention is to provide high-purity bis(4-hydroxymethylcyclohexylmethyl) terephthalate prepared by the method and its applications.
[0008] To achieve the aforementioned objectives, the technical solution adopted by this invention includes: This invention provides a method for preparing high-purity bis(4-hydroxymethylcyclohexylmethyl) terephthalate from PET, comprising: Under inert gas purging, a mixed reaction system containing PET material, 1,4-cyclohexanediethanol and MXene-metal salt composite catalyst is subjected to alcoholysis reaction to obtain a reaction solution containing bis(4-hydroxymethylcyclohexylmethyl) terephthalate. The reaction solution is brought into contact with the precipitating solvent to obtain a solid product, which is then purified to obtain high-purity bis(4-hydroxymethylcyclohexylmethyl) terephthalate.
[0009] In some embodiments, the MXene-metal salt composite catalyst is a combination of MXene material and a metal salt, wherein the MXene material includes Ti3C2T. x Ti2CT x Mo2Ti2C3T x One or more of the following, wherein the metal salt includes one or more of zinc acetate, manganese acetate, cobalt acetate, stannous octoate, and antimony acetate.
[0010] This invention also provides high-purity bis(4-hydroxymethylcyclohexylmethyl) terephthalate prepared by the aforementioned method.
[0011] Furthermore, the purity of the high-purity bis(4-hydroxymethylcyclohexylmethyl) terephthalate is not less than 95%, the content of bis(hydroxyethyl) terephthalate (BHET) is not more than 3%, and the residual amount of metal elements is not more than 20 ppm.
[0012] This invention also provides the application of the high-purity bis(4-hydroxymethylcyclohexylmethyl) terephthalate as a monomer raw material in the field of polyester or copolyester synthesis.
[0013] Compared with the prior art, the beneficial effects of the present invention are as follows: Compared to the direct polycondensation route of ethylene glycol / 1,4-cyclohexanediethanol mixed alcoholysis products, this invention, through the combination of direct alcoholysis of 1,4-cyclohexanediethanol, MXene-metal salt composite catalyst, nitrogen purging, precipitation, acid washing, and selective solvent purification, transforms waste PET recycling products from a complex polycondensation mixture into independently meterable bis(4-hydroxymethylcyclohexylmethyl) terephthalate (BHCT) monomer.
[0014] The MXene-metal salt composite catalyst used in this invention promotes the activation and cleavage of ester bonds in the PET backbone, while MXene improves the local contact and dispersion in the high-viscosity CHDM / PET system and helps reduce the tendency of BHCT monomers to undergo further transesterification or oligomerization. Through the synergistic effect of the composite catalyst and the separation and purification steps, the purity of the obtained BHCT monomer, calculated by nuclear magnetic resonance, can reach over 95%, the BHET content is no higher than 3%, and the residual amount of the catalyst-derived metal element, determined by ICP, is no higher than 20 ppm. This monomer can be used as a monomer raw material in the synthesis of polyesters or copolyesters. Attached Figure Description
[0015] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0016] Figure 1 The image shows the appearance of the BHCT product prepared in Example 1 of this invention. Figure 2 These are the 1H NMR spectra of the BHCT products prepared in Example 1 and Comparative Example 1 of this invention; Figure 3 These are the DSC images of the BHCT products prepared in Example 1 and Comparative Example 1 of this invention; Figure 4 This is the 1H NMR spectrum of the PETG copolyester prepared in Application Verification Example 1 of this invention. Detailed Implementation
[0017] In view of the deficiencies of existing technologies, the inventors of this invention, through long-term research and extensive practice, have proposed the technical solution of this invention, employing a catalytic design that combines low-content MXene with a metal salt. The metal salt can act as a Lewis acid center, coordinating and activating the carbonyl group of the PET backbone ester, increasing the electrophilicity of the carbonyl carbon, thereby promoting the attack of CHDM on the PET ester bond. Ti3C2T xMXene, as a two-dimensional layered material, contains Ti sites and end groups such as –O, –OH, and –F on its surface. These provide interfacial contact regions for PET segments, CHDM, and zinc salt active centers, which is beneficial for improving local dispersion and mass transfer in high-viscosity CHDM / PET systems. Simultaneously, the MXene surface end groups may coordinate, adsorb, or enrich with some metal ions or ester structures, making the catalytic process more likely to occur during the PET backbone breaking and CHDM end group formation stages, rather than indiscriminately promoting the oligomerization of BHCT. Therefore, the MXene-metal salt composite catalytic system holds promise for improving BHCT monomer selectivity while maintaining PET alcoholysis efficiency. Furthermore, combined with subsequent precipitation, acid washing, and solvent purification processes, it can reduce metal catalyst residue and obtain BHCT monomers more suitable as polymerization-grade feedstocks.
[0018] This invention aims to address the problem that existing waste PET recycling routes primarily use the products as raw materials for mixed polycondensation, making it difficult to obtain high-purity BHCT monomers from the direct reaction system of waste PET and CHDM. Specifically, the direct alcoholysis process of waste PET and CHDM suffers from several problems, including high viscosity of the CHDM system, insufficient contact between PET segments and the alcoholysis agent and catalytic active sites, in-situ release of EG during PET alcoholysis leading to the further formation of BHET or EG-terminated oligomers, continued transesterification or oligomerization of BHCT monomers under high temperature and in the presence of a catalyst, and difficulty in separating BHCT monomers from oligomers and catalyst residues. Therefore, this invention provides a method for directly preparing and purifying high-purity BHCT monomers from waste PET, resulting in polymer-grade BHCT monomers with well-defined composition, low BHET content, low catalyst residue, and independent metering for use.
[0019] The technical solution of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0020] Specifically, as one aspect of the technical solution of this invention, a method for preparing high-purity bis(4-hydroxymethylcyclohexylmethyl) terephthalate (BHCT) from PET includes: Under inert gas purging, a mixed reaction system containing PET material, 1,4-cyclohexanediethanol (CHDM), and MXene-metal salt composite catalyst is subjected to alcoholysis reaction to obtain a reaction solution containing bis(4-hydroxymethylcyclohexylmethyl) terephthalate. The reaction solution is brought into contact with the precipitating solvent to obtain a solid product, which is then purified to obtain high-purity bis(4-hydroxymethylcyclohexylmethyl) terephthalate.
[0021] In some embodiments, the method specifically includes: mixing PET material, 1,4-cyclohexanediethanol (CHDM), and MXene-metal salt composite catalyst, and carrying out an alcoholysis reaction under nitrogen purging to obtain a reaction solution containing bis(4-hydroxymethylcyclohexylmethyl) terephthalate; adding the reaction solution to a precipitation solvent to precipitate a solid product; acid washing and solid-liquid separation of the solid product to obtain a crude product; and then solvent purification of the crude product to separate the BHCT monomer from oligomers and / or polymers containing BHCT structural units to obtain high-purity bis(4-hydroxymethylcyclohexylmethyl) terephthalate.
[0022] In some typical embodiments, the reaction equation for the alcoholysis reaction of PET and CHDM in the method is as follows: .
[0023] The preparation method provided by this invention mainly includes the alcoholysis reaction of PET material with 1,4-cyclohexanediethanol under the action of an MXene-metal salt composite catalyst, precipitation, acid washing, filtration, and solvent purification steps. Through the above steps, high-purity BHCT monomer can be prepared and separated from PET material.
[0024] In some implementations, the PET material is waste PET, which refers to polyethylene terephthalate material derived from post-use recycling, production scraps, or other recycling systems.
[0025] Furthermore, the waste PET may include one or more of the following combinations: waste PET bottle flakes, waste PET film, waste PET fiber, PET scraps, and recycled PET granules, but is not limited to these.
[0026] In some preferred embodiments, the method further includes pretreatment of the PET material before it is added to the mixed reaction system. The pretreatment includes one or more of the following: washing, impurity removal, pulverization, and drying. Before use, waste PET can be pretreated by washing, removing labels and impurities, pulverizing, and drying, depending on the state of the raw materials, to reduce the impact of moisture and foreign impurities on the alcoholysis reaction.
[0027] In some embodiments, the MXene-metal salt composite catalyst is a combination of MXene material and a metal salt. The MXene material may be Ti3C2T. x Ti2CT x Mo2Ti2C3T x A combination of one or more of the following, preferably Ti3C2T xThe metal salt may include one or more of zinc acetate, manganese acetate, cobalt acetate, stannous octoate, and antimony acetate, preferably zinc acetate, but not limited thereto.
[0028] In some embodiments, the molar ratio of PET repeating units to 1,4-cyclohexanediethanol in the PET material is 1:(3~20), preferably 1:(4~10).
[0029] In some embodiments, the amount of MXene material used is 50 to 1000 ppm, preferably 100 to 500 ppm, based on the mass of PET material.
[0030] In some embodiments, the amount of the metal salt used is 300 to 3000 ppm based on the mass of the PET material, preferably 1000 to 2000 ppm.
[0031] In some embodiments, the alcoholysis reaction is carried out at a temperature of 200-260 °C for a duration of 0.5-6 h.
[0032] In some more specific embodiments, the method includes: disposing of waste PET, CHDM, and Ti3C2T x MXene reduces the influence of oxygen and moisture on the reaction process. Subsequently, under nitrogen purging conditions, the temperature is increased to induce alcoholysis between PET and CHDM, yielding a reaction solution containing BHCT.
[0033] In some embodiments, the nitrogen purging is a continuous nitrogen purging, and the nitrogen purging flow rate is 10~500 mL / min, preferably 50~200 mL / min.
[0034] In some preferred embodiments, after the alcoholysis reaction is completed, the resulting reaction solution containing BHCT is added to the precipitation solvent to precipitate the solid product containing the BHCT structure.
[0035] In some preferred embodiments, the precipitation solvent may include one or more of the following, but is not limited to: water, methanol, ethanol, isopropanol, acetone, butanone, ethyl acetate, toluene, xylene, dimethyl sulfoxide, tetrahydrofuran, etc.
[0036] In some preferred embodiments, the acid used for pickling includes one or more combinations of hydrochloric acid, sulfuric acid, phosphoric acid, acetic acid, citric acid, oxalic acid, etc., but is not limited to these.
[0037] In some preferred embodiments, the solvent used for solvent purification includes one or more combinations of methanol, ethanol, isopropanol, ethyl acetate, acetone, butanone, tetrahydrofuran, dimethyl sulfoxide, water, etc., but is not limited to these.
[0038] As another aspect of the technical solution of the present invention, it also relates to high-purity bis(4-hydroxymethylcyclohexylmethyl) terephthalate (BHCT) prepared by the above method.
[0039] Furthermore, the purity of the BHCT obtained by this invention is not less than 95%, the BHET content is not more than 3%, and the residual amount of metal elements in the metal catalyst is not more than 20 ppm.
[0040] In some embodiments, the purity of the BHCT is calculated quantitatively by nuclear magnetic resonance to be 95-98%.
[0041] In some embodiments, the content of BHET in the BHCT is calculated quantitatively as 0-3% by nuclear magnetic resonance.
[0042] In some embodiments, the residual amount of metal elements in the BHCT is not higher than 20 ppm as determined by ICP.
[0043] As another aspect of the technical solution of the present invention, it also relates to the application of the high-purity bis(4-hydroxymethylcyclohexylmethyl) terephthalate as a monomer raw material in the field of polyester or copolyester synthesis.
[0044] In some embodiments, the high-purity BHCT monomer obtained by the present invention can be used as a polymerization monomer for the preparation of polyesters or copolyesters. To verify the polymerization-grade performance of the BHCT monomer, the obtained BHCT monomer can be subjected to transesterification and polycondensation reactions with ethylene glycol, dimethyl terephthalate and / or other polyester monomers to prepare PETG copolyesters containing CHDM terephthalate structural units.
[0045] This invention reacts waste PET with CHDM under the action of an MXene-metal salt composite catalyst, converting the terephthalic acid structural units in the PET chain into terephthalic acid ester products with CHDM end groups. Unlike the route of direct polycondensation after alcoholysis of EG / CHDM, this invention does not use the mixed depolymerization products of BHET, BHCT, and oligomers as raw materials for subsequent polycondensation. Instead, it further regulates and separates the composition of the reaction products through composite catalysis, nitrogen purging, precipitation, acid washing, and solvent purification processes.
[0046] Among them, metal salts are beneficial for activating the ester carbonyl group of the PET backbone and promoting the attack of CHDM on the PET ester bond, MXene (such as Ti3C2T) xThe two-dimensional layered structure and surface end groups of BHCT facilitate the provision of interfacial contact regions for PET segments, CHDM, and metal salt active centers, thereby improving local mass transfer and dispersion in the high-viscosity CHDM / PET system and reducing the tendency of BHCT monomers to continue transesterification or oligomerization. Nitrogen purging helps reduce the residence of ethylene glycol byproducts in the system and decreases the formation of BHET and ethylene glycol-end-group-containing byproducts. The precipitation process helps separate the solid product containing the BHCT structure from unreacted CHDM, ethylene glycol, and some small molecule byproducts; the acid washing process helps reduce the residual metal elements from the catalyst; and the solvent purification process helps separate the BHCT monomer from oligomers and / or polymers containing BHCT structural units. Through the combination of the above steps, this invention can obtain BHCT monomers with high purity, low BHET content, and low metal element residue, transforming the recycled PET product from a mixture that can continue to polycondense into polyester monomers with a more defined composition and independent metering.
[0047] The technical solution of the present invention will be further described in detail below with reference to several preferred embodiments and accompanying drawings. This embodiment is implemented on the premise of the technical solution of the invention, and provides detailed implementation methods and specific operation processes. However, the protection scope of the present invention is not limited to the following embodiments.
[0048] Unless otherwise stated, all raw materials or reagents used in the examples are commercially available and can be purchased through commercial channels.
[0049] Example 1 This embodiment provides a method for preparing high-purity BHCT monomer from waste PET and CHDM, the specific steps of which include: Waste PET bottle flakes (30.00 g, 0.156 mol based on PET repeating units), CHDM (225.1 g, 1.561 mol), anhydrous zinc acetate (30 mg, 1000 ppm), and Ti3C2T were mixed. x MXene (9 mg, 300 ppm) was added to a reactor equipped with mechanical stirring, a nitrogen inlet, and a gas outlet.
[0050] Before the reaction, the air inside the reactor was replaced with nitrogen. Then, under nitrogen purging (nitrogen flow rate of 200 mL / min) and stirring conditions, the temperature was raised to 260 °C and the reaction was carried out for 1 h to allow PET and CHDM to undergo alcoholysis reaction, resulting in a hot reaction solution containing BHCT.
[0051] After the reaction was complete, the resulting hot reaction solution was added to the precipitation solvent, water, to precipitate the solid product containing the BHCT structure. The obtained solid product was washed with oxalic acid and then subjected to solid-liquid separation to obtain a crude product. Subsequently, the crude product was purified by solvent extraction using DMSO to obtain 56.2 g of BHCT monomer. The yield was 86.1% based on the molar amount of PET repeating units.
[0052] The BHCT monomer obtained in this embodiment, quantitatively calculated by NMR, had a purity of 97.1%, and BHET was not detected. ICP analysis showed a Zn residue of 9.7 ppm and a Ti residue of 5.0 ppm. The appearance of the obtained product is shown in [Figure showing appearance]. Figure 1 The proton NMR spectrum is shown below. Figure 2 DSC chart (see) Figure 3 The results of metal catalyst residues are shown in Table 1.
[0053] Table 1. Residual metal elements in the BHCT monomer obtained in Example 1 Example 2 Compared with Example 1, this embodiment is the same as Example 1 except that the molar ratio of PET repeating unit to CHDM is adjusted to 1:3.
[0054] After precipitation, oxalic acid washing, solid-liquid separation, and purification with DMSO solvent, 40.9 g of BHCT monomer was obtained. Based on the molar amount of PET repeating units, the yield of BHCT product was 62.6%.
[0055] The BHCT monomer obtained in this embodiment was quantitatively calculated to have a purity of 95.2% and a BHET content of 2.6% by NMR. ICP determination showed that the residual Zn content was 10.3 ppm and the residual Ti content was 5.4 ppm.
[0056] Example 3 Compared with Example 1, this embodiment is the same as Example 1 except that the molar ratio of PET repeating unit to CHDM is adjusted to 1:4.
[0057] After water precipitation, oxalic acid washing, solid-liquid separation, and purification with DMSO solvent, 46.9 g of BHCT monomer was obtained. Based on the molar amount of PET repeating units, the yield of BHCT product was 71.8%.
[0058] The BHCT monomer obtained in this embodiment was quantitatively calculated to have a purity of 95.4% and a BHET content of 2.1% by NMR. ICP determination showed that the residual Zn content was 10.5 ppm and the residual Ti content was 5.7 ppm.
[0059] Example 4 Compared with Example 1, this embodiment is the same as Example 1 except that the molar ratio of PET repeating unit to CHDM is adjusted to 1:6.
[0060] After water precipitation, oxalic acid washing, solid-liquid separation, and purification with DMSO solvent, 53.4 g of BHCT monomer was obtained. Based on the molar amount of PET repeating units, the yield of BHCT product was 81.8%.
[0061] The BHCT monomer obtained in this embodiment was quantitatively calculated to have a purity of 96.1% and a BHET content of 1.3% by NMR. ICP determination showed that the residual Zn content was 10.9 ppm and the residual Ti content was 5.2 ppm.
[0062] Example 5 Compared with Example 1, this embodiment is the same as Example 1 except that the molar ratio of PET repeating unit to CHDM is adjusted to 1:15.
[0063] After water precipitation, oxalic acid washing, solid-liquid separation, and purification with DMSO solvent, 61.6 g of BHCT monomer was obtained. The yield of BHCT product was 94.3% based on the molar amount of PET repeating units.
[0064] The BHCT monomer obtained in this embodiment was quantitatively calculated to have a purity of 97.3% by NMR, and BHET was not detected. ICP determination showed that the residual Zn content was 9.4 ppm and the residual Ti content was 4.9 ppm.
[0065] Example 6 Compared with Example 1, this embodiment is the same as Example 1 except that the molar ratio of PET repeating unit to CHDM is adjusted to 1:20.
[0066] After precipitation, oxalic acid washing, solid-liquid separation, and purification with DMSO solvent, 62.0 g of BHCT monomer was obtained. The yield of BHCT product was 95.0% based on the molar amount of PET repeating units.
[0067] The BHCT monomer obtained in this embodiment was quantitatively calculated to have a purity of 97.9% by NMR, and BHET was not detected. ICP determination showed that the residual Zn content was 8.9 ppm and the residual Ti content was 4.9 ppm.
[0068] Example 7 Compared with Example 1, this embodiment is the same as Example 1 except that the amount of zinc acetate is adjusted to 300 ppm based on the mass of waste PET bottle flakes.
[0069] After precipitation, oxalic acid washing, solid-liquid separation, and purification with DMSO solvent, 29.9 g of BHCT monomer was obtained. Based on the molar amount of PET repeating units, the yield of BHCT product was 45.8%.
[0070] The BHCT monomer obtained in this embodiment was quantitatively calculated to have a purity of 95.1% and a BHET content of 2.9% by NMR. ICP determination showed that the residual Zn content was 6.4 ppm and the residual Ti content was 5.1 ppm.
[0071] Example 8 Compared with Example 1, this embodiment is the same as Example 1 except that the amount of zinc acetate is adjusted to 1500 ppm based on the mass of waste PET bottle flakes.
[0072] After water precipitation, oxalic acid washing, solid-liquid separation, and purification with DMSO solvent, 57.3 g of BHCT monomer was obtained. The yield of BHCT product was 87.8% based on the molar amount of PET repeating units.
[0073] The BHCT monomer obtained in this embodiment was quantitatively calculated to have a purity of 97.2% by NMR, and BHET was not detected. ICP determination showed that the residual Zn content was 10.9 ppm and the residual Ti content was 5.3 ppm.
[0074] Example 9 Compared with Example 1, this embodiment is the same as Example 1 except that the amount of zinc acetate is adjusted to 2000 ppm based on the mass of waste PET bottle flakes.
[0075] After water precipitation, oxalic acid washing, solid-liquid separation, and purification with DMSO solvent, 58.9 g of BHCT monomer was obtained. The yield of BHCT product was 90.2% based on the molar amount of PET repeating units.
[0076] The BHCT monomer obtained in this embodiment was quantitatively calculated to have a purity of 97.1% by NMR, and BHET was not detected. ICP determination showed that the residual Zn content was 11.6 ppm and the residual Ti content was 5.0 ppm.
[0077] Example 10 Compared with Example 1, this embodiment is the same as Example 1 except that the amount of zinc acetate is adjusted to 3000 ppm based on the mass of waste PET bottle flakes.
[0078] After precipitation, oxalic acid washing, solid-liquid separation, and purification with DMSO solvent, 59.7 g of BHCT monomer was obtained. Based on the molar amount of PET repeating units, the yield of BHCT product was 91.4%.
[0079] The BHCT monomer obtained in this embodiment was quantitatively calculated to have a purity of 97.6% by NMR, and BHET was not detected. ICP determination showed that the residual Zn content was 12.3 ppm and the residual Ti content was 5.7 ppm.
[0080] Example 11 Compared with Example 1, this embodiment differs from Example 1 except for Ti3C2T. x Except for adjusting the MXene dosage to 50 ppm based on the mass of waste PET bottle flakes, the remaining steps are the same as in Example 1.
[0081] After precipitation, oxalic acid washing, solid-liquid separation, and purification with DMSO solvent, 44.5 g of BHCT monomer was obtained. Based on the molar amount of PET repeating units, the yield of BHCT product was 68.2%.
[0082] The BHCT monomer obtained in this embodiment was quantitatively calculated to have a purity of 95.1% by NMR, and BHET was not detected. ICP determination showed that the residual Zn content was 10.1 ppm and the residual Ti content was 2.9 ppm.
[0083] Example 12 Compared with Example 1, this embodiment differs from Example 1 except for Ti3C2T. x Except for adjusting the MXene dosage to 100 ppm based on the mass of waste PET bottle flakes, the remaining steps are the same as in Example 1.
[0084] After precipitation, oxalic acid washing, solid-liquid separation, and purification with DMSO solvent, 49.9 g of BHCT monomer was obtained. Based on the molar amount of PET repeating units, the yield of BHCT product was 76.4%.
[0085] The BHCT monomer obtained in this embodiment was quantitatively calculated to have a purity of 96.5% by NMR, and BHET was not detected. ICP determination showed that the residual Zn content was 9.1 ppm and the residual Ti content was 4.3 ppm.
[0086] Example 13 Compared with Example 1, this embodiment differs from Example 1 except for Ti3C2T. x Except for adjusting the MXene dosage to 500 ppm based on the mass of waste PET bottle flakes, the remaining steps are the same as in Example 1.
[0087] After precipitation, oxalic acid washing, solid-liquid separation, and purification with DMSO solvent, 54.5 g of BHCT monomer was obtained. Based on the molar amount of PET repeating units, the yield of BHCT product was 83.5%.
[0088] The BHCT monomer obtained in this embodiment was quantitatively calculated to have a purity of 95.3% by NMR, and BHET was not detected. ICP determination showed that the residual Zn content was 9.7 ppm and the residual Ti content was 7.3 ppm.
[0089] Example 14 Compared with Example 1, this embodiment differs from Example 1 except for Ti3C2T. x Except for adjusting the MXene dosage to 1000 ppm based on the mass of waste PET bottle flakes, the remaining steps are the same as in Example 1.
[0090] After precipitation, oxalic acid washing, solid-liquid separation, and purification with DMSO solvent, 46.9 g of BHCT monomer was obtained. Based on the molar amount of PET repeating units, the yield of BHCT product was 71.8%.
[0091] The BHCT monomer obtained in this embodiment was quantitatively calculated to have a purity of 94.4% by NMR, and BHET was not detected. ICP determination showed that the residual Zn content was 9.5 ppm and the residual Ti content was 23.3 ppm.
[0092] Example 15 Compared with Example 1, this embodiment differs from Example 1 except for Ti3C2T. x MXene replaced with an equivalent quality Ti2CT x Except for MXene, the remaining steps are the same as in Example 1.
[0093] After precipitation, oxalic acid washing, solid-liquid separation, and purification with DMSO solvent, approximately 52.6 g of BHCT monomer was obtained. Based on the molar amount of PET repeating units, the BHCT product yield was 80.5%. Quantitative analysis of the obtained BHCT monomer by NMR showed a purity of 96.3% and a BHET content of 0.8%. ICP analysis revealed a Zn residue of 10.9 ppm and a Ti residue of 9.8 ppm.
[0094] Example 16 Compared with Example 1, this embodiment differs from Example 1 except for Ti3C2T. x MXene was replaced with an equal mass of Mo2Ti2C3T x Except for MXene, the remaining steps are the same as in Example 1.
[0095] After precipitation, oxalic acid washing, solid-liquid separation, and purification with DMSO solvent, approximately 50.1 g of BHCT monomer was obtained. Based on the molar amount of PET repeating units, the BHCT product yield was 76.8%. Quantitative analysis of the obtained BHCT monomer by NMR showed a purity of 95.7% and a BHET content of 1.5%. ICP analysis revealed a Zn residue of 13.1 ppm and a Ti residue of 4.7 ppm.
[0096] Example 17 Compared with Example 1, this embodiment is the same as Example 1 except that the reaction temperature is adjusted to 230 ℃ and the reaction time is adjusted to 0.5 h.
[0097] After precipitation, oxalic acid washing, solid-liquid separation, and purification with DMSO solvent, 34.3 g of BHCT monomer was obtained. Based on the molar amount of PET repeating units, the yield of BHCT product was 52.6%.
[0098] The BHCT monomer obtained in this embodiment was quantitatively calculated by NMR to have a purity of 95.0% and a BHET content of 2.3%. ICP determination showed that the residual Zn content was 10.0 ppm and the residual Ti content was 5.2 ppm.
[0099] Example 18 Compared with Example 1, this embodiment is the same as Example 1 except that the reaction temperature is adjusted to 200 ℃ and the reaction time is adjusted to 6 h.
[0100] After precipitation, oxalic acid washing, solid-liquid separation, and purification with DMSO solvent, 48.7 g of BHCT monomer was obtained. Based on the molar amount of PET repeating units, the yield of BHCT product was 74.6%.
[0101] The BHCT monomer obtained in this embodiment was quantitatively calculated to have a purity of 95.7% and a BHET content of 2.6% by NMR. ICP determination showed that the residual Zn content was 11.9 ppm and the residual Ti content was 4.7 ppm.
[0102] Example 19 Compared with Example 1, this embodiment is the same as Example 1 except that the precipitation solvent water is replaced with xylene.
[0103] Specifically, after the reaction was completed, the resulting hot reaction solution containing BHCT was added to the precipitation solvent xylene, causing the solid product containing the BHCT structure to precipitate. The obtained solid product was washed with oxalic acid and then subjected to solid-liquid separation to obtain a crude product. Subsequently, the crude product was purified by solvent DMSO to obtain 35.6 g of BHCT monomer. Based on the molar amount of PET repeating units, the yield of BHCT product was 54.5%.
[0104] The BHCT monomer obtained in this embodiment was quantitatively calculated to have a purity of 96.4% and a BHET content of 1.3% by NMR. ICP determination showed that the residual Zn content was 9.5 ppm and the residual Ti content was 8.2 ppm.
[0105] Example 20 Compared with Example 1, this embodiment is the same as Example 1 except that the oxalic acid pickling is replaced with citric acid pickling.
[0106] After precipitation, citric acid washing, solid-liquid separation, and purification with DMSO solvent, 55.7 g of BHCT monomer was obtained. Based on the molar amount of PET repeating units, the yield of BHCT product was 85.3%.
[0107] The BHCT monomer obtained in this embodiment was quantitatively calculated to have a purity of 97.2% by NMR, and BHET was not detected. ICP determination showed that the residual Zn content was 7.5 ppm and the residual Ti content was 5.1 ppm.
[0108] Example 21 Compared with Example 1, this embodiment is the same as Example 1 except that the DMSO used for solvent purification is replaced with ethanol.
[0109] After precipitation, oxalic acid washing, solid-liquid separation, and purification with ethanol solvent, 57.3 g of BHCT monomer was obtained. Based on the molar amount of PET repeating units, the yield of BHCT product was 87.8%.
[0110] The BHCT monomer obtained in this embodiment was quantitatively calculated to have a purity of 97.4% by NMR, and BHET was not detected. ICP determination showed that the residual Zn content was 10.7 ppm and the residual Ti content was 5.3 ppm.
[0111] Example 22 Compared with Example 1, this embodiment is the same as Example 1 except that the DMSO used for solvent purification is replaced with an ethanol / DMSO mixed solvent and the nitrogen purging flow rate is 10 mL / min.
[0112] After precipitation, oxalic acid washing, solid-liquid separation, and purification with an ethanol / DMSO mixed solvent, 57.0 g of BHCT monomer was obtained. The yield of BHCT product was 87.3% based on the molar amount of PET repeating units.
[0113] The BHCT monomer obtained in this embodiment was quantitatively calculated to have a purity of 96.8% by NMR, and BHET was not detected. ICP analysis showed that the residual Zn content was 11.2 ppm and the residual Ti content was 5.8 ppm.
[0114] Example 23 Compared with Example 1, this embodiment is the same as Example 1 except that the DMSO used for solvent purification is replaced with a mixed solvent of ethanol / acetone and the nitrogen purging flow rate is 50 mL / min.
[0115] After precipitation, oxalic acid washing, solid-liquid separation, and purification with an ethanol / acetone mixed solvent, 56.5 g of BHCT monomer was obtained. The yield of BHCT product was 86.5% based on the molar amount of PET repeating units.
[0116] The BHCT monomer obtained in this embodiment was quantitatively calculated to have a purity of 97.2% by NMR, and BHET was not detected. ICP determination showed that the residual Zn content was 9.4 ppm and the residual Ti content was 5.1 ppm.
[0117] Example 24 Compared with Example 1, this embodiment is the same as Example 1 except that the DMSO used for solvent purification is replaced with a DMSO / acetone mixed solvent and the nitrogen purging flow rate is 500 mL / min.
[0118] After precipitation, oxalic acid washing, solid-liquid separation, and purification with a DMSO / acetone mixed solvent, 56.8 g of BHCT monomer was obtained. The yield of BHCT product was 87.0% based on the molar amount of PET repeating units.
[0119] The BHCT monomer obtained in this embodiment was quantitatively calculated to have a purity of 96.9% by NMR, and BHET was not detected. ICP determination showed that the residual Zn content was 9.8 ppm and the residual Ti content was 5.9 ppm.
[0120] Example 25 Compared with Example 1, this embodiment is the same as Example 1 except that the waste PET bottle flakes are replaced with recycled PET granules.
[0121] After precipitation, oxalic acid washing, solid-liquid separation, and purification with DMSO solvent, 55.8 g of BHCT monomer was obtained. Based on the molar amount of PET repeating units, the yield of BHCT product was 85.5%.
[0122] The BHCT monomer obtained in this embodiment was quantitatively calculated to have a purity of 96.7% by NMR, and BHET was not detected. ICP determination showed that the residual Zn content was 11.0 ppm and the residual Ti content was 6.2 ppm.
[0123] Example 26 Compared with Example 1, this embodiment is the same as Example 1 except that the waste PET bottle flakes are replaced with PET scraps.
[0124] After precipitation, oxalic acid washing, solid-liquid separation, and purification with DMSO solvent, 56.1 g of BHCT monomer was obtained. The yield of BHCT product was 85.9% based on the molar amount of PET repeating units.
[0125] The BHCT monomer obtained in this embodiment was quantitatively calculated to have a purity of 97.3% by NMR, and BHET was not detected. ICP determination showed that the residual Zn content was 10.6 ppm and the residual Ti content was 7.0 ppm.
[0126] Example 27 Compared with Example 1, this embodiment is the same as Example 1 except that anhydrous zinc acetate is replaced with antimony acetate.
[0127] After precipitation, oxalic acid washing, solid-liquid separation, and purification with DMSO solvent, 53.1 g of BHCT monomer was obtained. The yield of BHCT product was 81.3% based on the molar amount of PET repeating units.
[0128] The BHCT monomer obtained in this embodiment was found to have a purity of 96.0% by nuclear magnetic resonance quantification, and no BHET was detected. ICP analysis showed that the residual Sb content was 17.4 ppm and the residual Ti content was 5.1 ppm.
[0129] Comparative Example 1 Compared with Example 1, this comparative example does not contain Ti3C2T. x Except for MXene, the remaining steps are the same as in Example 1.
[0130] After precipitation, oxalic acid washing, solid-liquid separation, and purification with DMSO solvent, 46.2 g of BHCT monomer was obtained. Based on the molar amount of PET repeating units, the yield of BHCT product was 70.8%.
[0131] The BHCT monomer obtained in this comparative example was quantitatively calculated by NMR to have a purity of 93.6% and a BHET content of 5.0%. ICP analysis showed a Zn residue of 10.6 ppm and no Ti was detected.
[0132] The DSC charts of the BHCT products prepared in Example 1 and the comparative example are shown below. Figure 3 The melting peak of the product obtained in Example 1 was relatively simple, while that of Comparative Example 1 showed a shoulder peak. Combined with the NMR results, this indicates that Ti3C2T... x MXene helps reduce BHET residue and improve the selectivity and purity of BHCT.
[0133] Comparative Example 2 Compared with Example 1, this comparative example is identical to Example 1 except that anhydrous zinc acetate is not added.
[0134] After precipitation, oxalic acid washing, solid-liquid separation, and purification with DMSO solvent, 26.1 g of BHCT monomer was obtained. Based on the molar amount of PET repeating units, the yield of BHCT product was 40.2%.
[0135] The BHCT monomer obtained in this comparative example was quantitatively calculated by NMR to have a purity of 95.3% and a BHET content of 2.6%. ICP determination showed a Ti residue of 8.6 ppm and no Zn was detected.
[0136] Compared to Example 1, this comparative example only uses Ti3C2T x When MXene was applied, the BHCT monomer yield decreased significantly, indicating that Ti3C2T x When used alone, MXene has limited catalytic effect on the depolymerization of PET.
[0137] Comparative Example 3 Compared with Example 1, this comparative example is identical to Example 1 except that the obtained solid product is not subjected to oxalic acid washing.
[0138] Specifically, after the reaction was completed, the resulting hot reaction solution was added to the precipitation solvent, water, to precipitate the solid product containing the BHCT structure. The obtained solid product was not washed with oxalic acid but directly subjected to solid-liquid separation to obtain the crude product. Subsequently, the crude product was purified using DMSO to obtain 56.0 g of BHCT monomer. Based on the molar amount of PET repeating units, the yield of the BHCT product was 85.8%.
[0139] The BHCT monomer obtained in this comparative example was quantitatively calculated to have a purity of 96.9% by NMR, and BHET was not detected. ICP analysis showed that the residual Zn content was 82 ppm and the residual Ti content was 17.0 ppm.
[0140] Compared with Example 1, the residual Zn content in the product obtained in this comparative example was significantly increased, indicating that acid washing treatment is beneficial to reducing the residual metal catalyst in BHCT monomer.
[0141] Comparative Example 4 Compared with Example 1, this comparative example is identical to Example 1 except that the crude product obtained after acid washing is not purified by solvent DMSO.
[0142] Specifically, after the reaction was completed, the resulting hot reaction solution was added to the precipitation solvent, water, to precipitate the solid product containing the BHCT structure. The obtained solid product was washed with oxalic acid and then subjected to solid-liquid separation to obtain the crude product. The crude product was not purified by DMSO solvent but was directly dried to obtain 60.9 g of crude product.
[0143] The product obtained in this comparative example was quantitatively calculated by NMR, and the purity of BHCT was 91.1%, and the content of BHET was 0.7%. ICP determination showed that the residual Zn content was 13.4 ppm and the residual Ti content was 79.0 ppm.
[0144] Compared with Example 1, the purity of BHCT in the product obtained in this comparative example decreased, while the residual Ti content increased, indicating that solvent purification is beneficial for separating BHCT monomers, BHCT oligomers, and Ti3C2T. x MXene, thereby improving the purity of BHCT monomer.
[0145] Comparative Example 5 Compared with Example 1, this comparative example is the same as Example 1 except that continuous nitrogen purging is not performed during the alcoholysis reaction, and nitrogen is used to replace the air in the reactor and maintain a static nitrogen atmosphere before the reaction.
[0146] Specifically, waste PET bottle flakes, CHDM, anhydrous zinc acetate, and Ti3C2T are used. x MXene was added to a reactor equipped with mechanical stirring, a nitrogen inlet, and a gas outlet. Before the reaction, the air inside the reactor was purged with nitrogen. Subsequently, continuous nitrogen purging was stopped, and the temperature was raised to 260°C under a static nitrogen atmosphere and stirring conditions. The reaction was carried out for 1 h to allow PET and CHDM to undergo alcoholysis, yielding a hot reaction solution containing BHCT.
[0147] After the reaction was completed, 40.1 g of BHCT monomer was obtained after precipitation, oxalic acid washing, solid-liquid separation, and purification with DMSO solvent. The yield of BHCT product was 61.4% based on the molar amount of PET repeating units.
[0148] The BHCT monomer obtained in this comparative example was quantitatively calculated by NMR, and the purity of BHCT was 92.5%, and the BHET content was 6.1%. ICP determination showed that the residual Zn content was 14.1 ppm and the residual Ti content was 5.9 ppm.
[0149] Compared with Example 1, this comparative example did not undergo continuous nitrogen purging during the reaction process, resulting in a decrease in the yield and purity of BHCT monomer in the obtained product. This indicates that nitrogen purging helps reduce the residence of ethylene glycol byproducts in the reaction system, inhibits the formation of BHET, and thus improves the yield and purity of BHCT monomer.
[0150] Application Validation Example 1 This application verification example illustrates that the high-purity BHCT monomer prepared by this invention can be used as a polymer monomer for the preparation of PETG copolyester.
[0151] Dimethyl terephthalate (DMT) (15.0 g, 0.077 mol), ethylene glycol (EG) (10.5 g, 0.169 mol), BHCT monomer prepared in Example 1 (8.0 g, 0.019 mol), and anhydrous zinc acetate (9 mg, 300 ppm, based on the total mass of DMT and BHCT) were added to a polymerization reactor equipped with mechanical stirring, a nitrogen inlet, a condenser, and a methanol receiving device. The BHCT monomer was metered according to its CHDM structural units, and the feed design was intended to prepare a PETG copolyester with an EG / CHDM molar ratio of approximately 60 / 40.
[0152] Under nitrogen protection, the system was heated to 150 °C to melt and mix the materials uniformly. The temperature was then further increased to 180–210 °C to carry out the transesterification reaction, and the methanol produced was collected.
[0153] After the transesterification reaction was completed, antimony trioxide (Sb₂O₃) (16 mg, 500 ppm) and trimethyl phosphate stabilizer (8 mg, 300 ppm) were added to the reaction system, and the mixture was stirred and mixed. Then, the temperature was gradually increased to 280°C and the system pressure was gradually decreased to carry out the polycondensation reaction.
[0154] After polycondensation, the vacuum was released, and the product was discharged and cooled under nitrogen protection to obtain PETG copolyester. The yield of the obtained PETG copolyester was approximately 95.0% based on the theoretical polymer mass. The 1H NMR spectrum of the obtained PETG copolyester is shown below. Figure 4 After integration calculation, the corresponding EG / CHDM molar ratio in the obtained PETG is approximately 55.4 / 44.6. GPC testing shows that the number-average molecular weight of the obtained PETG is... M n 2.4 × 10 4 g / mol, weight-average molecular weight M w 4.2×10 4 g / mol, molecular weight distribution M w / M n The value is 1.75. The above results indicate that the BHCT monomer obtained in this invention can be used as a polymerization-grade monomer for the preparation of PETG copolyesters.
[0155] Quantitative analysis using nuclear magnetic resonance (NMR): An AVANCE NEO 600 NMR spectrometer (600 MHz) was used with chloroform as solvent and TMS as internal standard. For the BHCT monomer sample, the purity of BHCT monomer and the content of BHET were calculated based on the integrated areas of the characteristic peaks of BHCT and BHET. The products obtained in Example 1 and Comparative Example 1... 1 See the H NMR spectrum. Figure 2For PETG copolyester samples, the same testing conditions were used. 1 ¹H NMR analysis was performed, and the content of CHDM structural units in PETG was calculated based on the integrated areas of the characteristic peaks corresponding to ethylene glycol and CHDM structural units. The PETG copolyester obtained in Example 1 was then applied for verification. 1 See the H NMR spectrum. Figure 4 .
[0156] Molecular weight characterization: The molecular weight of the PETG copolyester obtained in Application Validation Example 1 was determined using an Agilent 1260 Infinity II gel permeation chromatograph. Chloroform was used as the mobile phase. The number-average molecular weight, weight-average molecular weight, and molecular weight distribution of the samples were obtained by gel permeation chromatography.
[0157] Melt behavior characterization: The melt behavior of the prepared BHCT monomer was characterized using a Diamond DSC3 differential scanning calorimeter. The sample weight was approximately 5 mg. First, the polyester was heated from -10℃ to 200℃ at a heating rate of 60℃ / min to eliminate thermal history, then cooled to -10℃ at a cooling rate of 10℃ / min. Then, it was heated to 200℃ at a heating rate of 10℃ / min to obtain the sample scanning curve. The results are shown below. Figure 3 As shown in the figure, the DSC curves of the products of Embodiment 1 and Comparative Example 1 of the present invention are displayed.
[0158] Metal catalyst residue test: The metal element content in the sample was determined using a SPECTRO ARCOS inductively coupled plasma atomic emission spectrometer. The results are shown in Table 1, which represents the metal content of the product in Example 1 of this invention.
[0159] In addition, the inventors of this case also conducted experiments with other raw materials, process operations, and process conditions described in this specification, referring to the aforementioned embodiments, and obtained relatively ideal results in all cases.
[0160] It should be understood that the technical solutions of the present invention are not limited to the specific embodiments described above. Any technical modifications made to the technical solutions of the present invention without departing from the spirit and scope of the claims are within the scope of protection of the present invention.
Claims
1. A method for preparing high-purity bis(4-hydroxymethylcyclohexylmethyl) terephthalate from PET, characterized in that, include: Under inert gas purging, a mixed reaction system containing PET material, 1,4-cyclohexanediethanol and MXene-metal salt composite catalyst is subjected to alcoholysis reaction to obtain a reaction solution containing bis(4-hydroxymethylcyclohexylmethyl) terephthalate. The reaction solution is brought into contact with the precipitating solvent to obtain a solid product, which is then purified to obtain high-purity bis(4-hydroxymethylcyclohexylmethyl) terephthalate.
2. The method according to claim 1, characterized in that: The MXene-metal salt composite catalyst is a combination of MXene material and metal salt, wherein the MXene material includes Ti3C2T. x Ti2CT x Mo2Ti2C3T x One or more combinations thereof, preferably Ti3C2T x The metal salt includes one or more combinations of zinc acetate, manganese acetate, cobalt acetate, stannous octoate, and antimony acetate, preferably zinc acetate.
3. The method according to claim 1, characterized in that: The PET material is waste PET, preferably including one or more of the following: waste PET bottle flakes, waste PET film, waste PET fiber, PET scraps, and recycled PET granules. And / or, the method further includes: the PET material is pretreated before being added to the mixing reaction system, the pretreatment including one or more of the following: washing, impurity removal, pulverization, and drying.
4. The method according to claim 1, characterized in that: The molar ratio of PET repeating units to 1,4-cyclohexanediethanol in the PET material is 1:(3~20), preferably 1:(4~10).
5. The method according to claim 2, characterized in that: The amount of MXene material used is 50-1000 ppm based on the mass of PET material, preferably 100-500 ppm; And / or, the amount of the metal salt used is 300 to 3000 ppm based on the mass of the PET material, preferably 1000 to 2000 ppm.
6. The method according to claim 1, characterized in that: The alcoholysis reaction is carried out at a temperature of 200-260 °C for 0.5-6 h.
7. The method according to claim 1, characterized in that, include: PET material, 1,4-cyclohexanediethanol, and MXene-metal salt composite catalyst were mixed and subjected to alcoholysis under nitrogen purging to obtain a reaction solution containing bis(4-hydroxymethylcyclohexylmethyl) terephthalate. The reaction solution was added to a precipitation solvent to precipitate a solid product. The solid product was then acid-washed and subjected to solid-liquid separation to obtain a crude product. The crude product was then purified by solvent separation to obtain high-purity bis(4-hydroxymethylcyclohexylmethyl) terephthalate.
8. The method according to claim 7, characterized in that: The nitrogen purging is a continuous nitrogen purging, with a nitrogen flow rate of 10~500 mL / min, preferably 50~200 mL / min; And / or, the precipitation solvent includes one or more combinations of water, methanol, ethanol, isopropanol, acetone, butanone, ethyl acetate, toluene, xylene, dimethyl sulfoxide, and tetrahydrofuran; And / or, the acid used for pickling includes one or more combinations of hydrochloric acid, sulfuric acid, phosphoric acid, acetic acid, citric acid, and oxalic acid; And / or, the solvent used for solvent purification includes one or more combinations of methanol, ethanol, isopropanol, ethyl acetate, acetone, butanone, tetrahydrofuran, dimethyl sulfoxide, and water.
9. High-purity bis(4-hydroxymethylcyclohexylmethyl) terephthalate prepared by the method according to any one of claims 1 to 8; Preferably, the high-purity bis(4-hydroxymethylcyclohexylmethyl) terephthalate has a purity of not less than 95%, a content of bis(hydroxyethyl) terephthalate of not more than 3%, and a residual metal element content of not more than 20 ppm.
10. The application of the high-purity bis(4-hydroxymethylcyclohexylmethyl) terephthalate as described in claim 9 as a monomer raw material in the field of polyester or copolyester synthesis.
Citation Information
Patent Citations
PETG (polyethylene terephthalate glycol) and method for preparing PETG from waste PET polyester
CN114853991A