A sulfide fluorenyl high refractive acrylate monomer, its preparation method and application

By preparing sulfide-based fluorene-based high-refractive-index acrylate monomers, the shortcomings of existing resin systems in terms of light utilization efficiency and mechanical properties have been overcome, achieving a balance between high refractive index and excellent mechanical properties, making it suitable for high-end optical brightening films.

CN123106491APending Publication Date: 2026-11-17SHANGHAI RES INST OF CHEM IND CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611314994.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-27
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing acrylate resin systems have encountered bottlenecks in improving light utilization efficiency, making it difficult to increase the refractive index while ensuring mechanical properties. Furthermore, the preparation process of existing high refractive index resins is complex or has a negative impact on mechanical properties.

Method used

A sulfide-based fluorene-containing high-refractive-index acrylate monomer was developed. Difunctional or trifunctional sulfide-containing fluorene-containing acrylate monomers were prepared by click reaction of mercaptoolefins and acyl chloride esterification reaction. The molecular structure was optimized by combining specific solvents and acid-binding agents to improve the refractive index and mechanical properties.

Benefits of technology

It achieves a balance between high refractive index and excellent mechanical properties, with a simple and efficient monomer synthesis route, suitable for high-end optical brightening films, improving light utilization efficiency and material stability, and solving the problem of insufficient material performance in existing technologies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106491A_ABST
    Figure CN123106491A_ABST
Patent Text Reader

Abstract

This invention relates to a fluorene-based high-refractive-index acrylate monomer, its preparation method, and its applications. The monomer molecule contains both fluorene and thioether groups and is prepared via efficient organic reactions such as the Williamson reaction, mercaptoolefin click reaction, and acyl chloride esterification reaction under mild conditions. The resulting monomers all have refractive indices greater than 1.58. Incremental film precursor adhesives prepared based on this monomer cure rapidly and exhibit excellent mechanical properties. This invention provides an efficient and reliable preparation strategy for the synthesis of high-refractive-index monomers used in high-end optical brightening films.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of acrylate monomer technology, and in particular to a sulfide-based fluorene-based high-refractive-index acrylate monomer, its preparation method, and its application. Background Technology

[0002] Liquid crystal displays (LCDs) are widely used in various electronic devices due to their high image quality and low power consumption. As market demands for display quality continue to rise, the backlight module, a key component of LCDs, faces greater challenges in achieving high optical efficiency and image uniformity. The brightness enhancement film, as the core optical film for improving the brightness of the front of the backlight module, directly determines the final energy efficiency and visual experience of the display.

[0003] Traditional brightness enhancement films mostly use acrylate resin systems, achieving light concentration and brightness enhancement through the refraction and total internal reflection principles of optical cooling structures. However, as display technology advances towards low power consumption and ultra-thin designs, existing material systems have reached their application bottleneck in terms of refractive index, making it difficult to further improve light utilization efficiency while maintaining mechanical properties. Increasing the refractive index of the resin monomers is an effective way to break through the brightness gain efficiency of brightness enhancement films.

[0004] Against this backdrop, the development of high-refractive-index monomers has become a research hotspot in the industry. Patent CN 114621429A reports a class of fluorene-based polyethylene glycol acrylate monomers. These monomers are easy to prepare and mass-produce, and exhibit excellent material adhesion. However, the presence of long EO segments in their molecular structure may negatively impact their mechanical properties. CN117659469A describes a high-refractive-index resin modified with sulfur-containing organic compounds. This resin achieves a refractive index exceeding 1.60, but requires two curing operations during product preparation. Summary of the Invention

[0005] The purpose of this invention is to provide a sulfide-based fluorene-based high-refractive-index acrylate monomer, its preparation method, and its application, which combines high refractive index with excellent mechanical properties.

[0006] The objective of this invention can be achieved through the following technical solution: a sulfide-based fluorene-based high-refractive-index acrylate monomer, wherein the monomer is a difunctional sulfide-containing fluorene-based acrylate monomer or a trifunctional sulfide-containing fluorene-based acrylate monomer; The difunctional thiofluorenyl acrylate monomer has the following general chemical structural formula: in, for or R1 is or ; The trifunctional sulfur-containing fluorene acrylate monomer has the following general chemical structural formula: in, for , , or R2 is or ; in, n The quantity is 1-4.

[0007] A method for preparing the above-mentioned sulfide-based fluorenyl high-refractive-index acrylate monomer involves mixing a di-functional sulfide-containing fluorenyl intermediate or a tri-functional sulfide-containing fluorenyl intermediate with an acid-binding agent and a polymerization inhibitor, dissolving the mixture in a solvent, and then adding an acyl chloride compound to react and obtain the di-functional sulfide-containing fluorenyl acrylate monomer or the tri-functional sulfide-containing fluorenyl acrylate monomer. The structural formula of the difunctional sulfofluorene intermediate is as follows: The structural formula of the trifunctional sulfur-containing fluorene intermediate is: .

[0008] Preferably, the preparation methods of the difunctional sulfur-containing fluorene intermediate and the trifunctional sulfur-containing fluorene intermediate include thermal initiation or photoinitiation.

[0009] More preferably, the thermal initiation method includes the following steps: Disubstituted thiols or trisubstituted thiols are dissolved in a solvent with monoallyl bisphenol fluorene, a thermal initiator is added, and the reaction system is heated to the solvent reflux temperature under a protective atmosphere. The substrate undergoes a thermally initiated thiol-ene click reaction to obtain the difunctional thiol-containing fluorene intermediate or the trifunctional thiol-containing fluorene intermediate. The photoinitiation method includes the following steps: A solvent and a photoinitiator are added to a disubstituted or trisubstituted thiol and monoallyl bisphenol fluorene. The reaction system is placed in an ultraviolet reactor under a protective atmosphere, and the substrate undergoes a photo-initiated thiol-ene click reaction to obtain the difunctional or trifunctional thiol-containing fluorene intermediate.

[0010] More preferably, the protective atmosphere is a nitrogen atmosphere.

[0011] More preferably, the disubstituted thiol is 1,3-propanedithiol or 4,4-thiodiphenylthiol.

[0012] More preferably, the trisubstituted thiol is polythiol 504, mesitylecithin, 1,1-tris(mercaptomethyl)undecane or trimethylolpropane-tris(3-mercaptopropionate).

[0013] More preferably, the monoallyl bisphenol fluorene has the following structural formula: .

[0014] More preferably, the method for preparing the monoallyl bisphenol fluorene includes the following steps: Bisphenol fluorene and basic inorganic salts were placed in a reactor, a solvent was added, and the mixture was heated and stirred to dissolve. Monohalogenated terminal olefins were dissolved in the same solvent, and the monohalogenated terminal olefin solution was slowly added dropwise to the system.

[0015] More preferably, the monohalogenated terminal olefin is selected from one or more of 1-chloropropene, 1-bromopropene, 1-bromobutene, 1-iodopropene, and 1-bromohexene.

[0016] More preferably, the solvent used to prepare the monoallyl bisphenol fluorene is one or more of acetonitrile, acetone, dichloromethane, chloroform, and ethyl acetate, preferably acetone or acetonitrile.

[0017] More preferably, the alkaline inorganic salt is selected from one or more of sodium carbonate, potassium carbonate, and cesium carbonate, with potassium carbonate being the most preferred.

[0018] More preferably, the solvent used to prepare the difunctional sulfonyl fluorene intermediate or the trifunctional sulfonyl fluorene intermediate is selected from one or more of acetonitrile, acetone, dichloromethane, chloroform, and ethyl acetate.

[0019] More preferably, the solvent used to prepare the difunctional sulfur-containing fluorene intermediate or the trifunctional sulfur-containing fluorene intermediate is dichloromethane.

[0020] More preferably, the thermal initiator is selected from one or more of azobisisobutyronitrile, azobisisoheptanenitrile, benzoyl peroxide, dicumyl peroxide, di-tert-butyl peroxide, benzoyl tert-butyl peroxide, tert-butyl peroxypentanoate, and diisopropyl peroxide.

[0021] More preferably, the thermal initiator is azobisisobutyronitrile (AIBN).

[0022] More preferably, the photoinitiator is selected from one or more of benzophenone, benzoyl peroxide, 2-hydroxy-2-methyl-1-phenyl-1-propanone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, ethyl 2,4,6-trimethylbenzoylphosphonate, 1-hydroxycyclohexylphenyl ketone, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, 2-methyl-1-(4-methylthiophenyl)-2-morpholino-1-propanone, 2-isopropylthioxanthone, sodium benzophenone-4-sulfonate, 2-hydroxy-4-(2-hydroxyethoxy)-2-methylphenylpropanone, 2-ethylanthraquinone, 4-methylbenzophenone, and tetraethylmichalcohol.

[0023] More preferably, the photoinitiator is 1-hydroxycyclohexylphenyl ketone or benzophenone. The photoinitiator used to prepare the difunctional sulfonyl fluorene intermediate is preferably 1-hydroxycyclohexylphenyl ketone, and the photoinitiator used to prepare the trifunctional sulfonyl fluorene intermediate is preferably benzophenone.

[0024] More preferably, in the thermal initiation method, the heating temperature is 36~150℃ and the time is 12~26 h.

[0025] More preferably, in the thermal initiation method, the molar ratio of disubstituted thiols, monoallyl bisphenol fluorene, and thermal initiator is 1:(2-4):(0.01-1).

[0026] More preferably, in the thermal initiation method, the molar ratio of disubstituted thiols, monoallyl bisphenol fluorene, and thermal initiator is 1:2.5:0.02.

[0027] More preferably, in the thermal initiation method, the molar ratio of trisubstituted thiol, monoallyl bisphenol fluorene, and thermal initiator is 1:(3-6):(0.01-1).

[0028] More preferably, in the thermal initiation method, the molar ratio of trisubstituted thiol, monoallyl bisphenol fluorene, and thermal initiator is 1:3.5:0.02.

[0029] More preferably, in the photoinitiation method, the ultraviolet light wavelength is 365 nm and the power is 20 watts.

[0030] More preferably, in the photoinitiation method, the molar ratio of disubstituted thiols, monoallyl bisphenol fluorene, and photoinitiator is 1:(2-5):(0.01-1).

[0031] More preferably, in the photoinitiation method, the molar ratio of disubstituted thiol, monoallyl bisphenol fluorene, and photoinitiator is 1:2.5:0.02.

[0032] More preferably, in the photoinitiation method, the molar ratio of trisubstituted thiol, monoallyl bisphenol fluorene, and photoinitiator is 1:(3-6):(0.01-1).

[0033] More preferably, in the photoinitiation method, the molar ratio of trisubstituted thiol, monoallyl bisphenol fluorene, and photoinitiator is 1:3.5:0.02.

[0034] Preferably, the preparation method of the difunctional sulfur-containing fluorene acrylate monomer includes the following steps: mixing the difunctional sulfur-containing fluorene intermediate with an acid-binding agent and a polymerization inhibitor, and dissolving it in a solvent; then adding acryloyl chloride / methacryloyl chloride under ice bath conditions, followed by heating and reflux reaction; after the reaction is completed, cooling, washing with water, and rotary evaporation to remove the solvent, thereby obtaining the difunctional sulfur-containing fluorene acrylate monomer, which is the target product.

[0035] Preferably, the preparation method of the trifunctional sulfur-containing fluorene acrylate monomer includes the following steps: the trifunctional sulfur-containing fluorene intermediate is mixed with an acid-binding agent and a polymerization inhibitor and dissolved in a solvent. Then, an acyl chloride compound is added under ice bath conditions, and the reaction is carried out at room temperature. After the reaction is completed, the organic phase is washed with water multiple times and decolorized by adsorption with activated carbon. After the solvent is removed by rotary evaporation, the trifunctional fluorene-containing acrylate resin monomer is obtained, which is the target product.

[0036] Preferably, the acid-binding agent is an inorganic or organic compound that can react with the hydrogen chloride generated during the process.

[0037] More preferably, the inorganic compound is a basic salt compound.

[0038] More preferably, the inorganic compound is selected from one or more of potassium carbonate, sodium carbonate, cesium carbonate, and sodium bicarbonate.

[0039] More preferably, the organic compound is a basic organic compound.

[0040] More preferably, the organic compound is selected from triethylamine, ethylenediamine, trimethylamine, pyridine, etc. N , N -One or more of alkylamide compounds.

[0041] More preferably, the acid-binding agent is triethylamine.

[0042] Preferably, the polymerization inhibitor is a compound that can prevent the self-polymerization of the product during the reaction heating.

[0043] More preferably, the polymerization inhibitor is selected from one or more of hydroquinones, p-methoxyphenol, phenothiazines, or p-tert-butylphenol.

[0044] More preferably, the polymerization inhibitor is hydroquinone.

[0045] Preferably, the acyl chloride compound is acryloyl chloride or methacryloyl chloride.

[0046] Preferably, the solvent used to prepare the difunctional fluorene-containing acrylate monomer or the trifunctional fluorene-containing acrylate monomer is a liquid compound that can dissolve the raw material but will not react with acyl chloride.

[0047] More preferably, the solvent used to prepare the difunctional fluorene-containing acrylate monomer or the trifunctional fluorene-containing acrylate monomer is selected from one or more of halogenated hydrocarbons, ethers, tetrahydrofurans, and benzene derivatives.

[0048] More preferably, the halogenated hydrocarbon is selected from one or more of dichloro / bromomethane, trichloro / bromomethane, dichloro / bromoethane, trichloro / bromoethane, tetrachloro / bromoethane, monochloro / bromopropane, monochloro / bromobutane, monochloro / bromopentane, monochloro / bromohexane, monochloro / bromoheptane, monochloro / bromooctane, monochloro / bromononane, or monochloro / bromodecane, trichloroethylene, tetrachloroethylene, and carbon tetrachloride.

[0049] More preferably, the solvent used to prepare the difunctional thiofluorenyl acrylate monomer is dichloromethane.

[0050] More preferably, the solvent used to prepare the trifunctional sulfur-containing fluorene acrylate monomer is chloroform.

[0051] More preferably, the ether is selected from one or more of diethyl ether, diethyl ether, tetrahydrofuran, methyl tert-butyl ether, diphenyl ether, anisole, and isopropyl ether.

[0052] More preferably, the benzene derivative is selected from one or more of benzene, toluene, xylene, trimethylbenzene, ethylbenzene, tert-butylbenzene, chlorobenzene, dichlorobenzene, trichlorobenzene, and cumene.

[0053] Preferably, the molar ratio of the acid-binding agent, polymerization inhibitor, acyl chloride compound, and difunctional sulfur-containing fluorene intermediate is (2-6):(0.01-1):(1-4):1.

[0054] More preferably, the molar ratio of the acid-binding agent, polymerization inhibitor, acyl chloride compound, and difunctional sulfur-containing fluorene intermediate is 4:0.1:2.2:1.

[0055] Preferably, the molar ratio of the acid-binding agent, polymerization inhibitor, acyl chloride compound and trifunctional sulfur-containing fluorene intermediate is (4-8):(0.01-1):(4-6):1.

[0056] More preferably, the molar ratio of the acid-binding agent, polymerization inhibitor, acyl chloride compound, and trifunctional sulfur-containing fluorene intermediate is 6:0.1:4:1.

[0057] Preferably, when preparing the difunctional thiofluorenyl acrylate monomer, an acyl chloride compound is added under ice bath conditions, and the monomer is obtained by heating and reflux reaction.

[0058] More preferably, the heating reflux reaction temperature is 36~150℃, and the reflux reaction time is 12~26 h.

[0059] Preferably, when preparing the trifunctional sulfur-containing fluorene acrylate monomer, an acyl chloride compound is added under ice bath conditions, and the reaction is carried out at room temperature to obtain the trifunctional sulfur-containing fluorene acrylate monomer.

[0060] An application of the above-mentioned sulfide-based fluorene-based high-refractive-index acrylate monomer is to use the sulfide-based fluorene-based high-refractive-index acrylate monomer to prepare a brightening film.

[0061] Preferably, the method for preparing the brightening film includes the following steps: The sulfide-based fluorene-based high-refractive-index acrylate monomer is uniformly mixed with an active diluent, and then a curing photoinitiator and a silicone-containing leveling agent are added. The resulting mixture is coated onto a film and then photocured to obtain an optical device brightness enhancement film.

[0062] More preferably, the resulting mixture is coated onto a PET film.

[0063] More preferably, the coating thickness of the mixed system on the membrane is 8-12 μm.

[0064] More preferably, the resulting mixture is coated onto a film and then UV cured.

[0065] More preferably, when the sulfide-based fluorene-based high-refractive-index acrylate monomer is a difunctional sulfide-containing fluorene-based acrylate monomer: the reactive diluent is selected from one or more of polyethylene glycol o-phenylphenyl ether acrylate, ethoxyphenol acrylate, benzyl acrylate, benzyl methacrylate, dicyclopentadiene acrylate, o-phenylphenoxyethyl acrylate (OPPEA), 2-hydroxyethyl acrylate, tetrahydrofuran acrylate, N-acryloylmorpholine, isobornyl acrylate, isobornyl methacrylate, and 4-phenylbutyl acrylate.

[0066] More preferably, when the sulfide-based fluorenyl high-refractive-index acrylate monomer is a difunctional sulfide-containing fluorenyl acrylate monomer: the reactive diluent is o-phenylphenoxyethyl acrylate (OPPEA).

[0067] More preferably, when the sulfide-based fluorene-based high-refractive-index acrylate monomer is a difunctional sulfonyl fluorene-based acrylate monomer: the curing photoinitiator is selected from one or more of 2-hydroxy-2-methyl-1-phenyl-1-propanone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide (TPO), ethyl 2,4,6-trimethylbenzoylphosphonate, 1-hydroxycyclohexylphenyl ketone (184), phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, 2-methyl-1-(4-methylthiophenyl)-2-morpholino-1-propanone, 2-isopropylthioxanthone, sodium benzophenone-4-sulfonate, 2-hydroxy-4-(2-hydroxyethoxy)-2-methylphenylpropanone, 2-ethylanthraquinone, 4-methylbenzophenone, and tetraethylmithrinone.

[0068] More preferably, when the sulfide-based fluorene-based high-refractive-index acrylate monomer is a difunctional sulfide-containing fluorene-based acrylate monomer: the curing photoinitiator is 1-hydroxycyclohexylphenyl ketone and 2,4,6-trimethylbenzoyl-diphenylphosphine oxide.

[0069] More preferably, when the sulfide-based fluorene-based high-refractive-index acrylate monomer is a difunctional sulfide-containing fluorene-based acrylate monomer: the silicone leveling agent is selected from one or more of BYK-320, BYK-322, BYK-077, BYK-325N, BYK-310, BYK-307, BYK-306, BYK-315N, BYK-329, BYK-333, TEGO10, TEGO41, TEGO432, TEGO435, TEGO450, TEGO482, SF3288, FL3777AN, FL3670, LEVELOL835, WE-D846R, WE-D888N, WE-D819C, and WE-D881R.

[0070] More preferably, when the sulfide-based fluorene-based high-refractive-index acrylate monomer is a difunctional sulfide-containing fluorene-based acrylate monomer: the silicone-containing leveling agent is BYK-333.

[0071] More preferably, when the sulfide-based fluorene-based high-refractive-index acrylate monomer is a difunctional sulfide-containing fluorene-based acrylate monomer: the molar ratio of the difunctional sulfide-containing fluorene-based acrylate monomer to the reactive diluent is 1:6~10.

[0072] More preferably, when the sulfide-based fluorene-based high-refractive-index acrylate monomer is a difunctional sulfide-containing fluorene-based acrylate monomer: the total mass fraction of the curing photoinitiator accounts for 0.5% to 5% of the mixed system.

[0073] More preferably, when the sulfide-based fluorenyl high-refractive-index acrylate monomer is a difunctional sulfide-containing fluorenyl acrylate monomer: the total mass fraction of the silicone leveling agent accounts for 0.05% to 0.5% of the mixed system.

[0074] More preferably, when the sulfide-based fluorenyl high-refractive-index acrylate monomer is a trifunctional sulfide-containing fluorenyl acrylate monomer: the reactive diluent is selected from one or more of biphenylmethanol acrylate, methyl 2-acrylate (4-phenoxyphenyl) (PPME), and o-phenylphenoxyethyl acrylate (OPPEA).

[0075] More preferably, when the sulfide-based fluorene-based high-refractive-index acrylate monomer is a trifunctional sulfide-containing fluorene-based acrylate monomer: the curing photoinitiator is selected from one or more of methyl benzoylformate, trimethylbenzoyl diphenylphosphine oxide (TPO), benzophenone, tetraethylmielone, 4-methylbenzophenone, methyl o-benzoylbenzoate, 2-hydroxy-2-methyl-1-phenylpropanone, 1-hydroxycyclohexylphenyl ketone, and 2-ethylanthraquinone.

[0076] More preferably, when the sulfide-based fluorene-based high-refractive-index acrylate monomer is a trifunctional sulfide-containing fluorene-based acrylate monomer: the silicone leveling agent is selected from one or more of the following: acrylate-modified polyether silicone Tego rad 2500, polydimethylsilane, polymethylphenylsiloxane, and silicone leveling agent BKY-333.

[0077] More preferably, when the sulfide-based fluorene-based high-refractive-index acrylate monomer is a trifunctional sulfide-containing fluorene-based acrylate monomer: the silicone leveling agent is organosilicon leveling agent BKY-333.

[0078] More preferably, when the sulfide-based fluorene-based high-refractive-index acrylate monomer is a trifunctional sulfide-containing fluorene-based acrylate monomer: the molar ratio of the trifunctional sulfide-containing fluorene-based acrylate monomer to the reactive diluent is 1:6~10.

[0079] More preferably, when the sulfide-based fluorene-based high-refractive-index acrylate monomer is a trifunctional sulfide-containing fluorene-based acrylate monomer: the total mass fraction of the curing photoinitiator accounts for 0.5% to 2% of the mixed system.

[0080] More preferably, when the sulfide-based fluorene-based high-refractive-index acrylate monomer is a trifunctional sulfide-containing fluorene-based acrylate monomer: the total mass fraction of the silicone-containing leveling agent accounts for 0.1% to 0.5% of the mixed system.

[0081] More preferably, the preparation method of the brightening film includes the following steps: uniformly mixing the sulfide-based fluorene-based high-refractive-index acrylate monomer with an active diluent, then adding a curing photoinitiator and a silicone-containing leveling agent, mixing and degassing the mixture using a homogenizer, coating the resulting mixture onto a PET film, covering it with a prism film mold, UV curing it using a mercury lamp, and demolding it to obtain the brightening film.

[0082] More preferably, the UV curing light intensity is 450-550 mJ / cm². 2 Curing time: 2-4 seconds.

[0083] More preferably, the homogenizer mixing and degassing process includes mixing at 2500-3500 rpm for 5-10 minutes, followed by vacuuming and then mixing at 2500-3500 rpm for another 5-10 minutes to obtain a high-refractive index brightening film adhesive, i.e., a mixed system.

[0084] In high-refractive-index molecular structure design, sulfur atoms possess high molar refractive index, which can significantly enhance the refractive index of the material. Meanwhile, the rigid fluorene group structure, while maintaining high refractive properties, also helps maintain the dimensional stability of the cured film. Therefore, the sulfur-containing and fluorene-containing acrylate monomers developed in this invention, which combine high refractive index, good process adaptability, and high performance, have significant technical value and industrial guiding significance for meeting the application requirements of next-generation high-performance backlight module brightness enhancement films.

[0085] Compared with the prior art, the present invention has the following technical advantages: 1) The monomer molecule of the present invention contains both fluorene and thioether groups, and has both excellent mechanical properties and high refractive index.

[0086] 2) This invention introduces both a fluorene group with a high molar refractive index and a sulfur atom into a single molecule. In the molecular structure, the fluorene group fixes the sulfur atom at the center of the molecule, which greatly reduces the pungent odor caused by the sulfur atom. At the same time, the solubility gain of the thioalkyl chain segment also solves the solubility problem of the fluorene group with a polybenzene ring structure.

[0087] 3) This invention integrates fluorene and thioether groups within a single molecule to form a difunctional / trifunctional acrylic resin that possesses both excellent mechanical properties and a high refractive index. Difunctional / trifunctional acrylic monomers account for over 60% of the production of commercial acrylic products, and their cured spatial topological structures are two-dimensional / three-dimensional network structures, respectively. This ensures strength while avoiding the negative effects of curing shrinkage caused by higher functionality.

[0088] 4) The monomers of this invention are prepared by comprehensively utilizing efficient organic reactions such as the Williamson reaction, the Thiol-Ene Click Reaction, and the acyl chloride esterification reaction. The synthetic route is simple, efficient, and the conditions are mild and controllable. In this strategy, sulfur-containing building blocks, fluorene building blocks, and (meth)acrylate building blocks can be flexibly replaced, greatly increasing the versatility and scalability of the strategy.

[0089] 5) This invention uses a side-chain segment synthesis and central linking strategy to control the number of each functional group of rigid fluorenyl, flexible thioalkyl segment and (meth)acrylate to be 1:1:1, which ensures the excellent optical properties, lipid solubility, UV-curing performance and brittle-tough balance of the cured material.

[0090] 6) The monomers obtained by this invention all have a refractive index greater than 1.58, cure rapidly, and have good wear resistance and adhesion properties, which can meet the application requirements of the high-end optical incremental film field.

[0091] 7) The brightness enhancement film precursor adhesive based on the monomer configuration of the present invention cures rapidly and has excellent mechanical properties, which can provide an efficient and reliable preparation strategy for the synthesis of high-refractive-index monomers for use in the field of high-end optical brightness enhancement films.

[0092] 8) The good solubility of the sulfide segments of this invention facilitates formulation design, and the introduction of various additives will not cause the designed monomers to precipitate, thus bringing good process adaptability.

[0093] 9) This invention utilizes a single-molecule design, linking the high-refractive-index fluorene group to the same molecule via sulfide segments. The resulting formulation has a refractive index exceeding 1.58, with each single chain containing 6 carbon atoms. This segment length not only improves solubility but also avoids hardness defects caused by excessively long segments. After a single curing cycle (within 3 seconds), the resulting brightening film achieves a hardness of 2H~3H and an adhesion rating of 0. Attached Figure Description

[0094] Figure 1 Nuclear magnetic resonance of monoallyl bisphenol fluorene in Example 1 1 H spectrum, solvent was deuterated chloroform, instrument was JEOL JNM-ECZL500R, MHz was 500 MHz; Figure 2 Nuclear magnetic resonance of the intermediate in Example 1 1 H spectrum, solvent was deuterated chloroform, instrument was JEOL JNM-ECZL500R, MHz was 500 MHz; Figure 3 Nuclear magnetic resonance of compound I in Example 1 1H spectrum, solvent was deuterated chloroform, instrument was JEOL JNM-ECZL500R, MHz was 500 MHz; Figure 4 Images of the brightening films prepared in Application Examples 1-3 and Comparative Examples 1 and 2; Figure 5 Nuclear magnetic resonance of monoallyl bisphenol fluorene in Example 7 1 H spectrum, solvent was deuterated chloroform, instrument was JEOL JNM-ECZL500R, MHz was 500 MHz; Figure 6 Nuclear magnetic resonance of the intermediate in Example 7 1 H spectrum, solvent was deuterated chloroform, instrument was JEOL JNM-ECZL500R, MHz was 500 MHz; Figure 7 Nuclear magnetic resonance (NMR) of trifunctionalized sulfide fluorene-based high-refractive-index acrylate monomer V in Example 7 1 H spectrum, solvent was deuterated chloroform, instrument was JEOL JNM-ECZL500R, MHz was 500 MHz; Figure 8 Images of the brightening films prepared in Application Examples 4-6 and Comparative Examples 3 and 4. Detailed Implementation

[0095] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments. These embodiments are based on the technical solution of the present invention and provide detailed implementation methods and specific operating procedures. However, the scope of protection of the present invention is not limited to the following embodiments.

[0096] In the following embodiments, unless otherwise specified, the raw materials, reagents, or processing techniques are all conventional commercially available products or conventional processing techniques in the art. The processing temperature is room temperature, the processing pressure is atmospheric pressure, and the processing atmosphere is air. All raw materials used were purchased from Shanghai Maclean Biochemical Technology Co., Ltd., and the actual brand is not limited. Their purity is all AR grade.

[0097] Example 1 In a 500 mL round-bottom flask, 10 g of bisphenol fluorene (CAS: 3236-71-3), 12 g of anhydrous potassium carbonate, and 200 mL of acetone were added. The reaction system was stirred and heated to 65 °C, while a solution of bromopropene in acetone (3.5 g of 1-bromopropene dissolved in 100 mL of acetone) was slowly added dropwise. After reacting for 24 h, the reaction system was cooled to room temperature. The potassium carbonate was removed by filtration, and then the reaction solution was rotary evaporated at 40 °C to remove the acetone. After rotary evaporation, the product was redissolved with 50 mL of ethyl acetate and washed three times with water (20 mL × 3). The organic phases were combined, dried over anhydrous sodium sulfate, and the solvent was removed by rotary evaporation to obtain 10.32 g of monoallyl bisphenol fluorene, with a yield of 92.6%.

[0098] In a 250 mL round-bottom flask, 1 g of allyl bisphenol fluorene, 30 mL of acetonitrile, and 0.02 g of azobisisobutyronitrile were added sequentially. Under a nitrogen atmosphere, the reaction system was heated to 75 °C and vigorously stirred until fully dissolved. After the system began to reflux, 0.14 g of 1,3-propanedithiol diluted in 10 mL of acetonitrile was slowly added dropwise to the reaction system. After reacting for 12 h, the reaction system was cooled to room temperature, and the acetonitrile solvent was removed by rotary evaporation. The product was then redissolved with 30 mL of dichloromethane and washed three times with deionized water (30 mL × 3). The organic phases were combined, dried over anhydrous sodium sulfate, and the solvent was removed by rotary evaporation. The crude product was a yellow gel; 40 mL of n-hexane was added to the product for washing. After vacuum drying, 1.07 g of a pale yellow transparent intermediate was obtained, with a yield of 94.0%.

[0099] In a 250 mL round-bottom flask, 1 g of intermediate, 0.52 g of triethylamine, 0.01 g of MEHQ, 30 mL of dichloromethane, and 0.31 g of acryloyl chloride were added sequentially. The reaction was carried out at room temperature for 24 h under a nitrogen atmosphere. After TLC confirmed the reaction was complete, the reaction solution was washed sequentially with 30 mL of 1M dilute hydrochloric acid, 60 mL of saturated sodium bicarbonate aqueous solution, and 60 mL of deionized water. The organic phase was dried over anhydrous sodium sulfate and the solvent was removed by rotary evaporation to obtain 1.03 g of a pale yellow viscous compound I, with a yield of 91.72%. The refractive index was 1.6226 as measured by an Abbe refractometer.

[0100] Figures 1-3 The NMR spectra of monoallyl bisphenol fluorene, the intermediate, and compound I in this embodiment are shown. 1 The H spectrum confirmed the successful execution of each reaction step.

[0101] Example 2 The difference between this embodiment and Example 1 is that photoinitiation is used to prepare the intermediate; the same steps will not be described again. In a 250 mL photoreactor equipped with a 365 nm 20 W light source, 1 g of allyl bisphenol fluorene, 0.02 g of 1-hydroxycyclohexylphenyl ketone, and 30 mL of acetonitrile were added sequentially. Under a nitrogen atmosphere and with vigorous stirring, 0.14 g of 1,3-propanedithiol dissolved in 10 mL of acetonitrile was added dropwise to the system, and the UV light source was turned on. After reacting for 12 h, the acetonitrile solvent was removed by rotary evaporation. Subsequently, 50 mL of dichloromethane was added to redissolve the crude product, and the mixture was washed three times with deionized water (30 mL × 3). The organic phases were combined, dried over anhydrous sodium sulfate, and the solvent was removed by rotary evaporation. The crude product was a yellow gel. 30 mL of n-hexane and 15 mL of methanol were added sequentially to the product for washing. After vacuum drying, 0.98 g of a pale yellow transparent intermediate was obtained, with a yield of 86.1%.

[0102] Example 3 The difference between this example and Example 1 is the use of methacryloyl chloride in the preparation; the same steps will not be described again. In a 250 mL round-bottom flask, 1 g of the intermediate was added, followed by 0.35 g of methacryloyl chloride, 30 mL of dichloromethane, 0.52 g of triethylamine, and 0.01 g of MEHQ. The reaction was carried out at room temperature for 24 h under a nitrogen atmosphere. After TLC confirmed the reaction was complete, the reaction mixture was washed sequentially with 30 mL of 1M dilute hydrochloric acid, 60 mL of saturated sodium bicarbonate aqueous solution, and 60 mL of deionized water. The organic phase was dried over anhydrous sodium sulfate, and the solvent was removed by rotary evaporation to obtain 1.07 g of a pale yellow viscous compound II, with a yield of 92.8%. The refractive index was 1.6230 as measured by an Abbe refractometer.

[0103] The synthetic routes for compounds I and II described in Examples 1 and 3 are shown below: Example 4 The difference between this embodiment and Embodiment 2 is that photoinitiation is used to prepare the intermediate; the same steps will not be described again. In a 250 mL photoreactor equipped with a 365 nm 20 W light source, 1 g of allyl bisphenol fluorene, 0.02 g of 1-hydroxycyclohexylphenyl ketone, and 30 mL of acetonitrile were added sequentially. Under a nitrogen atmosphere and with vigorous stirring, 0.14 g of 1,3-propanedithiol dissolved in 10 mL of acetonitrile was added dropwise to the system, and the UV light source was turned on. After reacting for 12 h, the acetonitrile solvent was removed by rotary evaporation. Subsequently, 50 mL of dichloromethane was added to redissolve the crude product, and the mixture was washed three times with deionized water (30 mL × 3). The organic phases were combined, dried over anhydrous sodium sulfate, and the solvent was removed by rotary evaporation. The crude product was a yellow gel. 30 mL of n-hexane and 15 mL of methanol were added sequentially to the product for washing. After vacuum drying, 0.96 g of a pale yellow transparent intermediate was obtained, with a yield of 84.9%. Example 5 In a 500 mL round-bottom flask, 10 g of bisphenol fluorene (CAS: 3236-71-3), 12 g of anhydrous potassium carbonate, and 200 mL of acetone were added. The reaction system was stirred and heated to 65 °C, while a solution of bromopropene in acetone (3.5 g of 1-bromopropene dissolved in 100 mL of acetone) was slowly added dropwise. After reacting for 24 h, the reaction system was cooled to room temperature. The potassium carbonate was removed by filtration, and then the reaction solution was rotary evaporated at 40 °C to remove the acetone. After rotary evaporation, the product was redissolved with 50 mL of ethyl acetate and washed three times with water (20 mL × 3). The organic phases were combined, dried over anhydrous sodium sulfate, and the solvent was removed by rotary evaporation to obtain 10.32 g of monoallyl bisphenol fluorene, with a yield of 92.6%.

[0104] In a 250 mL round-bottom flask, 1 g of allyl bisphenol fluorene, followed by 30 mL of acetonitrile and 0.02 g of azobisisobutyronitrile (AIBN). Under a nitrogen atmosphere, the reaction mixture was heated to 75 °C and vigorously stirred until fully dissolved. After the system began to reflux, 0.29 g of 4,4-thiodiphenylthiol diluted in 10 mL of acetonitrile was slowly added dropwise to the reaction mixture. After 12 h of reaction, the reaction mixture was cooled to room temperature, and the acetonitrile solvent was removed by rotary evaporation. The product was then redissolved in 30 mL of dichloromethane and washed three times with deionized water (30 mL × 3). The organic phases were combined, dried over anhydrous sodium sulfate, and the solvent was removed by rotary evaporation. The crude product was a yellow gel. 40 mL of n-hexane was added to the product for washing. After vacuum drying, 1.12 g of a pale yellow transparent intermediate was obtained, with a yield of 84.8%. In a 250 mL round-bottom flask, 1 g of the intermediate was added, followed by 0.27 g of acryloyl chloride, 30 mL of dichloromethane, 0.52 g of triethylamine, and 0.01 g of MEHQ. The reaction was carried out at room temperature for 24 h under a nitrogen atmosphere. After TLC confirmed the reaction was complete, the reaction mixture was washed sequentially with 30 mL of 1M dilute hydrochloric acid, 60 mL of saturated sodium bicarbonate aqueous solution, and 60 mL of deionized water. The organic phase was dried over anhydrous sodium sulfate, and the solvent was removed by rotary evaporation to obtain 1.03 g of a pale yellow viscous compound III, with a yield of 93.1%. The refractive index was 1.6224 as measured by an Abbe refractometer.

[0105] 1 H NMR (400 MHz, Chloroform- d ) δ 7.74 (d, J = 7.8 Hz, 4H), 7.46 -7.38 (m, 8H), 7.30 (d, J = 1.9 Hz, 4H), 7.24 (d, J = 8.1 Hz, 4H), 7.19 (d, J =9.2 Hz, 4H), 7.17 (d, J = 8.2 Hz, 4H), 7.14 (d, J = 9.2 Hz, 4H), 6.99 (d, J =9.2 Hz, 4H), 6.71 (d, J = 9.0 Hz, 4H), 6.55 (dd, J = 18.1, 1.8 Hz, 2H), 6.33(dd, J = 18.3, 10.9 Hz, 2H), 6.00 (dd, J = 10.9, 1.7 Hz, 2H), 3.90 (t, J =6.2 Hz, 4H), 2.64 (t, J = 6.0 Hz, 4H), 2.11 (p, J = 6.6 Hz, 4H), Example 6 The difference between this example and Example 5 is the use of methacryloyl chloride in the preparation; the same steps will not be described again. In a 250 mL round-bottom flask, 1 g of the intermediate was added, followed by 0.35 g of methacryloyl chloride, 30 mL of dichloromethane, 0.52 g of triethylamine, and 0.01 g of MEHQ. The reaction was carried out at room temperature for 24 h under a nitrogen atmosphere. After TLC confirmed the reaction was complete, the reaction mixture was washed sequentially with 30 mL of 1M dilute hydrochloric acid, 60 mL of saturated sodium bicarbonate aqueous solution, and 60 mL of deionized water. The organic phase was dried over anhydrous sodium sulfate, and the solvent was removed by rotary evaporation to obtain 1.05 g of a pale yellow viscous compound IV, with a yield of 92.7%. The refractive index was 1.6234 as measured by an Abbe refractometer.

[0106] Example 7 In a 250 mL round-bottom flask, 10 g of bisphenol fluorene (CAS: 3236-71-3), 12 g of anhydrous potassium carbonate, and 100 mL of acetone were added. The reaction system was stirred and heated to 65 °C, while a solution of bromopropene in acetone (3.5 g of 1-bromopropene dissolved in 50 mL of acetone) was slowly added dropwise. After reacting for 24 h, the reaction system was cooled to room temperature. The inorganic salts were removed by filtration, and the solvent was then removed by rotary evaporation. After rotary evaporation, the product was redissolved in 50 mL of ethyl acetate and washed three times with water (20 mL × 3). The organic phases were combined, dried over anhydrous sodium sulfate, and the solvent was removed by rotary evaporation. The yellow oily product was redissolved in 20 mL of dichloromethane, and the insoluble matter was removed by filtration to obtain 9.8 g of monoallyl bisphenol fluorene, with a yield of 88.3%.

[0107] In a 250 mL round-bottom flask, 3 g of allyl bisphenol fluorene, 30 mL of dichloromethane, and 0.007 g of azobisisobutyronitrile were added sequentially. The reactor was purged three times with high-purity nitrogen. Under a nitrogen atmosphere, the reaction system was heated to 40 °C and vigorously stirred to ensure complete dissolution. After the reaction system reached reflux temperature, 0.57 g of polythiol 504 (CAS: 131538-00-6) diluted in 10 mL of dichloromethane was slowly added dropwise to the reaction system. After reacting for 18 h, the reaction system was cooled to room temperature. The organic phase was washed three times with deionized water (30 mL × 3), and the aqueous phase was back-extracted once with 20 mL of dichloromethane. The organic phases were combined, dried over anhydrous sodium sulfate, and the solvent was removed by rotary evaporation. The crude product was a yellow, transparent, viscous liquid. 40 mL of methanol and acetonitrile in a 1:1 ratio was added to the product. v / v Mix the ingredients and stir vigorously. After centrifugation and desiccation, the remaining pale yellow viscous substance was dried under vacuum to obtain 2.87 g of trifunctional fluorene sulfide intermediate, with a yield of 94.1%.

[0108] In a 250 mL round-bottom flask, 2 g of a trifunctional fluorenyl thioether intermediate, 0.87 g of triethylamine, 0.017 g of MEHQ, and 40 mL of chloroform solvent were added sequentially. The reaction system was purged with nitrogen three times and then cooled to 0 °C in an ice bath. A chloroform solution of acryloyl chloride (0.52 g of acryloyl chloride dissolved in 10 mL of chloroform) was added dropwise to the reaction system. After the addition was complete, the reaction system was allowed to return to room temperature and reacted under a nitrogen atmosphere for 24 h. After TLC confirmed complete substrate reaction, the reaction solution was washed sequentially with 20 mL of 1M dilute hydrochloric acid, 50 mL of saturated sodium bicarbonate aqueous solution, and 50 mL of deionized water to remove excess triethylamine, acryloyl chloride, hydrochloric acid, and inorganic salts. The organic phase was dried over anhydrous sodium sulfate, and chloroform was removed by rotary evaporation to obtain 1.99 g of a pale yellow, viscous trifunctionalized sulfide fluorenyl high-refractive-index acrylate monomer V, with a yield of 89.0%. Its refractive index was measured to be 1.6332 using an Abbe refractometer.

[0109] Figures 5-7 The nuclear magnetic resonance (NMR) data of monoallyl bisphenol fluorene, the intermediate, and the trifunctional sulfide fluorene-based high-refractive-index acrylate monomer V in this embodiment are shown. 1 The H spectrum confirmed the successful execution of each reaction step.

[0110] Example 8 The preparation process of monoallyl bisphenol fluorene and trifunctional sulfide fluorene-based high-refractive-index acrylate monomer V is the same as in Example 7 and will not be described again.

[0111] In a 250 mL quartz photoreactor, 3 g of allyl bisphenol fluorene, 0.3 g of polythiol 504, 30 mL of dichloromethane, and 0.008 g of benzophenone were added sequentially. The reactor was purged three times with high-purity nitrogen. Under a nitrogen atmosphere, the reaction system was vigorously stirred to ensure complete dissolution. A 365 nm light source was turned on, and 0.27 g of polythiol 504 diluted in 20 mL of dichloromethane was slowly added dropwise to the reaction system. After 24 h of reaction, the reaction system was cooled to room temperature. The organic phase was washed three times with deionized water (30 mL × 3), and the aqueous phase was back-extracted once with 20 mL of dichloromethane. The organic phases were combined, dried over anhydrous sodium sulfate, and the solvent was removed by rotary evaporation. The crude product was a yellow, transparent, viscous liquid. 40 mL of a 1:1 mixture of methanol and acetonitrile was added to the product. v / v Mix the liquid and stir vigorously. After centrifugation and decanting, the remaining pale yellow viscous substance was dried under vacuum to obtain 2.15 g of trifunctional fluorene sulfide intermediate, with a yield of 70.5%.

[0112] Example 9 The preparation process of the intermediate between monoallyl bisphenol fluorene and trifunctional fluorene sulfide compounds is the same as in Example 7 and will not be described again.

[0113] In a 250 mL round-bottom flask, 2 g of a trifunctional fluorenyl thioether intermediate, 0.87 g of triethylamine, 0.017 g of MEHQ, and 40 mL of chloroform solvent were added sequentially. The reaction system was purged with nitrogen three times and then cooled to 0 °C in an ice bath. A chloroform solution of methacryloyl chloride (0.60 g of acryloyl chloride dissolved in 10 mL of chloroform) was added dropwise to the reaction system. After the addition was complete, the reaction system was allowed to return to room temperature and reacted under a nitrogen atmosphere for 24 h. After TLC confirmed complete substrate reaction, the reaction solution was washed sequentially with 20 mL of 1M dilute hydrochloric acid, 50 mL of saturated sodium bicarbonate aqueous solution, and 50 mL of deionized water to remove excess triethylamine, methacryloyl chloride, hydrochloric acid, and inorganic salts. The organic phase was dried over anhydrous sodium sulfate, and chloroform was removed by rotary evaporation to obtain 1.91 g of a pale yellow, viscous trifunctionalized sulfide fluorenyl high-refractive-index acrylate monomer VI, with a yield of 83.8%. Its refractive index was measured to be 1.6118 using an Abbe refractometer.

[0114] Example 10 In a 250 mL round-bottom flask, 10 g of bisphenol fluorene (CAS: 3236-71-3), 12 g of anhydrous potassium carbonate, and 100 mL of acetone were added. The reaction system was stirred and heated to 65 °C, while a solution of 1-bromo-n-butene in acetone (3.9 g of 1-bromopropene dissolved in 50 mL of acetone) was slowly added dropwise. After reacting for 24 h, the reaction system was cooled to room temperature. The inorganic salts were removed by filtration, and the solvent was then removed by rotary evaporation. After rotary evaporation, the product was redissolved in 50 mL of ethyl acetate and washed three times with water (20 mL × 3). The organic phases were combined, dried over anhydrous sodium sulfate, and the solvent was removed by rotary evaporation. The milky white oily substance was redissolved in 20 mL of dichloromethane, and the insoluble matter was removed by filtration to obtain 10.6 g of mono-1-n-butenylbisphenol fluorene, with a yield of 91.4%.

[0115] In a 250 mL round-bottom flask, 3 g of mono-1-n-butenylbisphenol fluorene, 30 mL of chloroform, and 0.007 g of azobisisobutyronitrile were added sequentially. The reactor was purged three times with high-purity nitrogen. Under a nitrogen atmosphere, the reaction system was heated to 40 °C and stirred vigorously to ensure complete dissolution. 0.37 g of trimercaptobenzene (CAS: 38004-59-0) was dissolved and added to 50 mL of hot chloroform, and stirred vigorously to dissolve. When the reaction system reached reflux temperature, this solution was added dropwise to the reaction system while hot. After reacting for 24 h, the mixture was cooled to room temperature. The organic phase was washed three times with deionized water (30 mL × 3), and the aqueous phase was back-extracted once with 20 mL of chloroform. The organic phases were combined, dried over anhydrous sodium sulfate, and the solvent was removed by rotary evaporation. The crude product was a yellow, transparent, viscous liquid. 40 mL of a 1:1 mixture of methanol and acetonitrile was added to the product. v / v Mix the liquid and stir vigorously. After centrifugation and decanting, the remaining pale yellow viscous substance was dried under vacuum to obtain 3.11 g of trifunctional fluorene sulfide intermediate, with a yield of 92.8%.

[0116] In a 250 mL round-bottom flask, 2 g of a trifunctional fluorenyl thioether intermediate, 0.88 g of triethylamine, 0.018 g of MEHQ, and 40 mL of chloroform solvent were added sequentially. The reaction system was purged with nitrogen three times and then cooled to 0 °C in an ice bath. A chloroform solution of acryloyl chloride (0.52 g of acryloyl chloride dissolved in 10 mL of chloroform) was added dropwise to the reaction system. After the addition was complete, the reaction system was allowed to return to room temperature and reacted under a nitrogen atmosphere for 24 h. After TLC confirmed complete substrate reaction, the reaction solution was washed sequentially with 20 mL of 1M dilute hydrochloric acid, 50 mL of saturated sodium bicarbonate aqueous solution, and 50 mL of deionized water to remove excess triethylamine, acryloyl chloride, hydrochloric acid, and inorganic salts. The organic phase was dried over anhydrous sodium sulfate, and chloroform was removed by rotary evaporation to obtain 1.87 g of a pale yellow, viscous trifunctionalized sulfide fluorenyl high-refractive-index acrylate monomer VII, with a yield of 83.9%. Its refractive index was measured to be 1.6359 using an Abbe refractometer.

[0117] Example 11 In a 250 mL round-bottom flask, 10 g of bisphenol fluorene (CAS: 3236-71-3), 12 g of anhydrous potassium carbonate, and 100 mL of acetone were added. The reaction system was stirred and heated to 65 °C, while a solution of 1-bromohexene in acetone (4.7 g of 1-bromohexene dissolved in 50 mL of acetone) was slowly added dropwise. After reacting for 24 h, the reaction system was cooled to room temperature. The inorganic salts were removed by filtration, and the solvent was then removed by rotary evaporation. After rotary evaporation, the product was redissolved in 50 mL of ethyl acetate and washed three times with water (20 mL × 3). The organic phases were combined, dried over anhydrous sodium sulfate, and the solvent was removed by rotary evaporation. The yellow oily product was redissolved in 20 mL of dichloromethane, and the insoluble matter was removed by filtration to obtain 10.7 g of mono-1-hexenylbisphenol fluorene, with a yield of 86.7%.

[0118] In a 250 mL round-bottom flask, 3 g of mono-1-hexenylbisphenol fluorene, 30 mL of dichloromethane, and 0.007 g of azobisisobutyronitrile were added sequentially. The reactor was purged three times with high-purity nitrogen. Under a nitrogen atmosphere, the reaction system was heated to 40 °C and stirred vigorously to ensure complete dissolution. After the reaction system reached reflux temperature, 0.58 g of 1,1-tris(mercaptomethyl)undecane (CAS: 850873-54-01) diluted in 10 mL of dichloromethane was slowly added dropwise to the reaction system. After reacting for 20 h, the reaction system was cooled to room temperature. The organic phase was washed three times with deionized water (30 mL × 3), and the aqueous phase was back-extracted once with 20 mL of dichloromethane. The organic phases were combined, dried over anhydrous sodium sulfate, and the solvent was removed by rotary evaporation. The crude product was a yellow, transparent, viscous liquid. 40 mL of a 1:1 mixture of methanol and acetonitrile was added to the product. v / v Mix the liquid and stir vigorously. After centrifugation and desiccation, the remaining pale yellow viscous substance was dried under vacuum to obtain 2.64 g of trifunctional fluorene sulfide intermediate, with a yield of 88.3%.

[0119] In a 250 mL round-bottom flask, 2 g of a trifunctional fluorenyl thioether intermediate, 0.80 g of triethylamine, 0.016 g of MEHQ, and 40 mL of chloroform solvent were added sequentially. The reaction system was purged with nitrogen three times and then cooled to 0 °C in an ice bath. A chloroform solution of acryloyl chloride (0.48 g of acryloyl chloride dissolved in 10 mL of chloroform) was added dropwise to the reaction system. After the addition was complete, the reaction system was allowed to return to room temperature and reacted under a nitrogen atmosphere for 18 h. After TLC confirmed complete substrate reaction, the reaction solution was washed sequentially with 20 mL of 1M dilute hydrochloric acid, 50 mL of saturated sodium bicarbonate aqueous solution, and 50 mL of deionized water to remove excess triethylamine, acryloyl chloride, hydrochloric acid, and inorganic salts. The organic phase was dried over anhydrous sodium sulfate, and chloroform was removed by rotary evaporation to obtain 1.97 g of a pale yellow, viscous trifunctionalized sulfide fluorenyl high-refractive-index acrylate monomer VIII, with a yield of 88.9%. Its refractive index was 1.5823 as measured by an Abbe refractometer.

[0120] Example 12 In a 250 mL round-bottom flask, 10 g of bisphenol fluorene (CAS: 3236-71-3), 12 g of anhydrous potassium carbonate, and 100 mL of acetone were added. The reaction system was stirred and heated to 65 °C, while a solution of 1-bromohexene in acetone (6.1 g of 1-iodohexene dissolved in 80 mL of acetone) was slowly added dropwise. After reacting for 18 h, the reaction system was cooled to room temperature. The inorganic salts were removed by filtration, and the solvent was then removed by rotary evaporation. After rotary evaporation, the product was redissolved in 50 mL of ethyl acetate and washed three times with water (20 mL × 3). The organic phases were combined, dried over anhydrous sodium sulfate, and the solvent was removed by rotary evaporation. The yellow oily product was redissolved in 20 mL of dichloromethane, and the insoluble matter was removed by filtration to obtain 11.8 g of mono-1-hexenylbisphenol fluorene, with a yield of 95.4%.

[0121] In a 250 mL round-bottom flask, 3 g of mono-1-hexenylbisphenol fluorene, 30 mL of dichloromethane, and 0.007 g of azobisisobutyronitrile were added sequentially. The reactor was purged three times with high-purity nitrogen. Under a nitrogen atmosphere, the reaction system was heated to 40 °C and vigorously stirred to ensure complete dissolution. After the reaction system reached reflux temperature, 0.79 g of trimethylolpropane-tris(3-mercaptopropionate) (CAS: 33007-83-9) diluted in 10 mL of dichloromethane was slowly added dropwise to the reaction system. After reacting for 24 h, the reaction system was cooled to room temperature. The organic phase was washed three times with deionized water (30 mL × 3), and the aqueous phase was back-extracted once with 30 mL of dichloromethane. The organic phases were combined, dried over anhydrous sodium sulfate, and the solvent was removed by rotary evaporation. The crude product was a transparent viscous liquid. 40 mL of methanol and acetonitrile in a 1:1 ratio was added to the product. v / v Mix the liquid and stir vigorously. After centrifugation and desiccation, the remaining transparent viscous substance is dried under vacuum to obtain 3.01 g of trifunctional fluorenyl sulfide intermediate, with a yield of 91.7%.

[0122] In a 250 mL round-bottom flask, 2 g of a trifunctional fluorenyl thioether intermediate, 0.73 g of triethylamine, 0.015 g of MEHQ, and 40 mL of chloroform solvent were added sequentially. The reaction system was purged with nitrogen three times and then cooled to 0 °C in an ice bath. A chloroform solution of acryloyl chloride (0.44 g of acryloyl chloride dissolved in 10 mL of chloroform) was added dropwise to the reaction system. After the addition was complete, the reaction system was allowed to return to room temperature and reacted under a nitrogen atmosphere for 24 h. After TLC confirmed complete substrate reaction, the reaction solution was washed sequentially with 20 mL of 1M dilute hydrochloric acid, 50 mL of saturated sodium bicarbonate aqueous solution, and 50 mL of deionized water to remove excess triethylamine, acryloyl chloride, hydrochloric acid, and inorganic salts. The organic phase was dried over anhydrous sodium sulfate, and chloroform was removed by rotary evaporation to obtain 2.02 g of a colorless, viscous trifunctionalized sulfide fluorenyl acrylate monomer IX, with a yield of 92.0%. Its refractive index was 1.5911 as measured by an Abbe refractometer.

[0123] Application Example 1 In this application example, the initiator is (2,4,6-trimethylbenzoyl)diphenylphosphine oxide (TPO), which accounts for 1% of the total system by mass; hydroxycyclohexane benzophenone (184), which accounts for 1% of the total system by mass; the leveling agent is acrylate-modified polyether silicone BYK-333, which accounts for 0.2% of the total system by mass; the organic acrylate diluent is o-phenylphenoxyethyl acrylate (OPPEA), which accounts for 90% of the total system by mass; and the difunctionalized fluorene-containing acrylate monomer synthesized in Example 1 accounts for 7.8% of the total system by mass. The total formulation mass is 10 g.

[0124] The components were weighed into a container according to their mass percentages and then uniformly dispersed for 15 minutes at 3000 rpm using a high-speed homogenizer. The refractive index, viscosity, and transmittance of the prepared brightening film precursor were then measured.

[0125] Subsequently, the brightness enhancement film precursor was coated onto the PET film, and a prism film mold was then applied on top, with a coating thickness of 10 μm and a light intensity energy of 500 mJ / (s·cm). 2 The system was cured under a UV mercury lamp for 3 seconds to obtain a brightening film. Viscosity, refractive index, transmittance, hardness, and adhesion were then tested.

[0126] Property tests: Refractive index was tested using an Abbe refractometer, referencing standard GB / T 614-2021, with a refractive index of 1.5884. Transmittance was measured using a transmittance meter, referencing standard GB / T 2410-2008, with a transmittance of 92.2%. Viscosity was measured using a viscometer at 25 ℃ and 200 rpm, with a system viscosity of 286.2 cp. Hardness was tested using the pencil test, referencing standard GB / T 6739-2006, with a hardness grade of 2H. Adhesion was tested using the cross-cut adhesion test, referencing standard GB / T7286-1998, where grade 0 is the optimal grade, and the test result was grade 1.

[0127] Application Example 2 The initiator used was (2,4,6-trimethylbenzoyl)diphenylphosphine oxide (TPO), accounting for 1% of the total system by mass; hydroxycyclohexanebenzophenone (184), accounting for 1% of the total system by mass; the leveling agent was acrylate-modified polyether silicone BYK-333, accounting for 0.2% of the total system by mass; the organic acrylate diluent was o-phenylphenoxyethyl acrylate (OPPEA), accounting for 85% of the total system by mass; and the difunctionalized fluorene-containing acrylate monomer synthesized in Example 1 accounted for 12.8% of the total system by mass. The total formulation mass was 10 g. The refractive index, viscosity, and transmittance of the prepared brightening film precursor were measured. The components were placed in a container according to the mass percentage and uniformly dispersed for 15 min using a high-speed homogenizer at 3000 rpm. Subsequently, the brightness enhancement film precursor was coated onto the PET film, and a prism film mold was then applied on top, with a coating thickness of 10 μm and a light intensity energy of 500 mJ / (s·cm). 2 The system was cured under a UV mercury lamp for 3 seconds to obtain a brightening film. Viscosity, refractive index, transmittance, hardness, and adhesion were then tested.

[0128] Property tests: Refractive index was tested using an Abbe refractometer, referencing standard GB / T 614-2021, with a refractive index of 1.5892. Transmittance was measured using a transmittance meter, referencing standard GB / T 2410-2008, with a transmittance of 93.1%. Viscosity was measured using a viscometer at 25 ℃ and 200 rpm, with a system viscosity of 309.48 cp. Hardness was tested using the pencil test, referencing standard GB / T 6739-2006, with a hardness grade of 2H. Adhesion was tested using the cross-cut adhesion test, referencing standard GB / T 7286-1998, where grade 0 is optimal, and the test result is grade 1.

[0129] Application Example 3 The initiator used was (2,4,6-trimethylbenzoyl)diphenylphosphine oxide (TPO), accounting for 1% of the total system by mass; hydroxycyclohexanebenzophenone (184), accounting for 1% of the total system by mass; the leveling agent was acrylate-modified polyether silicone BYK-333, accounting for 0.2% of the total system by mass; the organic acrylate diluent was o-phenylphenoxyethyl acrylate (OPPEA), accounting for 80% of the total system by mass; and the difunctionalized fluorene-containing acrylate monomer synthesized in Example 1 accounted for 17.8% of the total system by mass. The total formulation mass was 10 g. The refractive index, viscosity, and transmittance of the prepared brightening film precursor were measured. The components were placed in a container according to the mass percentage and uniformly dispersed for 15 min using a high-speed homogenizer at 3000 rpm. Subsequently, the brightness enhancement film precursor was coated onto the PET film, and a prism film mold was then applied on top, with a coating thickness of 10 μm and a light intensity energy of 500 mJ / (s·cm). 2 The system was cured under a UV mercury lamp for 3 seconds to obtain a brightening film. Viscosity, refractive index, transmittance, hardness, and adhesion were then tested.

[0130] Property tests: Refractive index was tested using an Abbe refractometer, referencing standard GB / T 614-2021, with a refractive index of 1.5925. Transmittance was measured using a transmittance meter, referencing standard GB / T 2410-2008, with a transmittance of 93.8%. Viscosity was measured using a viscometer at 25 ℃ and 200 rpm, with a system viscosity of 324.8 cp. Hardness was tested using the pencil test, referencing standard GB / T 6739-2006, with a hardness grade of 3H. Adhesion was tested using the cross-cut adhesion test, referencing standard GB / T7286-1998, where grade 0 is the optimal grade, and the test result was grade 0.

[0131] Application Example 4 The initiator used was (2,4,6-trimethylbenzoyl)diphenylphosphine oxide (TPO), which accounted for 1% of the total system by mass; hydroxycyclohexane benzophenone (184), which accounted for 1% of the total system by mass; the leveling agent was acrylate-modified polyether silicone BYK-333, which accounted for 0.2% of the total system by mass; o-phenylphenoxyethyl acrylate (OPPEA), which accounted for 90% of the total system by mass; and the trifunctional sulfide fluorene-based high-refractive-index acrylate monomer V synthesized in Example 7, which accounted for 7.8% of the total system by mass. The total formulation (including photoinitiator, diluent, leveling agent, and monomer) had a mass of 3 g.

[0132] The components were weighed into a container according to the formula percentage and then uniformly dispersed under vacuum at 2500 rpm for 5 minutes using a high-speed homogenizer. The refractive index, viscosity, and transmittance of the prepared brightening film adhesive were then measured.

[0133] Subsequently, the brightening film formulation adhesive was coated onto the PET film, and a prism film mold was then applied on top, with a coating thickness of 10 μm and a light intensity energy of 500 mJ / (s·cm). 2 The system was completely cured after being cured under a UV mercury lamp for 3 seconds, resulting in a brightening film sample. Hardness and adhesion tests were then performed.

[0134] Property tests: Refractive index was tested using an Abbe refractometer, referencing standard GB / T 614-2021, with a refractive index of 1.5832. Transmittance was measured using a transmittance meter, referencing standard GB / T 2410-2008, with a transmittance of 92.1%. Hardness was tested using the pencil test, referencing standard GB / T 6739-2006, with a hardness grade of 2H. Adhesion was tested using the cross-cut adhesion test, referencing standard GB / T 7286-1998, with a test result of grade 1.

[0135] Application Example 5 The initiator used was (2,4,6-trimethylbenzoyl)diphenylphosphine oxide (TPO), which accounted for 1% of the total system by mass; hydroxycyclohexane benzophenone (184), which accounted for 1% of the total system by mass; the leveling agent was acrylate-modified polyether silicone BYK-333, which accounted for 0.2% of the total system by mass; o-phenylphenoxyethyl acrylate (OPPEA), which accounted for 85% of the total system by mass; and the trifunctionalized sulfide fluorene-based high-refractive-index acrylate monomer V synthesized in Example 7, which accounted for 12.8% of the total system by mass. The total formulation mass was 3 g.

[0136] The components were weighed into a container according to the formula percentage and then uniformly dispersed under vacuum at 2500 rpm for 5 minutes using a high-speed homogenizer. The refractive index, viscosity, and transmittance of the prepared brightening film adhesive were then measured.

[0137] Subsequently, the brightening film formulation adhesive was coated onto the PET film, and a prism film mold was then applied on top, with a coating thickness of 10 μm and a light intensity energy of 500 mJ / (s·cm). 2 The system was completely cured after being cured under a UV mercury lamp for 2 seconds, resulting in a brightening film sample. Hardness and adhesion tests were then performed.

[0138] Property tests: Refractive index was tested using an Abbe refractometer, referencing standard GB / T 614-2021, with a refractive index of 1.5895. Transmittance was measured using a transmittance meter, referencing standard GB / T 2410-2008, with a transmittance of 91.7%. Hardness was tested using the pencil test, referencing standard GB / T 6739-2006, with a hardness grade of 2H. Adhesion was tested using the cross-cut adhesion test, referencing standard GB / T 7286-1998, with a test result of grade 1.

[0139] Application Example 6 The initiator used was (2,4,6-trimethylbenzoyl)diphenylphosphine oxide (TPO), which accounted for 1% of the total system by mass; hydroxycyclohexane benzophenone (184), which accounted for 1% of the total system by mass; the leveling agent was acrylate-modified polyether silicone BYK-333, which accounted for 0.2% of the total system by mass; o-phenylphenoxyethyl acrylate (OPPEA), which accounted for 80% of the total system; the trifunctionalized sulfide fluorene-based high-refractive-index acrylate monomer V synthesized in Example 7 accounted for 17.8% of the total system by mass; and the total formulation mass was 3 g.

[0140] The components were weighed into a container according to the formula percentage and then uniformly dispersed under vacuum at 2500 rpm for 5 minutes using a high-speed homogenizer. The refractive index, viscosity, and transmittance of the prepared brightening film adhesive were then measured.

[0141] Subsequently, the brightening film formulation adhesive was coated onto the PET film, and a prism film mold was then applied on top, with a coating thickness of 10 μm and a light intensity energy of 500 mJ / (s·cm). 2 The system was completely cured after being cured under a UV mercury lamp for 2 seconds, resulting in a brightening film sample. Hardness and adhesion tests were then performed.

[0142] Property tests: Refractive index was tested using an Abbe refractometer, referencing standard GB / T 614-2021, with a refractive index of 1.5963. Transmittance was measured using a transmittance meter, referencing standard GB / T 2410-2008, with a transmittance of 91.3%. Hardness was tested using the pencil test, referencing standard GB / T 6739-2006, with a hardness grade of 3H. Adhesion was tested using the cross-cut adhesion test, referencing standard GB / T 7286-1998, with a test result of grade 0.

[0143] Comparative Example 1 The initiator used was (2,4,6-trimethylbenzoyl)diphenylphosphine oxide (TPO), accounting for 1% of the total system mass; hydroxycyclohexanebenzophenone (184), accounting for 1% of the total system mass; the leveling agent was acrylate-modified polyether silicone BYK-333, accounting for 0.2% of the total system mass; the organic acrylate diluent was o-phenylphenoxyethyl acrylate (OPPEA), accounting for 85% of the total system mass; and (20-ethoxy)bisphenol A diacrylate (BPA(EO)) was used. 20DA (structural formula shown in the figure above, n+m=20), accounting for 12.8% of the total system mass, with a total formulation mass of 10 g. The refractive index, viscosity, and transmittance of the prepared brightening film precursor were measured. The components were placed in a container according to their mass percentages and uniformly dispersed for 15 min at 3000 rpm using a high-speed homogenizer. The mixture was then coated onto a PET film, covered with a prism film mold, with a coating thickness of 10 μm, and subjected to light intensity of 500 mJ / (s·cm). 2 The formulation was cured under a UV mercury lamp. After 2 seconds, it was in a viscous, semi-cured colloidal state. After 4 seconds, the system was completely cured, yielding a brightening film. Viscosity, refractive index, light transmittance, hardness, and adhesion were tested.

[0144] Brightness-enhancing film property tests: Refractive index test, using an Abbe refractometer, reference standard GB / T 614-2021, refractive index 1.5604. Transmittance measurement, using a transmittance meter, reference standard GB / T 2410-2008, transmittance 94.5%. Hardness test, using the pencil method, reference standard GB / T 6739-2006, hardness grade 2H. Adhesion test, using the cross-cut adhesion test, reference standard GB / T 7286-1998, where grade 0 is optimal, test result is grade 1.

[0145] Comparative Example 2 The initiator used was (2,4,6-trimethylbenzoyl)diphenylphosphine oxide (TPO), accounting for 1% of the total system by mass; hydroxycyclohexane benzophenone (184), accounting for 1% of the total system by mass; the leveling agent was acrylate-modified polyether silicone BYK-333, accounting for 0.2% of the total system by mass; the organic acrylate diluent was o-phenylphenoxyethyl acrylate (OPPEA), accounting for 85% of the total system by mass; and ethoxytrimethylolpropane triacrylate (TMP(EO)9TA) (structure shown in the figure above, n+m+L=9), accounting for 12.8% of the total system by mass, with a total formulation mass of 10 g. The refractive index, viscosity, and transmittance of the prepared brightening film precursor were measured. Each component was placed in a container according to the mass percentage and uniformly dispersed for 15 min using a high-speed homogenizer at 3000 rpm. The mixture was then coated onto a PET film, and a prism film mold was applied on top. The coating thickness was 10 μm, and the light intensity energy was 500 mJ / (s·cm). 2 The formulation was cured under a UV mercury lamp. After 2 seconds, the system was in a viscous, semi-cured colloidal state. After 4 seconds of curing, the system was completely cured, resulting in a brightening film. Hardness and adhesion tests were then performed.

[0146] Brightness-enhancing film property tests: Refractive index test, using an Abbe refractometer, reference standard GB / T 614-2021, refractive index 1.5536. Transmittance measurement, using a transmittance meter, reference standard GB / T 2410-2008, transmittance 94.2%. Hardness test, using the pencil method, reference standard GB / T 6739-2006, hardness grade H. Adhesion test, using the cross-cut adhesion test, reference standard GB / T 7286-1998, where grade 0 is optimal, test result is grade 2.

[0147] Comparative Example 3 A-BPEF structure The initiator used was (2,4,6-trimethylbenzoyl)diphenylphosphine oxide (TPO), accounting for 1% of the total system mass; hydroxycyclohexanebenzophenone (184), accounting for 1% of the total system mass; the leveling agent was acrylate-modified polyether silicone BYK-333, accounting for 0.2% of the total system mass; the organic acrylate diluent was o-phenylphenoxyethyl acrylate (OPPEA), accounting for 85% of the total system mass; and 9,9-bis[4-(2-acryloyloxyethoxy)phenyl]fluorene (A-BPEF), accounting for 12.8% of the total system mass. The total mass of the formulation was 3 g. The refractive index, viscosity, and transmittance of the prepared brightening film precursor were measured.

[0148] The components were placed in a container according to their mass percentages and homogenized using a high-speed homogenizer at 2500 rpm for 5 minutes to remove bubbles and achieve uniform dispersion. The mixture was then coated onto a PET film, covered with a prism mold, and coated to a thickness of 10 μm. The mixture was then subjected to light with an intensity of 500 mJ / (s·cm²). 2 The formulation was cured under a UV mercury lamp. After 3 seconds, the system was in a viscous, semi-cured colloid state. After 7 seconds of curing, the system was completely cured, resulting in a brightening film. Hardness and adhesion tests were then performed.

[0149] Brightness-enhancing film property tests: Refractive index test, using an Abbe refractometer, reference standard GB / T 614-2021, refractive index 1.5811. Transmittance measurement, using a transmittance meter, reference standard GB / T 2410-2008, transmittance 91.2%. Hardness test, using the pencil method, reference standard GB / T 6739-2006, hardness grade H. Adhesion test, using the cross-cut adhesion test, reference standard GB / T 7286-1998, where grade 0 is optimal, test result is grade 2.

[0150] Comparative Example 4 A-MBPF structure The initiator used was (2,4,6-trimethylbenzoyl)diphenylphosphine oxide (TPO), accounting for 1% of the total system mass; hydroxycyclohexanebenzophenone (184), accounting for 1% of the total system mass; the leveling agent was organosilicon leveling agent BYK-333, accounting for 0.2% of the total system mass; the organic acrylate diluent was o-phenylphenoxyethyl acrylate (OPPEA), accounting for 85% of the total system mass; and 9,9-bis[4-(2-hydroxy-3-acryloyloxypropoxy)phenyl]fluorene (A-MBPF), accounting for 12.8% of the total system mass. The total mass of the formulation was 3 g. The refractive index, viscosity, and transmittance of the prepared brightening film precursor were measured. Each component was placed in a container according to the mass percentage and uniformly dispersed for 5 min using a high-speed homogenizer at 2500 rpm. Subsequently, the brightness enhancement film precursor was coated onto the PET film, and a prism film mold was then applied on top, with a coating thickness of 10 μm and a light intensity energy of 500 mJ / (s·cm). 2 The system was cured under a UV mercury lamp for 7 seconds to obtain a brightening film. Hardness and adhesion tests were then performed.

[0151] Brightness-enhancing film property tests: Refractive index test, using an Abbe refractometer, reference standard GB / T 614-2021, refractive index 1.5756. Transmittance measurement, using a transmittance meter, reference standard GB / T 2410-2008, transmittance 90.6%. Hardness test, using the pencil method, reference standard GB / T 6739-2006, hardness grade HB. Adhesion test, using the cross-cut adhesion test, reference standard GB / T 7286-1998, where grade 0 is optimal, test result is grade 2.

[0152] Table 1. Formulation composition (mass ratio) of Application Examples 1-6 Table 2. Formulation composition (mass ratio) of Comparative Examples 1-4 Figure 4 Images of the brightening films prepared in Application Examples 1-3 and Comparative Examples 1 and 2 are shown. The samples prepared from left to right in the top row are Application Example 1, Application Example 2, and Application Example 3, and the samples prepared in the bottom row are Comparative Example 1 and Comparative Example 2.

[0153] Figure 8 Images of the brightening films prepared in Application Examples 4-6 and Comparative Examples 3 and 4 are shown. In the top row, from left to right, the brightening film samples prepared are Application Example 4, Application Example 5, and Application Example 6, respectively. In the bottom row, from left to right, the brightening film samples prepared are Comparative Example 3 and Comparative Example 4.

[0154] Table 3 Test results of the formulations used in Examples 1-6 Table 4 Test results of the formulations in Application Examples 1-3 and Comparative Example 1 Experimental test data show that the curing times of Examples 1-6 are all shorter than those of Comparative Examples 1-4, and the suitable molecular toughness ensures the reaction efficiency of double bond curing. Regarding optical properties, the molecule exhibits good compatibility with the biphenyl diluent OPPEA, with transmittance exceeding 90%. For the highly soluble multi-EO structure compounds (Comparative Examples 1 and 2), although the transmittance of Examples 1-6 is slightly lower than that of the comparative examples, the refractive index of their formulations is far higher than that of Comparative Examples 1-2 due to the contribution of the fluorene group and sulfur to the molar refractive index. Compared to Comparative Examples 3-4 containing fluorene structures, the molecules of this invention have higher curing activity and OPPEA compatibility. Furthermore, in this embodiment, the novel sulfur-containing fluorene acrylate molecule also exhibits good hardness and adhesion. In summary, the novel sulfur-containing fluorene acrylate monomer in this technical solution possesses excellent curing activity, optical properties, and good mechanical properties, and the prepared products have broad application prospects.

[0155] This invention utilizes efficient organic reactions to obtain various di- and tri-functional high-refractive-index fluorene thioether acrylate monomers. The entire preparation process employs mature reactions, requiring no high temperature, high pressure, or hazardous reagents, and operates under mild conditions. The obtained monomers all have refractive indices higher than 1.58, providing an effective strategy for the design and fabrication of thin-film brightening agents.

[0156] The above description of the embodiments is provided to enable those skilled in the art to understand and use the invention. It will be apparent to those skilled in the art that various modifications can be made to these embodiments, and the general principles described herein can be applied to other embodiments without inventive effort. Therefore, the present invention is not limited to the above embodiments, and any improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the invention should be within the protection scope of the present invention.

Claims

1. A sulfide-based fluorene-based high-refractive-index acrylate monomer, characterized in that, The monomer is a difunctional sulfur-containing fluorene acrylate monomer or a trifunctional sulfur-containing fluorene acrylate monomer; The difunctional thiofluorenyl acrylate monomer has the following general chemical structural formula: in, for or R1 is or ; The trifunctional sulfur-containing fluorene acrylate monomer has the following general chemical structural formula: in, for , , or R2 is or ; in, n The quantity is 1-4.

2. A method for preparing the sulfide-based fluorene-based high-refractive-index acrylate monomer according to claim 1, characterized in that, The di- or tri-sulfur-containing fluorene intermediate is mixed with an acid-binding agent and a polymerization inhibitor and dissolved in a solvent. Then, an acyl chloride compound is added to react and obtain the di- or tri-sulfur-containing fluorene acrylate monomer. The structural formula of the difunctional sulfofluorene intermediate is as follows: The structural formula of the trifunctional sulfur-containing fluorene intermediate is: 。 3. The method for preparing sulfide-based fluorene-based high-refractive-index acrylate monomers according to claim 2, characterized in that, The preparation methods of the difunctional sulfonyl fluorene intermediate and the trifunctional sulfonyl fluorene intermediate include thermal initiation or photoinitiation. The thermal initiation method includes the following steps: Disubstituted or trisubstituted thiols are dissolved in a solvent with monoallyl bisphenol fluorene, a thermal initiator is added, and the reaction system is heated to the solvent reflux temperature under a protective atmosphere. The substrate undergoes a thermally initiated click reaction of mercaptoolefins to obtain the difunctional sulfur-containing fluorene intermediate or the trifunctional sulfur-containing fluorene intermediate. The photoinitiation method includes the following steps: A solvent and a photoinitiator are added to a disubstituted or trisubstituted thiol and monoallyl bisphenol fluorene. The reaction system is placed in a UV reactor under a protective atmosphere, and the substrate undergoes a photo-initiated click reaction of a mercaptoolefin to obtain the difunctional or trifunctional sulfur-containing fluorene intermediate.

4. The method for preparing sulfide-based fluorene-based high-refractive-index acrylate monomers according to claim 3, characterized in that, The disubstituted thiol is 1,3-propanedithiol or 4,4-thiodiphenylthiol. The trisubstituted thiol is polythiol 504, mesmerized trimercaptobenzene, 1,1-tris(mercaptomethyl)undecane or trimethylolpropane-tris(3-mercaptopropionate); The preparation method of the monoallyl bisphenol fluorene includes the following steps: Bisphenol fluorene and anhydrous potassium carbonate were placed in a reactor, a solvent was added, and the mixture was heated and stirred to dissolve. Monohalogenated terminal olefins were dissolved in the same solvent, and the monohalogenated terminal olefin solution was slowly added dropwise to the system. The monohalogenated terminal olefin is selected from one or more of 1-chloropropene, 1-bromopropene, 1-bromobutene, 1-iodopropene, and 1-bromohexene; The solvent used to prepare the difunctional sulfonyl fluorene intermediate or the trifunctional sulfonyl fluorene intermediate is selected from one or more of acetonitrile, acetone, dichloromethane, chloroform, and ethyl acetate; The thermal initiator is selected from one or more of azobisisobutyronitrile, azobisisoheptanenitrile, benzoyl peroxide, dicumyl peroxide, di-tert-butyl peroxide, benzoyl tert-butyl peroxide, tert-butyl peroxypentanoate, and diisopropyl peroxide. The photoinitiator is selected from one or more of benzophenone, benzoyl peroxide, 2-hydroxy-2-methyl-1-phenyl-1-propanone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, ethyl 2,4,6-trimethylbenzoylphosphonate, 1-hydroxycyclohexylphenyl ketone, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, 2-methyl-1-(4-methylthiophenyl)-2-morpholino-1-propanone, 2-isopropylthioxanthone, sodium benzophenone-4-sulfonate, 2-hydroxy-4-(2-hydroxyethoxy)-2-methylphenylpropanone, 2-ethylanthraquinone, 4-methylbenzophenone, and tetraethylmichalcohol.

5. The method for preparing sulfide-based fluorene-based high-refractive-index acrylate monomers according to claim 3, characterized in that, In the thermal initiation method, the heating temperature is 36~150℃ and the time is 12~26 h; In the thermal initiation method, the molar ratio of disubstituted thiols, monoallyl bisphenol fluorene, and thermal initiator is 1:(2-4):(0.01-1). In the thermal initiation method, the molar ratio of trisubstituted thiol, monoallyl bisphenol fluorene, and thermal initiator is 1:(3-6):(0.01-1). In the photoinitiation method, the ultraviolet light wavelength is 365 nm and the power is 20 watts; In the photoinitiation method, the molar ratio of disubstituted thiols, monoallyl bisphenol fluorene, and photoinitiator is 1:(2-5):(0.01-1). In the photoinitiation method, the molar ratio of trisubstituted thiol, monoallyl bisphenol fluorene, and photoinitiator is 1:(3-6):(0.01-1).

6. The method for preparing sulfide-based fluorene-based high-refractive-index acrylate monomers according to claim 2, characterized in that, The acid-binding agent is an inorganic or organic compound that can react with the hydrogen chloride generated during the process; The inorganic compound is selected from one or more of potassium carbonate, sodium carbonate, cesium carbonate, and sodium bicarbonate. The organic compound is selected from triethylamine, ethylenediamine, trimethylamine, pyridine, N , N One or more of the alkylamide class of compounds; The polymerization inhibitor is a compound that can prevent the self-polymerization of the product during the reaction heating process; The polymerization inhibitor is selected from one or more of hydroquinones, p-methoxyphenol, phenothiazines, or p-tert-butylphenol; The acyl chloride compound is acryloyl chloride or methacryloyl chloride; The solvent is a liquid compound that can dissolve the raw material but will not react with acyl chloride; The solvent is selected from one or more of halogenated hydrocarbons, ethers, tetrahydrofurans, and benzene derivatives.

7. The method for preparing sulfide-based fluorene-based high-refractive-index acrylate monomers according to claim 2, characterized in that, The molar ratio of the acid-binding agent, polymerization inhibitor, acyl chloride compound, and difunctional sulfur-containing fluorene intermediate is (2-6):(0.01-1):(1-4):1; The molar ratio of the acid-binding agent, polymerization inhibitor, acyl chloride compound and trifunctional sulfur-containing fluorene intermediate is (4-8):(0.01-1):(4-6):

1.

8. The method for preparing sulfide-based fluorene-based high-refractive-index acrylate monomers according to claim 2, characterized in that, When preparing difunctional thiofluorenyl acrylate monomers, an acyl chloride compound is added under ice bath conditions, and the difunctional thiofluorenyl acrylate monomers are obtained by heating and reflux reaction. The heating and reflux reaction temperature is 36~150℃, and the reflux reaction time is 12~26 h; When preparing trifunctional sulfur-containing fluorene acrylate monomers, an acyl chloride compound is added under ice bath conditions, and the reaction is carried out at room temperature to obtain the trifunctional sulfur-containing fluorene acrylate monomers.

9. The application of the sulfide-based fluorene-based high-refractive-index acrylate monomer according to claim 2, characterized in that, The sulfide-based fluorene-based high-refractive-index acrylate monomer was used to prepare a brightening film; The method for preparing the brightness enhancement film includes the following steps: The sulfide-based fluorene-based high-refractive-index acrylate monomer is uniformly mixed with an active diluent, and then a curing photoinitiator and a silicone-containing leveling agent are added. The resulting mixture is coated onto a PET film and then photocured to obtain an optical device brightness enhancement film.

10. The application of the sulfide-based fluorene-based high-refractive-index acrylate monomer according to claim 9, characterized in that, When the sulfide-based fluorene-based high-refractive-index acrylate monomer is a difunctional sulfofluorene-containing acrylate monomer: The active diluent is selected from one or more of the following: polyethylene glycol o-phenylphenyl ether acrylate, ethoxyphenol acrylate, benzyl acrylate, benzyl methacrylate, dicyclopentadienyl acrylate, o-phenylphenoxyethyl acrylate, 2-hydroxyethyl acrylate, tetrahydrofuran acrylate, N-acryloylmorpholine, isobornyl acrylate, isobornyl methacrylate, and 4-phenylbutyl acrylate. The curing photoinitiator is selected from one or more of the following: 2-hydroxy-2-methyl-1-phenyl-1-propanone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, ethyl 2,4,6-trimethylbenzoylphosphonate, 1-hydroxycyclohexylphenyl ketone, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, 2-methyl-1-(4-methylthiophenyl)-2-morpholino-1-propanone, 2-isopropylthioxanthone, sodium benzophenone-4-sulfonate, 2-hydroxy-4-(2-hydroxyethoxy)-2-methylphenylpropanone, 2-ethylanthraquinone, 4-methylbenzophenone, and tetraethylmichalcohol. The silicone-containing leveling agent is selected from one or more of the following: BYK-320, BYK-322, BYK-077, BYK-325N, BYK-310, BYK-307, BYK-306, BYK-315N, BYK-329, BYK-333, TEGO10, TEGO41, TEGO432, TEGO435, TEGO450, TEGO482, SF3288, FL3777AN, FL3670, LEVELOL835, WE-D846R, WE-D888N, WE-D819C, and WE-D881R. The molar ratio of the difunctional sulfur-containing fluorene acrylate monomer to the reactive diluent is 1:6~10; The total mass fraction of the curing photoinitiator accounts for 0.5% to 5% of the mixed system; The total mass fraction of the silicone-containing leveling agent accounts for 0.05% to 0.5% of the mixed system; When the sulfide-based fluorene-based high-refractive-index acrylate monomer is a trifunctional sulfide-containing fluorene-based acrylate monomer: The reactive diluent is selected from one or more of biphenylmethanol acrylate, methyl 2-acrylate (4-phenoxyphenyl) acrylate, and o-phenylphenoxyethyl acrylate; The curing photoinitiator is selected from one or more of the following: methyl benzoylcarbamate, trimethylbenzoyl diphenylphosphine oxide, benzophenone, tetraethylmiel ketone, 4-methylbenzophenone, methyl o-benzoylbenzoate, 2-hydroxy-2-methyl-1-phenylpropanone, 1-hydroxycyclohexylphenyl ketone, and 2-ethylanthraquinone. The silicone leveling agent is selected from one or more of the following: acrylate-modified polyether silicone Tego rad 2500, polydimethylsilane, polymethylphenylsiloxane, and silicone leveling agent BKY-333. The molar ratio of the trifunctional sulfur-containing fluorene acrylate monomer to the reactive diluent is 1:6~10; The total mass fraction of the curing photoinitiator accounts for 0.5% to 2% of the mixed system; The total mass fraction of the silicone-containing leveling agent accounts for 0.1% to 0.5% of the mixed system.

Citation Information

Patent Citations

  • Fluorenyl-containing acrylate polymer and fluorenyl-containing photosensitive composition

    CN114621429A

  • High-refractive-index resin wafer based on sulfur-containing organic matter modification and preparation method of high-refractive-index resin wafer

    CN117659469A