A water-based metal rust inhibitor based on succinic anhydride derivative, its preparation method and application

By preparing a succinic anhydride derivative water-based metal rust inhibitor, the problems of insufficient rust prevention and poor solubilization of existing water-based rust inhibitors have been solved, achieving environmentally friendly and efficient rust prevention and solubilization effects, suitable for various environments and processing techniques.

CN123106542APending Publication Date: 2026-11-17深圳市如钦巴化学材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611295082.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-25
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing water-based metal rust inhibitors suffer from problems such as insufficient rust prevention performance, poor solubilization performance, poor environmental protection, weak compatibility, and high cost, making it difficult to meet industrial needs.

Method used

Using succinic anhydride derivatives as the main components, a water-based metal rust inhibitor with both rust-preventing and solubilizing properties is prepared through the reaction of maleic anhydride with imidazoline and alkenyl succinic anhydride, avoiding the use of toxic substances such as nitrites and dichromates.

Benefits of technology

It achieves environmentally friendly and non-toxic high-efficiency rust prevention and good solubilization effect, simplifies cutting fluid formulation, reduces costs, and is suitable for various environments and subsequent processing techniques.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123106542A_ABST
    Figure CN123106542A_ABST
Patent Text Reader

Abstract

This application provides a succinic anhydride derivative water-based metal rust inhibitor, its preparation method, and its application. The succinic anhydride derivative water-based metal rust inhibitor has the structure shown in Formula I. The succinic anhydride derivative water-based metal rust inhibitor of this application has both good solubilizing effect and overcomes the problem that current cutting fluid rust inhibitors have no solubilizing properties and poor rust-preventing properties due to solubilizing properties. It combines good rust-preventing and solubilizing properties, greatly simplifies the cutting fluid formulation, and reduces the overall cost of the formulation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of rust inhibitor technology, and relates to a succinic anhydride derivative water-based metal rust inhibitor, its preparation method and application. Background Technology

[0002] Metal materials and products are susceptible to corrosion from moisture, salt, acids and alkalis in the environment during production, storage, transportation and use, which can lead to damage to appearance, performance degradation or even scrapping, causing serious economic losses. Therefore, metal rust prevention is an indispensable part of the manufacturing industry.

[0003] Traditional rust prevention technologies mostly use oil-based rust inhibitors, which can achieve a certain rust prevention effect, but have drawbacks such as the need for additional degreasing after use, high VOC emissions, environmental pollution, and high production costs, making it difficult to meet the current green and environmentally friendly industrial policies and production needs.

[0004] Water-based metal rust inhibitors, using water as the primary medium, offer advantages such as environmental friendliness, zero VOC emissions, ease of use, no need for subsequent degreasing, and low cost, making them a mainstream alternative to oil-based rust inhibitors. However, current water-based metal rust inhibitors still face several technical bottlenecks: The mainstream rust inhibitors used in water-based cutting fluids include tribasic acids, sebacic acid, neodecanoic acid, and dodecanoic acid. Tribasic acids contain chloride ions, which can easily cause pitting corrosion in metal materials; sebacic acid has relatively limited rust-preventive performance; neodecanoic acid has an irritating odor, making it inconvenient to use on-site; and dodecanoic acid has poor resistance to hard water. Furthermore, there are no products on the market that balance rust prevention and solubilization, leading to complex cutting fluid formulations and increased additive usage. Some rust inhibitor products use toxic components such as nitrites and chromates, posing environmental and safety risks. Additionally, existing products suffer from issues such as easy flash rusting in low-temperature, high-humidity environments and poor compatibility with subsequent coating processes. Furthermore, the key corrosion inhibitors for high-end water-based metal rust inhibitors rely on imports, and the nanocomposite modification technology is limited by poor dispersibility and high cost, making it difficult to achieve industrial-scale promotion.

[0005] Therefore, developing an environmentally friendly, non-toxic, rust-preventive, solubilizing, highly adaptable, and cost-controllable water-based metal rust inhibitor to address the shortcomings of existing technologies and meet the actual needs of metal protection in various industries has become a pressing technical problem for those skilled in the art. Summary of the Invention

[0006] To address the shortcomings of existing technologies, the purpose of this application is to provide a succinic anhydride derivative water-based metal rust inhibitor, its preparation method, and its application. The succinic anhydride derivative water-based metal rust inhibitor of this application possesses both excellent rust-preventive and solubilizing properties.

[0007] To achieve this objective, the present application adopts the following technical solution: On the one hand, this application provides a succinic anhydride derivative water-based metal rust inhibitor, wherein the succinic anhydride derivative water-based metal rust inhibitor has the structure shown in Formula I below: ; R is selected from alkenyl groups of C6-C20.

[0008] The succinic anhydride derivative water-based metal rust inhibitor of this application not only has excellent rust-preventive properties but also good solubilizing effects. It is environmentally friendly and non-toxic, avoiding the use of toxic substances such as nitrites and dichromates, and possesses highly efficient rust-preventive performance. Furthermore, the succinic anhydride derivative water-based metal rust inhibitor of this application also has excellent solubilizing effects, overcoming the problem that current cutting fluid rust inhibitors lack solubilizing properties and have poor rust-preventive performance due to solubilization.

[0009] In some implementations, R is selected from... , , , , , , , or .

[0010] On the other hand, this application provides a method for preparing the succinic anhydride derivative water-based metal rust inhibitor as described above, wherein the preparation method is any one of method 1 to method 3; Method 1 includes the following steps: (1) Maleic anhydride reacts with imidazoline to give intermediate product A, as shown in the following reaction formula: (2) Intermediate product A reacts with alkenyl succinic anhydride B to obtain the succinic anhydride derivative water-based metal rust inhibitor; the reaction formula is as follows: ; Method 2 includes the following steps: I. Alkenyl succinic anhydride B reacts with imidazoline to give intermediate product C, as shown in the following reaction formula: ; II. Intermediate product C reacts with maleic anhydride to obtain the succinic anhydride derivative water-based metal rust inhibitor; the reaction formula is as follows: ; Method 3 includes the following steps: Maleic anhydride was reacted with imidazoline and alkenyl succinic anhydride B to obtain the succinic anhydride derivative water-based metal rust inhibitor, as shown in the following reaction formula: .

[0011] In some embodiments, the molar ratio of imidazoline to maleic anhydride in step (1) is 1:0.8 to 1.3, for example, 1:0.8, 1:0.9, 1:1, 1:1.1, 1:1.2 or 1:1.3.

[0012] In some embodiments, step (1) involves melting the maleic anhydride at 50-70°C (e.g., 50°C, 55°C, 60°C, 65°C, or 70°C) before reacting it with imidazoline, and then adding imidazoline dropwise to the molten maleic anhydride.

[0013] In some embodiments, the temperature of the reaction in step (1) is 70~100℃ (e.g., 70℃, 72℃, 74℃, 76℃, 78℃, 80℃, 82℃, 84℃, 86℃, 88℃, 90℃, 92℃, 94℃, 96℃ or 100℃, etc.), preferably 80~90℃.

[0014] In some embodiments, the reaction time in step (1) is 0.5-2h (e.g., 0.5h, 0.7h, 0.9h, 1.1h, 1.3h, 1.5h, 1.7h, 1.9h or 2h, etc.), preferably 1h.

[0015] In some embodiments, the molar ratio of the alkenyl succinic anhydride B in step (2) to the imidazoline in step (1) is 1:0.8 to 1.3, for example, 1:0.8, 1:0.9, 1:1, 1:1.1, 1:1.2 or 1:1.3, etc.

[0016] In some embodiments, the alkenyl succinic anhydride B in step (2) is selected from one or a combination of at least two of the following: straight-chain or branched octenyl succinic anhydride, nonenyl succinic anhydride, decenyl succinic anhydride, dodecenyl succinic anhydride, tetradecenyl succinic anhydride, hexadecenyl succinic anhydride, or octadecenyl succinic anhydride.

[0017] In some embodiments, the reaction temperature in step (2) is 70~100℃ (e.g., 70℃, 72℃, 74℃, 76℃, 78℃, 80℃, 82℃, 84℃, 86℃, 88℃, 90℃, 92℃, 94℃, 96℃ or 100℃, etc.), preferably 80~90℃.

[0018] In some embodiments, the reaction time in step (2) is more than 1 hour (e.g., 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 8 hours, etc.), preferably 3 hours.

[0019] In some embodiments, the reactions described in steps (1) and (2) are carried out under the protection of a protective gas. In some embodiments, the protective gas is nitrogen.

[0020] In some embodiments, the molar ratio of the alkenyl succinic anhydride B to the imidazoline in step I is 1:0.8 to 1.3, for example, 1:0.8, 1:0.9, 1:1, 1:1.1, 1:1.2 or 1:1.3.

[0021] In some embodiments, the alkenyl succinic anhydride B in step I is selected from one or a combination of at least two of the following: straight-chain or branched octenyl succinic anhydride, nonenyl succinic anhydride, decenyl succinic anhydride, dodecenyl succinic anhydride, tetradecenyl succinic anhydride, hexadecenyl succinic anhydride, or octadecenyl succinic anhydride.

[0022] In some embodiments, the reaction temperature in step I is 70~100°C (e.g., 70°C, 72°C, 74°C, 76°C, 78°C, 80°C, 82°C, 84°C, 86°C, 88°C, 90°C, 92°C, 94°C, 96°C, or 100°C, etc.), preferably 80~90°C.

[0023] In some embodiments, the reaction time in step I is 0.5-2 hours (e.g., 0.5 hours, 0.7 hours, 0.9 hours, 1.1 hours, 1.3 hours, 1.5 hours, 1.7 hours, 1.9 hours, or 2 hours), preferably 1 hour.

[0024] In some embodiments, the molar ratio of maleic anhydride in step II to imidazoline in step I is 0.8 to 1.3:1.

[0025] In some embodiments, the reaction temperature in step II is 70~100°C (e.g., 70°C, 72°C, 74°C, 76°C, 78°C, 80°C, 82°C, 84°C, 86°C, 88°C, 90°C, 92°C, 94°C, 96°C, or 100°C, etc.), preferably 80~90°C.

[0026] In some embodiments, the reaction time in step II is more than 1 hour (e.g., 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 8 hours, etc.), preferably 3 hours.

[0027] In some embodiments, the reactions described in steps I and II are carried out under a protective gas atmosphere. In some embodiments, the protective gas is nitrogen.

[0028] In some embodiments, the molar ratio of the imidazoline to maleic anhydride in method 3 is 1:0.8 to 1.3 (e.g., 1:0.8, 1:0.9, 1:1, 1:1.1, 1:1.2, or 1:1.3, etc.), and the molar ratio of the alkenyl succinic anhydride B to the imidazoline is 1:0.8 to 1.3 (e.g., 1:0.8, 1:0.9, 1:1, 1:1.1, 1:1.2, or 1:1.3, etc.).

[0029] In some embodiments, in method 3, alkenyl succinic anhydride and imidazoline are simultaneously added dropwise to molten maleic anhydride for reaction, wherein the maleic anhydride is molten at 50-70°C (e.g., 50°C, 55°C, 60°C, 65°C, or 70°C).

[0030] In some embodiments, the reaction temperature in method 3 is 70-100°C (e.g., 70°C, 72°C, 74°C, 76°C, 78°C, 80°C, 82°C, 84°C, 86°C, 88°C, 90°C, 92°C, 94°C, 96°C, or 100°C, etc.), and the reaction time is more than 1 hour (e.g., 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 8 hours, etc.), preferably 3 hours.

[0031] In some embodiments, the reaction in method 3 is carried out under the protection of a protective gas. In some embodiments, the protective gas is nitrogen.

[0032] On the other hand, this application provides a metal surface rust-preventing treatment liquid, which includes a water-based lubricant or metal cleaner, as well as a succinic anhydride derivative water-based metal rust inhibitor as described above.

[0033] Preferably, the amount of succinic anhydride derivative water-based metal rust inhibitor added to the metal surface rust prevention treatment liquid is 0.5 to 3.0 wt% (e.g., 0.5 wt%, 1 wt%, 1.5 wt%, 2 wt%, or 3 wt%).

[0034] On the other hand, this application provides the application of the succinic anhydride derivative water-based metal rust inhibitor as described above or the metal surface rust prevention treatment liquid as described above in metal surface rust prevention treatment.

[0035] Compared with the prior art, this application has the following advantages: The succinic anhydride derivative water-based metal rust inhibitor of this application is environmentally friendly and non-toxic, avoiding the use of toxic substances such as nitrites and dichromates, and possesses highly efficient rust-preventing properties. This succinic anhydride derivative water-based metal rust inhibitor also has excellent solubilizing effects, overcoming the problem that current cutting fluid rust inhibitors lack solubilizing properties while having poor rust-preventing performance due to solubilization. It combines excellent rust-preventing and solubilizing properties, greatly simplifying cutting fluid formulations and reducing overall formulation costs. This succinic anhydride derivative water-based metal rust inhibitor can also be used in the metal cleaning field, suitable for inter-process rust prevention without affecting subsequent workpiece processing. Attached Figure Description

[0036] Figure 1 This is a comparison chart of the rust-preventive performance test results of the succinic anhydride derivative of Example 1 and the sebacic acid of Comparative Example 1.

[0037] Figure 2The graph shows the rust-preventive performance test results of the succinic anhydride derivative in Example 2.

[0038] Figure 3 The graph shows the rust-preventive performance test results of the succinic anhydride derivative in Example 3.

[0039] Figure 4 The graph shows the rust-preventive performance test results of the succinic anhydride derivative in Example 4.

[0040] Figure 5 The graph shows the rust-preventive performance test results of the succinic anhydride derivative in Example 5.

[0041] Figure 6 The graph shows the rust-preventive performance test results of the succinic anhydride derivative in Example 6.

[0042] Figure 7 The graph shows the rust-preventive performance test results of the succinic anhydride derivative in Example 7. Detailed Implementation

[0043] The technical solution of this application will be further described below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely to help understand this application and should not be regarded as specific limitations on this application.

[0044] Example 1 This embodiment provides a succinic anhydride derivative water-based metal rust inhibitor, the preparation method of which includes the following steps: 88 g (0.9 mol) of maleic anhydride was placed in a reaction vessel, nitrogen gas was introduced, and the mixture was heated to 60 °C. 72 g (1 mol) of imidazoline was slowly added dropwise to the reaction vessel under stirring. The temperature was raised to 90 °C and reacted at this temperature for 1 h. Subsequently, 210 g (1 mol) of 2-octenylsuccinic anhydride was slowly added dropwise to the reaction vessel. After the addition was complete, the reaction was maintained at 90 °C for 1 h. After the reaction was completed, the target succinic anhydride derivative was obtained.

[0045] Example 2 This embodiment provides a succinic anhydride derivative water-based metal rust inhibitor, the preparation method of which includes the following steps: 88 g (0.9 mol) of maleic anhydride was placed in a reaction vessel, nitrogen gas was introduced, and the mixture was heated to 60 °C. 72 g (1 mol) of imidazoline was slowly added dropwise to the reaction vessel under stirring. The temperature was then raised to 90 °C and reacted at this temperature for 1 hour. Subsequently, 224 g (1 mol) of nonenylsuccinic anhydride was slowly added dropwise to the reaction vessel. After the addition was complete, the reaction was maintained at 90 °C for 1 hour. After the reaction was completed, the target succinic anhydride derivative was obtained.

[0046] Example 3 This embodiment provides a succinic anhydride derivative water-based metal rust inhibitor, the preparation method of which includes the following steps: 88 g (0.9 mol) of maleic anhydride was placed in a reaction vessel, nitrogen gas was introduced, and the mixture was heated to 60 °C. 72 g (1 mol) of imidazoline was slowly added dropwise to the reaction vessel under stirring. The temperature was then raised to 90 °C and reacted at this temperature for 1 hour. Subsequently, 238 g (1 mol) of decenylsuccinic anhydride was slowly added dropwise to the reaction vessel. After the addition was complete, the reaction was maintained at 90 °C for 1 hour. After the reaction was completed, the target succinic anhydride derivative was obtained.

[0047] Example 4 This embodiment provides a succinic anhydride derivative water-based metal rust inhibitor, the preparation method of which includes the following steps: 98 g (1 mol) of maleic anhydride was placed in a reaction vessel, nitrogen gas was introduced, and the mixture was heated to 60 °C. 72 g (1 mol) of imidazoline was slowly added dropwise to the reaction vessel under stirring. The temperature was then raised to 90 °C and reacted at this temperature for 1 hour. Subsequently, 266 g (1 mol) of dodecenylsuccinic anhydride was slowly added dropwise to the reaction vessel. After the addition was complete, the reaction was maintained at 90 °C for 1 hour. After the reaction was completed, the target succinic anhydride derivative was obtained.

[0048] Example 5 This embodiment provides a succinic anhydride derivative water-based metal rust inhibitor, the preparation method of which includes the following steps: 88 g (0.9 mol) of maleic anhydride was placed in a reaction vessel, nitrogen gas was introduced, and the mixture was heated to 60 °C. 72 g (1 mol) of imidazoline was slowly added dropwise to the reaction vessel under stirring. The temperature was raised to 90 °C and reacted at this temperature for 1 h. Subsequently, 294 g (1 mol) of tetradecenyl succinic anhydride was slowly added dropwise to the reaction vessel. After the addition was complete, the reaction was maintained at 90 °C for 3 h. After the reaction was completed, the target succinic anhydride derivative was obtained.

[0049] Example 6 This embodiment provides a succinic anhydride derivative water-based metal rust inhibitor, the preparation method of which includes the following steps: 72 g (1 mol) of imidazoline was placed in a reaction vessel, nitrogen gas was introduced, and the mixture was heated to 60 °C. Under stirring, 322.5 g (1 mol) of hexadecenylsuccinic anhydride was slowly added dropwise to the reaction vessel. The temperature was raised to 80 °C and the reaction was maintained at this temperature for 2 h. Subsequently, 88 g (1 mol) of maleic anhydride was added to the reaction vessel in batches. After the addition was complete, the reaction was maintained at 80 °C for 3 h. After the reaction was completed, the target succinic anhydride derivative was obtained.

[0050] Example 7 This embodiment provides a succinic anhydride derivative water-based metal rust inhibitor, the preparation method of which includes the following steps: 88 g (0.9 mol) of maleic anhydride was placed in a reaction vessel, nitrogen gas was introduced, and the mixture was heated to 60 °C. Under stirring, 72 g (1 mol) of imidazoline and 350.5 g (1 mol) of octadecenyl succinic anhydride were simultaneously added dropwise to the reaction vessel, and the temperature was raised to 80 °C and reacted at this temperature for 3 hours. After the reaction was completed, the target succinic anhydride derivative was obtained.

[0051] Application Example 1 The rust-preventive performance of the succinic anhydride derivative obtained in Example 1 was compared with that of sebacic acid, a commonly used rust inhibitor. The rust-preventive performance test was conducted in accordance with the mechanical industry standard JB / T 9189-2016. The preparation process of the rust-preventive solution is as follows: The compound obtained in Example 1 was added at 2%, along with 10% triethanolamine, 2% diethanolamine, and 86% pure water, to obtain a rust inhibitor stock solution containing the rust inhibitor stock solution of Example 1. The rust inhibitor stock solution was diluted with tap water at a ratio of 1:20 to obtain the rust inhibitor dilution solution 1 used in the test. Sebacic acid was added at 2%, along with 10% triethanolamine, 2% diethanolamine, and 86% pure water, to obtain a rust inhibitor stock solution containing sebacic acid. The rust inhibitor stock solution was diluted with tap water at a ratio of 1:20 to obtain the comparative rust inhibitor dilution solution 1 used in the test. Rust prevention performance testing was conducted according to the mechanical industry standard JB / T 9189-2016.

[0052] Comparison of the rust-preventive properties of succinic anhydride derivatives and sebacic acid in Example 1 Figure 1 As shown, it can be seen that the rust-preventive effect of the succinic anhydride derivative in Example 1 is significantly better than that of sebacic acid.

[0053] Application Example 2 The succinic anhydride derivative obtained in Example 2 was added at 2%, along with 10% triethanolamine, 2% diethanolamine, and 86% pure water, to obtain the rust inhibitor stock solution containing the solution from Example 2. The rust inhibitor stock solution was diluted with tap water at a ratio of 1:20 to obtain the rust inhibitor diluted solution 2 used in the test. Rust prevention performance testing was conducted according to the mechanical industry standard JB / T 9189-2016.

[0054] The rust-preventive performance test results of the succinic anhydride derivative in Example 2 are as follows: Figure 2 As shown, it can be seen that the rust-preventive effect of the succinic anhydride derivative in Example 2 is significantly better than that of sebacic acid.

[0055] Application Example 3 The succinic anhydride derivative obtained in Example 3 was added at 2%, along with 10% triethanolamine, 2% diethanolamine, and 86% pure water, to obtain the rust inhibitor stock solution containing the solution from Example 2. The rust inhibitor stock solution was diluted with tap water at a ratio of 1:20 to obtain the rust inhibitor diluted solution 2 used in the test. Rust prevention performance testing was conducted according to the mechanical industry standard JB / T 9189-2016.

[0056] The rust-preventive performance test results of the succinic anhydride derivative in Example 3 are as follows: Figure 3 As shown, it can be seen that the rust-preventive effect of the succinic anhydride derivative in Example 3 is significantly better than that of sebacic acid.

[0057] Application Examples 4-7 Unlike Application Example 1, the succinic anhydride derivative of Example 1 was replaced with the succinic anhydride derivatives of Examples 4-7. Its rust-preventive performance was excellent, with no rust formation observed during the test period.

[0058] The rust-preventive performance test results of the succinic anhydride derivatives in Examples 4-7 are as follows: Figures 4-7 As shown, it can be seen that the rust-preventive effect of the succinic anhydride derivatives in Examples 4-7 is significantly better than that of sebacic acid.

[0059] Application Example 8 The solubilizing properties of the succinic anhydride derivative obtained in Example 1 were compared with those of neodecanoic acid, a commonly used solubilizing solvent. The preparation process of the comparative formulation is as follows: Add 10g of 1720 to a beaker, then add 10g of triethanolamine, 2g of diethanolamine, and 74g of pure water. While stirring, add the product obtained in Example 1 to the system until the system is clear and transparent, consuming 4g of the product obtained in Example 1.

[0060] Neodecanoic acid solubilization test: Add 10g of 1720 to a beaker, add 10g of triethanolamine, 2g of diethanolamine, and 74g of pure water. Add neodecanoic acid to the system while stirring until the system is clear and transparent, consuming 6g of neodecanoic acid.

[0061] The solubilization properties were tested using the succinic anhydride derivatives from Examples 2-7, in the same manner as the experiments described above, except that the succinic anhydride derivatives obtained in Example 1 were replaced with the succinic anhydride derivatives from Examples 2-7. The test results are shown in Table 1.

[0062] Table 1 The applicant declares that this application illustrates the succinic anhydride derivative water-based metal rust inhibitor, its preparation method, and its application through the above embodiments. However, this application is not limited to the above embodiments, meaning that this application does not necessarily rely on the above embodiments for implementation. Those skilled in the art should understand that any improvements to this application, equivalent substitutions of the raw materials used, additions of auxiliary components, and selection of specific methods, etc., all fall within the protection and disclosure scope of this application.

Claims

1. A succinic anhydride derivative water-based metal rust inhibitor, characterized in that, The succinic anhydride derivative water-based metal rust inhibitor has the structure shown in Formula I: ; R is selected from alkenyl groups of C6-C20.

2. The succinic anhydride derivative water-based metal rust inhibitor according to claim 1, characterized in that, R is selected from , , , , , , , or .

3. The preparation method of the succinic anhydride derivative water-based metal rust inhibitor according to claim 1 or 2, characterized in that, The preparation method is any one of method 1 to method 3; Method 1 includes the following steps: (1) Maleic anhydride reacts with imidazoline to give intermediate product A, as shown in the following reaction formula: ; (2) Intermediate product A reacts with alkenyl succinic anhydride B to obtain the succinic anhydride derivative water-based metal rust inhibitor; the reaction formula is as follows: ; Method 2 includes the following steps: I. Alkenyl succinic anhydride B reacts with imidazoline to give intermediate product C, as shown in the following reaction formula: ; II. Intermediate product C reacts with maleic anhydride to obtain the succinic anhydride derivative water-based metal rust inhibitor; the reaction formula is as follows: ; Method 3 includes the following steps: Maleic anhydride was reacted with imidazoline and alkenyl succinic anhydride B to obtain the succinic anhydride derivative water-based metal rust inhibitor, as shown in the following reaction formula: 。 4. The preparation method according to claim 3, characterized in that, The molar ratio of imidazoline to maleic anhydride in step (1) is 1:0.8~1.3; And / or, in step (1), before reacting maleic anhydride with imidazoline, maleic anhydride is melted at 50-70°C, and then imidazoline is added dropwise to the molten maleic anhydride. And / or, the temperature of the reaction in step (1) is 70~100℃, preferably 80~90℃; And / or, the reaction time in step (1) is 0.5-2 hours, preferably 1 hour; And / or, the molar ratio of the alkenyl succinic anhydride B in step (2) to the imidazoline in step (1) is 1:0.8~1.3; And / or, the alkenyl succinic anhydride B in step (2) is selected from one or a combination of at least two of the following: straight-chain or branched octenyl succinic anhydride, nonenyl succinic anhydride, decenyl succinic anhydride, dodecenyl succinic anhydride, tetradecenyl succinic anhydride, hexadecenyl succinic anhydride or octadecenyl succinic anhydride. And / or, the temperature of the reaction in step (2) is 70~100℃, preferably 80~90℃; And / or, the reaction time in step (2) is more than 1 hour, preferably 3 hours; And / or, the reactions described in steps (1) and (2) are carried out under the protection of a protective gas, namely nitrogen.

5. The preparation method according to claim 3, characterized in that, The molar ratio of alkenyl succinic anhydride B to imidazoline in step I is 1:0.8~1.3; And / or, the alkenyl succinic anhydride B in step I is selected from one or a combination of at least two of the following: straight-chain or branched octenyl succinic anhydride, nonenyl succinic anhydride, decenyl succinic anhydride, dodecenyl succinic anhydride, tetradecenyl succinic anhydride, hexadecenyl succinic anhydride or octadecenyl succinic anhydride. And / or, the reaction temperature in step I is 70~100℃, preferably 80~90℃; And / or, the reaction time in step I is 0.5-2 hours, preferably 1 hour; And / or, the molar ratio of maleic anhydride in step II to imidazoline in step I is 0.8~1.3:1; And / or, in step II, maleic anhydride is melted at 50-70°C before reacting with intermediate product C; And / or, the reaction temperature in step II is 70~100℃, preferably 80~90℃; And / or, the reaction time in step II is more than 1 hour, preferably 3 hours; And / or, the reactions described in steps I and II are carried out under a protective gas, namely nitrogen.

6. The preparation method according to claim 3, characterized in that, In Method 3, the molar ratio of imidazoline to maleic anhydride is 1:0.8~1.3, and the molar ratio of alkenyl succinic anhydride B to imidazoline is 1:0.8~1.

3.

7. The preparation method according to claim 3, characterized in that, In method 3, alkenyl succinic anhydride and imidazoline are simultaneously added dropwise to molten maleic anhydride to carry out the reaction, wherein the maleic anhydride is molten at 50~70℃; And / or, the reaction temperature in method 3 is 70-100°C, and the reaction time is more than 1 hour, preferably 3 hours; And / or, the reaction described in method 3 is carried out under a protective gas atmosphere. In some embodiments, the protective gas is nitrogen.

8. A rust-preventive liquid for metal surfaces, characterized in that, The metal surface rust prevention treatment liquid includes water-based lubricant or metal cleaning agent, as well as the succinic anhydride derivative water-based metal rust inhibitor as described in claim 1 or 2.

9. The metal surface rust-preventive treatment liquid according to claim 8, characterized in that, The amount of succinic anhydride derivative water-based metal rust inhibitor added to the metal surface rust prevention treatment solution is 0.5-3.0 wt%.

10. The application of the succinic anhydride derivative water-based metal rust inhibitor according to claim 1 or 2, or the metal surface rust-preventing treatment liquid according to claim 8 or 9, in the rust-preventing treatment of metal surfaces.