A resin, its preparation method and uses
By designing resins with specific structures and preparing photoresists through anionic polymerization and coupling reactions, the problems of insufficient development contrast and high edge roughness are solved, achieving high-precision pattern transfer and excellent etching performance, suitable for integrated circuits and optoelectronic products.
Patent Information
- Application Number
- CN202611532087.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-30
- Publication Date
- 2026-11-17
AI Technical Summary
Existing chemically amplified photoresists suffer from insufficient contrast between exposed and unexposed areas, high edge roughness, and poor etching resistance, which affect pattern transfer accuracy and device performance.
A resin containing specific repeating units was designed and prepared by anionic polymerization and coupling reaction. The resulting photoresist exhibits significant contrast and improved edge steepness during exposure, while maintaining excellent etching resistance.
The development process improves the steepness of the pattern sidewalls, reduces the roughness of the photoresist edges, and results in clear etched patterns, making it suitable for integrated circuits and optoelectronic products.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of photoresist technology, specifically to a resin, its preparation method, and its uses. Background Technology
[0002] Photoresist (or photoresist) is a core material in semiconductor photolithography, and its properties determine the quality of the final micro-pattern. Among them, chemically amplified resist (CAR) has become the mainstream photoresist material in current advanced photolithography processes due to its outstanding advantages such as high photosensitivity, high resolution, and strong process adaptability. It is widely used in mainstream photolithography processes such as KrF and ArF, as well as in the fabrication of micro-patterns. Its core principle is: during exposure, the photoacid generator (PAG) absorbs light energy and decomposes to produce a strong acid; during the post-baking process, this acid acts as a catalyst, efficiently inducing a large number of acid-sensitive groups on the resin to react, thereby realizing the catalysis of multiple chemical reactions by a single photon, which greatly improves the sensitivity of the photoresist.
[0003] Despite the great success of chemically amplified photoresist technology, key issues still need to be addressed in existing KrF photoresist systems: Insufficient development contrast: The existing CAR resin does not exhibit a significant difference in dissolution rate between the exposed and unexposed areas, resulting in insufficient steepness of the pattern sidewalls during development and decreased pattern transfer accuracy. This low contrast limits further improvements in resolution.
[0004] High Line Edge Roughness (LER / Line Width Roughness (LWR): The roughness of the pattern edges is a key factor affecting device performance and yield. In existing technologies, due to the influence of factors such as acid diffusion control, resin molecular weight distribution, and development kinetics, the resulting pattern edges often exhibit irregular fluctuations and high roughness, directly affecting the electrical performance and reliability of the device.
[0005] Etching resistance matching issues: Although chemical amplification improves photosensitivity, the inherent structure or reaction products of some CAR resins make their corrosion resistance relatively insufficient in subsequent plasma etching processes, which may lead to unclear etching boundaries, deterioration of pattern morphology, and ultimately affect the size control of the device. Summary of the Invention
[0006] This invention provides a resin, its preparation method, and its uses to solve the problems of insufficient contrast between exposed and non-exposed areas, excessively high edge roughness, or poor etching resistance in existing photoresists.
[0007] Therefore, the present invention provides a resin having the structural formula shown in formula (I):
[0008] (I); Wherein, at least one of group M and group N has a repeating unit as shown in formula (II), and at least one of group M and group N has a repeating unit as shown in formula (III);
[0009] Formula (II);
[0010] Formula (III); R1, R3, and R4 are independently selected from H, unsubstituted or substituted C1-C6 alkyl groups, and unsubstituted or substituted C6-C12 aryl groups, and R2 is selected from unsubstituted or substituted C1-C6 alkyl groups and unsubstituted or substituted C6-C12 aryl groups. L is selected from unsubstituted or substituted C2-C8 aliphatic hydrocarbon group, unsubstituted or substituted C3-C12 aliphatic cycloalkyl group, unsubstituted or substituted C6-C12 aryl group, unsubstituted or substituted C3-C12 heteroaryl group, unsubstituted or substituted C8-C22 cycloalkylene alkylene cycloalkylene group, unsubstituted or substituted C8-C22 arylalkylene alkylene aryl group, unsubstituted or substituted C1-C6 alkoxy group, unsubstituted or substituted C1-C6 siloxyalkylene group, and unsubstituted or substituted C1-C6 alkylthio group.
[0011] In this document, the term "substituted" means that at least one hydrogen atom of the compound or chemical moiety is substituted by a substituent in another chemical moiety, wherein each substituent is independently selected from: hydroxyl, mercapto, amino, cyano, nitro, aldehyde, halogen atom (e.g., F, Cl, Br, I), alkenyl, alkynyl, aryl, heteroaryl, C1-C6 alkyl, C1-C6 alkoxy, C1-C6 alkylthio, C1-C6 haloalkyl, or C1-C6 siloxane. For example, for R1, R2, R3, and R4, the substituent may be, but is not limited to, one or more of hydroxyl, C1-C3 alkyl, or phenyl. For the L group, the substituent may be, but is not limited to, one or more of hydroxyl, halogen atom, nitro, cyano, C1-C3 alkyl, C1-C3 alkoxy, C1-C3 alkylthio, C1-C3 haloalkyl, or C1-C3 siloxane.
[0012] "Cycloalkylenealkylenealkylenealkylene" refers to a complex group formed by two cycloalkylene groups linked by an alkylene group, while "C8-C22 cycloalkylenealkylenealkylenealkylene" refers to a cycloalkylene ...
[0013] "Arylalkylene arylene" is a complex group consisting of two arylene groups linked by an alkylene group. "C8-C22 arylene alkylene arylene" refers to an arylene alkylene arylene group with 8-22 carbon atoms. The two arylene groups can be the same or different.
[0014] In some embodiments, R1, R3, and R4 are independently selected from H and C1-C6 alkyl groups.
[0015] In some embodiments, R2 is selected from unsubstituted or phenyl-substituted C1-C6 alkyl groups.
[0016] In some embodiments, L is selected from unsubstituted or substituted C4-C8 alkylene, unsubstituted or substituted phenylene, unsubstituted or substituted C13-C16 phenylene alkylene phenylene, and unsubstituted or substituted C10-C16 cycloalkylene alkylene cycloalkylene.
[0017] In some embodiments, R1, R3, and R4 are independently selected from H, methyl, or ethyl.
[0018] In some embodiments, R2 is selected from tert-butyl, methyl, ethyl, or benzyl.
[0019] In some implementations, L is selected from , , , or ,in, Indicates the connection site.
[0020] In some embodiments, the resin is selected from one of the following resins:
[0021] In some embodiments, both group M and group N in the resin have repeating units shown in formula (II) and repeating units shown in formula (III).
[0022] In this invention, the repeating units represented by formula (II) and formula (III) contained in groups M and N are connected by random polymerization.
[0023] In some embodiments, with the total molar amount of the repeating units shown in formula (II) and formula (III) being 100%, the molar amount percentage of the repeating units shown in formula (II) in the resin is x, and the molar amount percentage of the repeating units shown in formula (III) is y, where 10%≤x≤30% and 70%≤y≤90%.
[0024] In this invention, since the polymer chain can be considered symmetrical on both sides, the deprotection reaction of the two chain segments exhibits spatial equivalence. During the deprotection process, the conversion rates of the protecting groups on both sides are always maintained at a 1:1 ratio. Therefore, the molar percentage of the repeating unit represented by formula (II) in group M is equal to the molar percentage of the repeating unit represented by formula (II) in group N, which is equal to x.
[0025] In some embodiments, the structural formulas of group M and group N are independent: Where x1 and y1 represent the molar percentages of the two repeating units. 10%≤x1≤30%, 70%≤y1≤90%; where R1, R2, R3, and R4 are as defined in any of the above terms.
[0026] In some embodiments, the weight-average molecular weight of the resin is greater than or equal to 1000; preferably 5000 to 30000.
[0027] In some embodiments, the molecular weight distribution of the resin is in the range of 1.0 to 1.5; preferably 1.0 to 1.3; more preferably 1.0 to 1.2.
[0028] On the other hand, the present invention also provides a method for preparing any of the above-mentioned resins, comprising the following steps: anionicly polymerizing the monomer shown in formula (IV) in the presence of an initiator and a reaction solvent to obtain anionic polymer; then coupling the anionic polymer with a coupling reaction reagent to obtain a coupling polymer; and performing partial deprotection treatment on the coupling polymer to obtain a resin.
[0029] Formula (IV); Wherein, R1, R2, R3, and R4 are as defined in any of the above terms; the structural formula of the coupling reaction reagent is as follows: O=C=NLN=C=O; where L is as defined in any of the above terms.
[0030] In some embodiments, the initiator is selected from one or more of alkali metals, alkyl metal reagents, Grignard reagents, and alkoxy metal reagents. The alkali metal is, for example, one or more of lithium metal, sodium metal, and potassium metal; the alkyl metal reagent is, for example, one or more of n-butyllithium, sec-butyllithium, tert-butyllithium, methyllithium, and ethyllithium; the Grignard reagent is, for example, one or more of methylmagnesium bromide, ethylmagnesium bromide, phenylmagnesium bromide, and isopropylmagnesium chloride; and the alkoxy metal reagent is, for example, one or more of potassium tert-butoxide, sodium tert-butoxide, lithium methoxide, and sodium ethoxide.
[0031] Preferably, the initiator is an alkyl metal reagent, and more preferably one or more of n-butyllithium and sec-butyllithium.
[0032] In some embodiments, the reaction solvent is selected from one or more of benzene, toluene, tetrahydrofuran, diethyl ether, isopropyl ether, methyl ethyl ether, n-propyl ether, heptane, octane, n-hexane, cyclohexane, and dioxane.
[0033] In some embodiments, the molar ratio of the monomer to the initiator is 20-60:1. For example, the molar ratio of the monomer to the initiator can be 20:1, 30:1, 40:1, 50:1, 60:1, or within any two of the above values.
[0034] In some embodiments, the mass ratio of the monomer to the volume of the reaction solvent is 10-30 g: 100 mL. For example, the mass ratio of the monomer to the volume of the reaction solvent can be 10 g: 100 mL, 15 g: 100 mL, 20 g: 100 mL, 25 g: 100 mL, 30 g: 100 mL, or within any two of these ranges.
[0035] In some embodiments, the anionic polymerization temperature is -80°C to 0°C, and the time is 0.5 to 12 hours. For example, the anionic polymerization temperature can be -80°C, -70°C, -60°C, -50°C, -40°C, -30°C, -20°C, -10°C, 0°C, or any range of two of these values. The time can be 0.5 hours, 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours, 12 hours, or any range of two of these values.
[0036] In some embodiments, the anionic polymerization is carried out under an inert atmosphere.
[0037] In some embodiments, the molar ratio of the monomer to the coupling reagent is 40-200:1. For example, the molar ratio of the monomer to the coupling reagent can be 40:1, 50:1, 60:1, 70:1, 80:1, 90:1, 100:1, 120:1, 140:1, 160:1, 180:1, 200:1, or within any two of these ranges.
[0038] In some embodiments, the coupling reaction is carried out at a temperature of -80°C to 0°C for a time of 0.5 to 2 hours. For example, the coupling reaction temperature can be -80°C, -70°C, -60°C, -50°C, -40°C, -30°C, -20°C, -10°C, or 0°C, and the time can be 0.5 hours, 0.8 hours, 1 hour, 1.5 hours, or 2 hours, or within any two of the above values.
[0039] In some embodiments, the deprotection treatment is performed at a temperature of 50°C to 60°C for a duration of 4 to 6 hours. For example, the deprotection treatment temperature can be 50°C, 52°C, 54°C, 56°C, 58°C, or 60°C, and the time can be 4 hours, 4.5 hours, 5 hours, 5.5 hours, or 6 hours, or within any two of the above values.
[0040] In some embodiments, the molar ratio of the monomer to the deprotecting agent used in the deprotection treatment is 150-200:1. For example, the molar ratio of the monomer to the deprotecting agent used in the deprotection treatment can be 150:1, 160:1, 170:1, 180:1, 190:1, 200:1, or within any two of the above values.
[0041] In some embodiments, the reaction solvent is selected from one or more of benzene, toluene, tetrahydrofuran, diethyl ether, isopropyl ether, methyl ethyl ether, n-propyl ether, heptane, octane, n-hexane, cyclohexane, and dioxane.
[0042] In some embodiments, the deprotection reagent used in the deprotection treatment is an organic acid and / or an inorganic acid.
[0043] In some specific embodiments, the deprotecting agent is selected from one or more of hydrohalic acid, sulfuric acid, p-toluenesulfonic acid, benzenesulfonic acid, trifluoromethanesulfonic acid, acetic acid, trifluoroacetic acid, pentafluoropropionic acid, and heptafluorobutyric acid.
[0044] In some embodiments, the deprotection treatment is carried out in the presence of an alcohol solvent.
[0045] In some specific embodiments, the alcohol solvent is selected from one or more of isopropanol, methanol, ethanol, n-butanol, isobutanol, and tert-butanol.
[0046] In some embodiments, the mass ratio of the monomer to the volume of the alcohol solvent is 20-60 g: 100 mL.
[0047] On the other hand, the present invention also provides the use of any of the above-described resins or the resins prepared by the above-described preparation methods in the preparation of photoresists.
[0048] On the other hand, the present invention also provides a photoresist comprising any of the resins described above or the resins prepared by the methods described above, and further comprising a photoacid generator and a solvent.
[0049] In this invention, the specific type of photoacid-generating agent is not specifically limited and can be selected according to requirements. For example, the photoacid-generating agent can be one or more of sulfonium salt photoacid-generating agents and iodonium salt photoacid-generating agents; the sulfonium salt photoacid-generating agent is, for example, triphenylsulfonium perfluorobutyl sulfonate; the iodonium salt photoacid-generating agent is, for example, bis(4-tert-butylphenyl)iodonium perfluorobutane sulfonate, bis(4-tert-butylphenyl)iodotrifluoromethanesulfonate, etc. The specific type of solvent is not specifically limited and can be selected according to requirements. For example, it can be one or more of propylene glycol monomethyl ether and propylene glycol monomethyl ether acetate.
[0050] In addition, the photoresist components of this invention may also include one or more of the following: alkali, surfactant, and dissolution inhibitor. This invention is not specifically limited to the specific types of these substances and can be selected according to requirements. For example, the alkali may be one or more of triethanolamine, diethanolamine, ethanolamine, tetramethylammonium hydroxide, and tert-butanolamine; the surfactant may be a fluorinated surfactant, and may be one or more of FC-4430, FC-4432, and FS-310; the dissolution inhibitor may be one or more of bisphenol A di-tert-butyl ether, tert-butylphenol, and 2,2-bis(4-tert-butoxyphenyl)propane.
[0051] In some embodiments, the photoresist comprises, by weight, 3 to 33 parts of resin, 0.01 to 1 part of photoacid generator, 65 to 96 parts of solvent, 0.01 to 1 part of alkali, 0.01 to 0.1 parts of surfactant, and 0.01 to 0.5 parts of small molecule dissolution inhibitor.
[0052] Line-Width Roughness (LWR): Indicates the degree of local undulation at the edge of a photoresist line (unit: nm), used to measure the smoothness of the pattern edge.
[0053] Etching selectivity: The ratio of the etching rate of the material being etched to the etching rate of the photoresist during the etching process. A higher value is better, indicating that the photoresist is more durable.
[0054] The technical solution of this invention has the following advantages: 1. The resin provided by the present invention has the structural formula shown in formula (I), in which two polymer chains (groups M and N) are linked together by groups with amide groups at both ends. The photoresist prepared therefrom, compared with commonly used photoresists, shows that during exposure, the linker undergoes hydrolysis under the action of photoacid, resulting in a significant contrast between the exposed and non-exposed areas. The steepness of the sidewalls of the pattern is significantly improved during the development process, and the edge roughness of the photoresist is effectively reduced. Furthermore, it maintains excellent etching resistance, and the sidewalls of the etched trenches are steep and vertical, without footing (bottom widening) phenomenon. The top edge contour is sharp and clear, making it suitable for forming micron- or nano-scale patterns in integrated circuits or for applications in optoelectronic products and other fields.
[0055] 2. The resin provided by the present invention, with the total molar amount of the repeating units shown in formula (II) and formula (III) being 100%, has the molar percentage of the repeating units shown in formula (II) as x and the molar percentage of the repeating units shown in formula (III) as y, wherein 10%≤x≤30% and 70%≤y≤90%. Controlling x and y within the above ranges can further reduce the edge roughness of the photoresist.
[0056] 3. Research has shown that when the L group of the resin provided by this invention is selected from unsubstituted or substituted phenylene, or unsubstituted or substituted C13-C16 phenylene alkylene, it can further reduce the edge roughness of the photoresist and improve its etching resistance.
[0057] 4. The resin preparation method provided by the present invention firstly involves anionic polymerization of the monomer shown in formula (IV) to obtain anionic polymers with active ends, then connecting the active ends of the two anionic polymers through a coupling reaction reagent, and then partially deprotecting them to remove the R2 protecting group from some repeating units, finally obtaining a resin with the structure shown in formula (I). The preparation method is simple, easy to operate, and convenient for industrial production. Detailed Implementation
[0058] The following embodiments are provided to better understand the present invention, but the following embodiments do not constitute a limitation on the content and scope of protection of the present invention. Any product that is the same as or similar to the present invention, derived by any person under the guidance of the present invention or by combining the features of the present invention with other prior art, falls within the scope of protection of the present invention.
[0059] Unless otherwise specified, all experimental steps or conditions in the examples were performed according to conventional experimental procedures and conditions in the art. Reagents or instruments whose manufacturers are not specified are all commercially available products.
[0060] The main raw materials used in the following examples are from the following sources: p-Methoxystyrene (purity ≥99%), p-tert-butoxystyrene (purity ≥99%), p-isopropenyl anisole (purity ≥99%), azobisisobutyronitrile (purity ≥95%), n-butyllithium in n-hexane solution (concentration 1.6 mol / L), sec-butyllithium in n-hexane solution (concentration 1.3 mol / L). The following substances were purchased from Inokai Technology Co., Ltd.: bisphenol A di-tert-butyl ether (purity ≥99%, CAS No.: 64309-46-2), propylene glycol monomethyl ether acetate (PGMEA, purity ≥99%), propylene glycol monomethyl ether (PGME, purity ≥99%), tetrahydrofuran (THF, purity ≥99%), n-hexane (purity ≥99%), p-toluenesulfonic acid (purity ≥98%), benzenesulfonic acid (purity ≥98%), isopropanol (IPA, purity ≥99.8%), triphenylsulfonium perfluorobutyl sulfonate (purity ≥99%, CAS No.: 144317-44-2, abbreviated as PAG), and fluorosurfactant FC-4430 (purity ≥99%).
[0061] 4,4'-Methylenebis(phenyl isocyanate) (MDI, purity ≥99%), toluene diisocyanate (TDI, purity ≥99%), hexamethylene isocyanate (HDI, purity ≥99%), 4,4-diisocyanate dicyclohexylmethane (H12MDI, purity ≥99%), and terephthalic diisocyanate (purity ≥99%) were all sourced from Wanhua Chemical Group Co., Ltd.
[0062] The analysis methods involved in the embodiments are as follows: Nuclear magnetic resonance spectroscopy (NMR) test: Instrument: Bruker 300M NMR spectrometer; Deuterated reagent: chloroform or dimethyl sulfoxide; Test temperature: room temperature.
[0063] Gel permeation chromatography (GPC) test: instrument: Shimadzu LC-ADXR-2, standard: polystyrene (PS), prepared as a 1 wt% THF solution containing PS before use, test temperature: 35 ℃, flow rate: 1 mL / min.
[0064] Example A1 This embodiment provides a resin and its preparation method, including the following steps: (1) Synthesis of resin A-1: A 500 mL pear-shaped flask was purged with nitrogen three times. 150 mL of anhydrous tetrahydrofuran was added, followed by p-tert-butoxystyrene (26.44 g, 150 mmol). After thorough mixing, the system was placed in a -80°C cold bath for 30 min. Using a syringe, 2.8 mL (4.5 mmol) of a hexane solution of n-butyllithium (n-BuLi) was rapidly added to the system to initiate the reaction. The reaction was maintained at -80°C for 3 h. A sample was taken for gas chromatography to verify complete monomer reaction. Using a syringe, 5 mL (2.3 mmol) of a hexane solution of MDI (4,4'-methylenebis(phenyl isocyanate)) was rapidly added to the system, and the reaction was maintained at -80°C for 1 h. After the reaction was complete, 1 mL of degassed methanol was added to terminate the reaction. The reaction solution was poured into 1.5 L of methanol to precipitate the precipitate. After filtration, the filter cake was redissolved in 100 mL of tetrahydrofuran, and then poured into 1.5 L of methanol to precipitate. The resulting filter cake was washed with 500 mL of methanol and then placed in a vacuum drying oven for overnight vacuum drying to obtain resin A-1.
[0065] (2) Synthesis of chemically amplified resin B-1: Resin A-1 was placed in a three-necked flask and purged with nitrogen. Then, 50 mL of isopropanol was added as a solvent. Next, p-toluenesulfonic acid (0.17 g, 1 mmol) was added. The reaction flask was heated in an oil bath at 55°C for 5 hours. After the reaction, the reaction solution was poured into 1 L of deionized water to precipitate. After filtration, the filter cake was redissolved in 50 mL of tetrahydrofuran, poured into 1 L of deionized water again to precipitate, and the resulting filter cake was washed with 200 mL of deionized water and then vacuum dried overnight in a vacuum drying oven to obtain resin B-1, with a yield of 18.9 g and a recovery rate of 71.48%. GPC analysis of resin B-1 showed its weight-average molecular weight... M w It is 9200, and PDI is 1.10.
[0066] The structural formula of resin B-1 is as follows: In this case, both the M and N groups contain repeating units as shown in formula (II): The repeating unit shown in equation (III): In this embodiment, R1, R3, and R4 are all H, and R2 is tert-butyl.
[0067] 13C NMR (400 MHz, DMSO-D6): δ 171.9 ppm (characteristic peak of amide carbonyl carbon), 155-153 ppm, 141-139 ppm, 138-136 ppm, 129.7 ppm, 128.5 ppm, 127.6 ppm, 123.6 ppm, 122.0 ppm, 114.9 ppm, 77.2 ppm (characteristic peak of tert-butoxy quaternary carbon), 47-42 ppm, 41.2 ppm, 39.7 ppm, 30-27 ppm.
[0068] Analysis of the NMR data showed that in resin B-1, x was 24.5% (the characteristic signal of the benzene ring carbon bonded to oxygen is located at 155-153 ppm. The integral value of the peak area at 155-153 ppm was marked as 100%, and the integral of the peak area at 77.2 ppm was the value of x), and y was 75.5%. Furthermore, compared with the NMR spectrum of resin C-1 prepared in comparative example A1, resin B-1 showed a new characteristic peak signal of carbonyl carbon at 171.9 ppm. These findings demonstrate that the coupling reaction and partial deprotection reaction occurred successfully, and resin B-1 was successfully synthesized.
[0069] Example A2 This embodiment provides a resin and its preparation method, including the following steps: (1) Synthesis of resin A-2: A 500 mL pear-shaped flask was purged with nitrogen three times. 160 mL of anhydrous tetrahydrofuran was added, followed by 23.71 g (160 mmol) of p-isopropenyl anisole. After thorough mixing, the system was placed in a -80°C cold bath for 30 min. A 2.5 mL (4 mmol) solution of n-butyllithium in n-hexane was rapidly added to the system using a syringe to initiate the reaction. The reaction was maintained at -60°C for 4 h. A sample was taken for gas chromatography to verify complete monomer reaction. A 5 mL (2 mmol) solution of HDI (hexamethylene isocyanate) in tetrahydrofuran was rapidly added to the system using a syringe, and the reaction was maintained at -60°C for 1 h. After the reaction was complete, 1 mL of degassed methanol was added to terminate the reaction. The reaction solution was poured into 1.5 L of methanol to precipitate the precipitate. After filtration, the filter cake was redissolved in 100 mL of tetrahydrofuran, and then poured into 1.5 L of methanol to precipitate. The resulting filter cake was washed with 500 mL of methanol and then placed in a vacuum drying oven for overnight vacuum drying to obtain resin A-2.
[0070] (2) Synthesis of chemically amplified resin B-2: Resin A-2 was placed in a three-necked flask and purged with nitrogen. Then, 50 mL of isopropanol was added as a solvent. Benzenesulfonic acid (0.16 g, 1 mmol) was then added. The reaction flask was heated in an oil bath at 55°C for 6 hours. After the reaction, the reaction solution was poured into 1 L of deionized water to precipitate. After filtration, the filter cake was redissolved in 50 mL of tetrahydrofuran, poured into 1 L of deionized water again to precipitate, and the resulting filter cake was washed with 200 mL of deionized water and then vacuum dried overnight in a vacuum drying oven to obtain resin B-2, with a yield of 20.8 g and a recovery rate of 87.73%. GPC analysis of resin B-2 showed its weight-average molecular weight... M w It is 10500, and PDI is 1.08.
[0071] The structural formula of resin B-2 is as follows: In this case, both the M and N groups contain repeating units as shown in formula (II): The repeating unit shown in equation (III): In this embodiment, R1 is methyl, R3 and R4 are both H, and R2 is methyl.
[0072] 13 C NMR (400 MHz, DMSO-D6): δ 180.0 ppm (characteristic peak of amide carbonyl carbon), 156-153 ppm, 141-139 ppm, 138-136 ppm, 128.6 ppm, 127.7 ppm, 123.7 ppm, 115.2 ppm, 55.8 ppm (characteristic peak of methoxy carbon), 51.1 ppm, 47-42 ppm, 39.8 ppm, 30-27 ppm, 26.4 ppm, 23-22 ppm.
[0073] Analysis of the NMR data showed that in resin B-2, x was 20.3% (the characteristic signal of the benzene ring carbon bonded to oxygen is located at 156-153 ppm. The integral value of the peak area at 156-153 ppm was marked as 100%, and the integral of the peak area at 55.8 ppm was the value of x), and y was 79.7%. Furthermore, compared with the NMR spectrum of resin C-2 prepared in comparative example A2, resin B-2 showed a new characteristic peak signal of carbonyl carbon at 180 ppm. These findings demonstrate that the coupling reaction and partial deprotection reaction occurred successfully, and resin B-2 was successfully synthesized.
[0074] Example A3 This embodiment provides a resin and its preparation method, including the following steps: (1) Synthesis of resin A-3: A 500 mL pear-shaped flask was purged with nitrogen three times. 110 mL of anhydrous n-hexane was added, followed by p-methoxystyrene (24.15 g, 180 mmol). After thorough mixing, the system was placed in a -40°C cold bath for 30 min. Using a syringe, 2.4 mL of a sec-butyllithium n-hexane solution (3.8 mmol) was rapidly added to the system to initiate the reaction. The reaction was maintained at -40°C for 6 h. A sample was taken for gas chromatography to verify complete monomer reaction. Using a syringe, 5 mL of a TDI (toluene diisocyanate) n-hexane solution (1.9 mmol) was rapidly added to the system, and the reaction was maintained at -40°C for 1 h. After the reaction was complete, 1 mL of degassed methanol was added to terminate the reaction. The reaction solution was poured into 1.5 L of methanol to precipitate the precipitate. After filtration, the filter cake was redissolved in 100 mL of tetrahydrofuran, and then poured into 1.5 L of methanol to precipitate. The resulting filter cake was washed with 500 mL of methanol and then placed in a vacuum drying oven for overnight vacuum drying to obtain resin A-3.
[0075] (2) Synthesis of chemically amplified resin B-3: Resin A-3 was placed in a three-necked flask and purged with nitrogen. Then, 50 mL of isopropanol was added as a solvent. Next, p-toluenesulfonic acid (0.17 g, 1 mmol) was added. The reaction flask was heated in an oil bath at 55°C for 5 hours. After the reaction, the reaction solution was poured into 1 L of deionized water to precipitate. After filtration, the filter cake was redissolved in 50 mL of tetrahydrofuran, poured into 1 L of deionized water again to precipitate, and the resulting filter cake was washed with 200 mL of deionized water and then vacuum dried overnight in a vacuum drying oven to obtain resin B-3, with a yield of 20.8 g and a recovery rate of 86.13%. GPC analysis of resin B-3 showed its weight-average molecular weight... M w The value is 12300, and the PDI is 1.10.
[0076] The structural formula of resin B-3 is as follows: In this case, both the M and N groups contain repeating units as shown in formula (II): The repeating unit shown in equation (III): In this embodiment, R1, R3, and R4 are all H, and R2 is a methyl group.
[0077] 13C NMR (400 MHz, DMSO-D6): δ 172.1 ppm (characteristic peak of amide carbonyl carbon), 156-153 ppm, 141-139 ppm, 138-136 ppm, 135.8 ppm, 130-129 ppm, 128.7 ppm, 127.8 ppm, 127.3 ppm, 123.8 ppm, 117.2 ppm, 115.1 ppm, 113.3 ppm, 55.9 ppm (characteristic peak of methoxy carbon), 47-42 ppm, 30-27 ppm, 17.4 ppm.
[0078] through 13 C10 NMR analysis showed that in resin B-3, x was 29.8% (a characteristic peak signal of the methoxy carbon in the R2 group was observed at 55.9 ppm, and the characteristic signal of the benzene ring carbon bonded to oxygen was observed at 156-153 ppm. The integral value of the peak area at 156-153 ppm was marked as 100%, and the integral of the peak area at 55.9 ppm was the value of x), and y was 70.2%. In addition, compared with the NMR spectrum of resin C-3 prepared by comparative example A3, resin B-3 showed a new characteristic peak signal of carbonyl carbon at 172.1 ppm. These findings demonstrate that the coupling reaction and partial deprotection reaction occurred successfully, and resin B-3 was successfully synthesized.
[0079] Example A4 This embodiment provides a resin and its preparation method, which differs from Example A1 only in the type of coupling reaction reagent. Specifically, "a hexane solution (5 mL, 2.3 mmol) of MDI (4,4'-methylenebis(phenyl isocyanate))" is replaced with "a hexane solution (5 mL, 2.3 mmol) of H12MDI (4,4-diisocyanate dicyclohexylmethane)". The rest of the synthesis process and the amount of materials used are kept the same, and resin B-4 is obtained.
[0080] The structural formula of resin B-4 is as follows: In this case, both the M and N groups contain repeating units as shown in formula (II): The repeating unit shown in equation (III): In this embodiment, R1, R3, and R4 are all H, and R2 is tert-butyl. GPC testing of resin B-4 shows its weight-average molecular weight... M w It is 9250, and PDI is 1.10.
[0081] 13C NMR (400 MHz, DMSO-D6): δ 170.1 ppm (characteristic peak of amide carbonyl carbon), 155-153 ppm, 141-139 ppm, 138-136 ppm, 128.6 ppm, 127.7 ppm, 123.7 ppm, 115.0 ppm, 77.3 ppm (characteristic peak of tert-butyl quaternary carbon), 50.6 ppm, 47-42 ppm, 39.8 ppm, 34.1 ppm, 32.3 ppm, 30-27 ppm.
[0082] Analysis of the NMR data showed that in resin B-4, x was 24.2% (the characteristic peak signal of the tert-butoxy quaternary carbon in the R2 group was observed at 77.3 ppm, and the characteristic signal of the benzene ring carbon connected to oxygen was observed at 155-153 ppm. The integral value of the peak area at 155-153 ppm was marked as 100%, and the integral of the peak area at 77.3 ppm was the value of x), and y was 75.8%. In addition, compared with the NMR spectrum of resin C-4 prepared by comparative example A4, the characteristic peak of the carbonyl carbon in the linker group was observed in resin B-4 at 170.1 ppm. These results proved that the coupling reaction and partial deprotection reaction occurred successfully, and resin B-4 was successfully synthesized.
[0083] Example A5 This embodiment provides a resin and its preparation method. The only difference from Example A2 is that the type of coupling reaction reagent is different. Specifically, "tetrahydrofuran solution of HDI (hexamethylene isocyanate) (5 mL, 2 mmol)" is replaced with "tetrahydrofuran solution of terephthalic diisocyanate (5 mL, 2 mmol)". The rest of the synthesis process and the amount of materials used are the same, and resin B-5 is obtained.
[0084] The structural formula of resin B-5 is as follows: In this case, both the M and N groups contain repeating units as shown in formula (II): The repeating unit shown in equation (III): In this embodiment, R1 is methyl, R3 and R4 are both H, and R2 is methyl. GPC testing of resin B-5 shows its weight-average molecular weight... M w The value is 10600, and the PDI is 1.09.
[0085] 13C NMR (400 MHz, DMSO-D6): δ 172.2 ppm (characteristic peak of amide carbonyl carbon), 156-153 ppm, 141-139 ppm, 138-136 ppm, 134.1 ppm, 128.6 ppm, 127.7 ppm, 123.7 ppm, 121.8 ppm, 115.0 ppm, 55.8 ppm (characteristic peak of methoxy carbon), 50.6 ppm, 47-42 ppm, 39.8 ppm, 34.1 ppm, 32.3 ppm, 30-27 ppm, 23-22 ppm.
[0086] Analysis of the NMR data showed that in resin B-5, x was 20.5% (the characteristic peak signal of the methoxy carbon in the R2 group was observed at 55.8 ppm, and the characteristic signal of the benzene ring carbon bonded to oxygen was observed at 156-153 ppm. The integral value of the peak area at 156-153 ppm was marked as 100%, and the integral of the peak area at 55.8 ppm was the value of x), and y was 79.5%. In addition, compared with the NMR spectrum of resin C-2 prepared by comparative example A2, the characteristic peak signal of the newly added carbonyl carbon was observed in resin B-5 at 172.2 ppm. These results demonstrate that the coupling reaction and partial deprotection reaction occurred successfully, and resin B-5 was successfully synthesized.
[0087] Comparative Example A1 This comparative example provides a resin and its preparation method. Compared with Example A1, the only difference is that a coupling reaction was not performed in step (1). The specific method is as follows: (1) Replace the nitrogen gas in a 500 mL round-bottom flask three times, add 150 mL of anhydrous tetrahydrofuran, and then add p-tert-butoxystyrene (26.44 g, 150 mmol). After mixing thoroughly, place the system in a -80℃ cold bath for 30 min. Use a syringe to quickly add 2.8 mL (4.5 mmol) of n-butyllithium (n-BuLi) in n-hexane to the above system to initiate the reaction. Maintain the reaction at -80℃ for 3 h. Take a sample and verify that the monomer has reacted completely by gas chromatography. After the reaction is complete, add 1 mL of degassed methanol to the reaction system to terminate the reaction. Pour the reaction solution into 1.5 L of methanol to precipitate. After filtration, dissolve the filter cake in 100 mL of tetrahydrofuran, pour it into 1.5 L of methanol again to precipitate, and rinse the filter cake with 500 mL of methanol and then place it in a vacuum drying oven to dry overnight.
[0088] (2) The above resin was placed in a three-necked flask and nitrogen gas was purged. Then, 50 mL of isopropanol was added to the system to dissolve the resin. Next, p-toluenesulfonic acid (0.17 g, 1 mmol) was added. The reaction flask was placed in an oil bath at 55°C and heated for 5 hours. After the reaction was complete, the reaction solution was poured into 1 L of deionized water to precipitate. After filtration, the filter cake was redissolved in 50 mL of tetrahydrofuran, poured into 1 L of deionized water again to precipitate, and the resulting filter cake was rinsed with 200 mL of deionized water and then vacuum dried overnight in a vacuum drying oven to obtain resin C-1, with a yield of 18.7 g and a recovery rate of 70.73%. GPC testing of resin C-1 showed its weight-average molecular weight... M w = 4600, PDI = 1.10.
[0089] The structural formula of resin C-1 is as follows: Where x1 and y1 represent the molar percentages of the two repeating units, and NMR testing shows that x1 is 24.8% and y1 is 75.2% in resin C-1.
[0090] Comparative Example A2 This comparative example provides a resin and its preparation method. Compared with Example A2, the only difference is that the C-2 resin is synthesized using a conventional free radical polymerization method. The specific steps are as follows: A 250 mL three-necked flask was purged with nitrogen three times, and 70 mL of PGMEA was added. Heating was then initiated. p-Isopropyl anisole (23.71 g, 160 mmol) and azobisisobutyronitrile (1.8 g) were dissolved in 5 mL of PGMEA to obtain a mixed solution of monomer and initiator. After reflux, the mixed solution was added dropwise to the three-necked reaction flask over a period of 3 hours. The reaction was continued for another 5 hours after the addition was complete. After the reaction was complete, 10 mL of methanol was added to quench the reaction. The reaction solution was poured into 1.5 L of methanol to precipitate the precipitate. After filtration, the filter cake was redissolved in 100 mL of tetrahydrofuran, and then poured into 1.5 L of methanol to precipitate again. The resulting filter cake was washed with 500 mL of methanol and then vacuum dried overnight in a vacuum drying oven.
[0091] The above resin was placed in a three-necked flask and purged with nitrogen. Then, 50 mL of tetrahydrofuran was added to dissolve the resin. Next, benzenesulfonic acid (0.17 g, 1 mmol) was added. The reaction flask was placed in an oil bath at 55°C and heated for 6 hours. After the reaction was complete, the reaction solution was poured into 1 L of deionized water to precipitate. After filtration, the filter cake was redissolved in 50 mL of tetrahydrofuran, poured into 1 L of deionized water again to precipitate, and the resulting filter cake was rinsed with 200 mL of deionized water and then vacuum dried overnight in a vacuum drying oven to obtain resin C-2, with a yield of 17.5 g and a recovery rate of 73.81%. GPC analysis of resin C-2 showed its weight-average molecular weight... M w = 10800, PDI = 1.93.
[0092] The structural formula of resin C-2 is as follows: Where x1 and y1 represent the molar percentage of the two repeating units, NMR testing showed that x1 was 20.5% and y1 was 79.5% in resin C-2.
[0093] Comparative Example A3 This comparative example provides a resin and its preparation method. Compared with Example A3, the only difference is that the C-3 resin is synthesized using a conventional free radical polymerization method. The specific steps are as follows: A 250 mL three-necked flask was purged with nitrogen three times, and 70 mL of PGMEA was added. Heating was initiated. A mixture of p-methoxystyrene (24.15 g, 180 mmol) and azobisisobutyronitrile (1.6 g) was dissolved in 5 mL of PGMEA to obtain a mixed solution of monomer and initiator. After reflux, the mixed solution was added dropwise to the three-necked reaction flask over a period of 3 h. After the addition was complete, the reaction was continued for another 5 h. After the reaction was complete, 10 mL of methanol was added to quench the reaction. The reaction solution was poured into 1.5 L of methanol to precipitate. After filtration, the filter cake was redissolved in 100 mL of tetrahydrofuran, and then poured into 1.5 L of methanol again to precipitate. The resulting filter cake was washed with 500 mL of methanol and then vacuum dried overnight in a vacuum drying oven.
[0094] The resin was placed in a three-necked flask and purged with nitrogen. Then, 50 mL of isopropanol was added as a solvent. Next, p-toluenesulfonic acid (0.17 g, 1 mmol) was added. The reaction flask was heated in an oil bath at 55°C for 5 hours. After the reaction, the reaction solution was poured into 1 L of deionized water to precipitate. After filtration, the filter cake was redissolved in 50 mL of tetrahydrofuran, poured into 1 L of deionized water again to precipitate, and the resulting filter cake was washed with 200 mL of deionized water and then vacuum dried overnight in a vacuum drying oven to obtain ternary copolymer resin C-3, with a yield of 19.6 g and a recovery rate of 81.16%. GPC testing of resin C-3 showed its weight-average molecular weight... M w = 12500, PDI = 1.88.
[0095] The structural formula of resin C-3 is as follows: Where x1 and y1 represent the molar percentage of the two repeating units, NMR testing showed that x1 was 28.4% and y1 was 71.6% in resin C-3.
[0096] Comparative Example A4 This comparative example provides a resin and its preparation method. Compared with Example A4, the only difference is that the C-4 resin is synthesized using a conventional free radical polymerization method. The specific method is as follows: A 250 mL three-necked flask was purged with nitrogen three times, and 70 mL of PGMEA was added. Heating was initiated. Tert-butoxystyrene (26.25 g, 149 mmol) and azobisisobutyronitrile (1.08 g) were dissolved in 5 mL of PGMEA to obtain a mixed solution of monomer and initiator. After reflux, the mixed solution was added dropwise to the three-necked reaction flask over a period of 3 h. After the addition was complete, the reaction was continued for another 5 h. After the reaction was complete, 10 mL of methanol was added to quench the reaction. The reaction solution was poured into 1.5 L of methanol to precipitate. After filtration, the filter cake was redissolved in 100 mL of tetrahydrofuran, and then poured into 1.5 L of methanol again to precipitate. The resulting filter cake was washed with 500 mL of methanol and then vacuum dried overnight in a vacuum drying oven.
[0097] The above resin was placed in a three-necked flask and purged with nitrogen. Then, 50 mL of tetrahydrofuran was added to dissolve the resin. Next, p-toluenesulfonic acid (0.17 g, 1 mmol) was added. The reaction flask was placed in an oil bath at 55°C and heated for 5 hours. After the reaction was complete, the reaction solution was poured into 1 L of deionized water to precipitate. After filtration, the filter cake was redissolved in 50 mL of tetrahydrofuran, poured into 1 L of deionized water again to precipitate, and the resulting filter cake was washed with 200 mL of deionized water and then vacuum dried overnight in a vacuum drying oven to obtain resin C-4, with a yield of 16.3 g and a yield of 62.1%. GPC testing of resin C-4 showed its weight-average molecular weight... M w = 15300, PDI = 1.82.
[0098] The structural formula of resin C-4 is as follows: Where x1 and y1 represent the molar percentage of the two repeating units, NMR testing showed that x1 was 26.9% and y1 was 73.1% in resin C-4.
[0099] Comparative Example A5 This comparative example provides a resin and its preparation method, differing from Example A1 only in that step (2) is omitted, and the resin is directly prepared using the method of step (1) in Example 1. This resin is designated as resin C-5. GPC testing of resin C-5 shows its weight-average molecular weight... M w = 12000, PDI = 1.09, after 13 C10 NMR testing showed that x was 100% and y was 0% in resin C-5.
[0100] Comparative Example A6 This comparative example provides a resin and its preparation method, differing from Example A1 only in that the amount of p-toluenesulfonic acid in step (2) is adjusted to 5 mmol, while the remaining steps are the same as in Example A1, ultimately yielding resin C-6. GPC testing of resin C-6 shows its weight-average molecular weight... M w = 8200, PDI = 1.10. (This is followed by a seemingly unrelated sentence fragment: "After...") 13 C10 NMR testing showed that x was 0% and y was 100% in resin C-6.
[0101] Example B1 This embodiment provides a photoresist, the raw materials of which are shown in Table 1.
[0102] Table 1. Raw material composition and weight parts
[0103] The preparation method is as follows: Weigh the resin, photoacid generator, alkali, solvent, surfactant and dissolution inhibitor according to the above weight proportions, put them in the sample bottle and mix them evenly. After shaking in a shaker for 4 h, filter them with a 0.22 μm filter membrane. After filtration, continue to shake for 1 h to obtain the photoresist.
[0104] Example B2 This embodiment provides a photoresist, the raw materials of which are shown in Table 2.
[0105] Table 2 Raw material composition and weight parts
[0106] The preparation method is as follows: Weigh the resin, photoacid generator, alkali, solvent, surfactant and dissolution inhibitor according to the above weight proportions, put them in the sample bottle and mix them evenly. After shaking in a shaker for 4 h, filter them with a 0.22 μm filter membrane. After filtration, continue to shake for 1 h to obtain the photoresist.
[0107] Example B3 This embodiment provides a photoresist, the raw materials of which are shown in Table 3.
[0108] Table 3 Raw material composition and weight parts
[0109] The preparation method is as follows: Weigh the resin, photoacid generator, alkali, solvent, surfactant and dissolution inhibitor according to the above weight proportions, put them in the sample bottle and mix them evenly. After shaking in a shaker for 4 h, filter them with a 0.22 μm filter membrane. After filtration, continue to shake for 1 h to obtain the photoresist.
[0110] Example B4 This embodiment provides a photoresist and its preparation method, which is basically the same as that in embodiment B1, except that the type of resin is different. In this embodiment, resin B-4 with the same weight parts is used instead of resin B-1 used in embodiment B1.
[0111] Example B5 This embodiment provides a photoresist and its preparation method, which is basically the same as that in embodiment B2, except that the type of resin is different. In this embodiment, resin B-5 with the same weight parts is used instead of resin B-2 used in embodiment B2.
[0112] Comparative Example B1 This comparative example provides a photoresist and its preparation method, which is basically the same as that in Example B1, except that the type of resin is different. In this comparative example, the same weight of resin C-1 is used instead of resin B-1 used in Example B1.
[0113] Comparative Example B2 This comparative example provides a photoresist and its preparation method, which is basically the same as Example B2, except that the type of resin is different. This comparative example uses the same weight of resin C-2 instead of resin B-2 used in Example B2.
[0114] Comparative Example B3 This comparative example provides a photoresist and its preparation method. The only difference from Example B3 is the type of resin. This comparative example uses the same weight of resin C-3 instead of resin B-3 used in Example B3.
[0115] Comparative Example B4 This comparative example provides a photoresist and its preparation method. The only difference from Example B4 is the type of resin. This comparative example uses the same weight of resin C-4 instead of resin B-4 used in Example B4.
[0116] Comparative Example B5 This comparative example provides a photoresist and its preparation method. The only difference from Example B1 is that the type of resin is different. This comparative example uses the same weight of resin C-5 instead of resin B-1 used in Example B1.
[0117] Comparative Example B6 This comparative example provides a photoresist and its preparation method. The only difference from Example B1 is that the type of resin is different. This comparative example uses the same weight of resin C-6 instead of resin B-1 used in Example B1.
[0118] Test case The photoresists prepared in each embodiment and comparative example were tested and evaluated for photolithography and morphology according to the following methods, and then etched and the etching results were observed.
[0119] In the hexamethyldisilazane (HMDS) chamber of a spin coater, gaseous HMDS was deposited onto the surface of a wafer substrate to form a passivation layer with a thickness of 5 nm. Photoresist was then spin-coated onto the HMDS-pretreated silicon wafer at 2500 rpm, baked on a hot plate at 120 °C for 90 seconds, and cooled to room temperature in a cold plate chamber to form a photoresist coating with a thickness of 100 nm ± 10 nm. The coating was then exposed on an exposure machine at a wavelength of 248 nm and an exposure intensity of 50 mJ / cm². 2 After exposure, the image was baked on a hot plate at 110 °C for 90 seconds, and finally developed in 2.38% tetramethylammonium hydroxide (TMAH) developer for 60 seconds. After drying, the photolithography results were examined using a scanning electron microscope (SEM). The feature width of the photolithographic pattern was measured at 50,000x magnification using a SEM, and its standard deviation was calculated as the LWR value (unit: nm).
[0120] The substrate was etched in a stable plasma environment, with the etching time set to 60 seconds based on the material thickness and etching rate. During etching, the bias power was set to 200W to control the ion bombardment energy, achieving anisotropic etching. Scanning electron microscopy (SEM) was used to measure the cross-section of the etched pattern at 50,000x magnification, recording the etching depth of both the etched material and the photoresist. The etching rates of both were calculated from the etching depth. The ratio of their etching rates is the etching selectivity.
[0121] Observe the morphology of the etched pattern and evaluate the steepness and verticality of the groove sidewalls, the footing phenomenon, and the sharpness and clarity of the edge contours.
[0122] The evaluation criteria for the steepness and verticality of the trench sidewalls are as follows: 1-4 points, with 1 point being the worst and 4 points being the best. 1 point indicates no photolithography or etching pattern; 2 points indicate that the sidewalls of the etched lines have obvious inclination; 3 points indicate that the sidewalls of the etched lines have slight inclination; and 4 points indicate that the sidewalls of the etched trenches are vertical.
[0123] Evaluation criteria for footing phenomenon: 1-4 points, with 1 point being the worst and 4 points being the best. 1 point indicates no photolithography or etching pattern, 2 points indicates obvious widening phenomenon, 3 points indicates slight widening phenomenon, and 4 points indicates no bottom widening phenomenon.
[0124] Evaluation criteria for the top edge contour: 1-4 points, with 1 point being the worst and 4 points being the best. 1 point indicates no lithography or etching pattern, 2 points indicates obvious blurring at the top edge, 3 points indicates slight blurring at the top edge, and 4 points indicates a sharp and clear top edge contour.
[0125] Table 4 Test Results
[0126] The results above show that the photoresist prepared from the resin synthesized in this invention exhibits significantly improved morphology and reduced roughness during photolithography. Compared with Examples B1-B5, Examples B1, B3, and B5, by employing preferred L groups, are able to better reduce roughness, improve etching morphology, and enhance etching selectivity.
[0127] After developing the B5 photolithography sample, it was found that there was significant residual photoresist at the bottom of the exposed area. The photoresist was not completely removed by the developer, and a continuous photoresist coating remained on the substrate surface. In subsequent etching processes, because the photoresist was not completely removed by the developer, the etching only acted on the residual photoresist layer and failed to reach the silicon substrate surface, resulting in the inability to obtain effective etching selectivity test data.
[0128] Comparative analysis using B6 photolithography and development confirmed that no photoresist residue was observed on either the exposed or unexposed substrate surfaces, indicating that the developer had completely removed the cover layer. In subsequent etching processes, because the photoresist protective layer was completely removed, the etching process acted directly on the silicon substrate surface. Since the photoresist itself did not experience observable etching loss, an effective etching rate comparison could not be established, ultimately resulting in the failure to obtain analyzable etching selectivity test data.
[0129] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.
Claims
1. A resin, characterized in that, The resin has the following structural formula (I): (I); Wherein, at least one of group M and group N has a repeating unit as shown in formula (II), and at least one of group M and group N has a repeating unit as shown in formula (III); Formula (II); Formula (III); R1, R3, and R4 are independently selected from H, unsubstituted or substituted C1-C6 alkyl groups, and unsubstituted or substituted C6-C12 aryl groups, and R2 is selected from unsubstituted or substituted C1-C6 alkyl groups and unsubstituted or substituted C6-C12 aryl groups. L is selected from unsubstituted or substituted C2-C8 aliphatic hydrocarbon group, unsubstituted or substituted C3-C12 aliphatic cycloalkyl group, unsubstituted or substituted C6-C12 aryl group, unsubstituted or substituted C3-C30 heteroaryl group, unsubstituted or substituted C8-C22 cycloalkylene alkylene cycloalkylene group, unsubstituted or substituted C8-C22 arylalkylene alkylene aryl group, unsubstituted or substituted C1-C6 alkoxy group, unsubstituted or substituted C1-C6 siloxyalkylene group, or unsubstituted or substituted C1-C6 alkylthio group.
2. The resin according to claim 1, characterized in that, R1, R3, and R4 are independently selected from H and C1-C6 alkyl groups; And / or, R2 is selected from unsubstituted or phenyl-substituted C1-C6 alkyl groups; And / or, L is selected from unsubstituted or substituted C4-C8 alkylene, unsubstituted or substituted phenylene, unsubstituted or substituted C13-C16 phenylene alkylene phenylene, and unsubstituted or substituted C10-C16 cycloalkylene alkylene cycloalkylene.
3. The resin according to claim 1 or 2, characterized in that, R1, R3, and R4 are independently selected from H, methyl, or ethyl; And / or, R2 is selected from tert-butyl, methyl, ethyl, or benzyl; And / or, L is selected from , , , or ,in, Indicates the connection site.
4. The resin according to claim 1 or 2, characterized in that, The resin is selected from one of the following resins: 。 5. The resin according to claim 1 or 2, characterized in that, The resin contains repeating units in groups M and N, both of which have repeating units as shown in formula (II) and formula (III). And / or, with the total molar amount of the repeating units shown in formula (II) and the repeating units shown in formula (III) being 100%, the molar amount percentage of the repeating units shown in formula (II) in the resin is x, and the molar amount percentage of the repeating units shown in formula (III) is y, where 10%≤x≤30% and 70%≤y≤90%.
6. The resin according to claim 1 or 2, characterized in that, The resin has a weight-average molecular weight greater than or equal to 1000; and / or, the molecular weight distribution range of the resin is 1.0 to 1.
5.
7. A method for preparing the resin according to any one of claims 1-6, characterized in that, The process includes the following steps: anionic polymerization of the monomer shown in formula (IV) in the presence of an initiator and a reaction solvent to obtain anionic polymer; coupling reaction of the anionic polymer with a coupling reagent to obtain a coupling polymer; partial deprotection treatment of the coupling polymer to obtain a resin. Formula (IV); Wherein, R1, R2, R3, and R4 are as defined in any one of claims 1-3; the structural formula of the coupling reaction reagent is as follows: O=C=NLN=C=O; where L is as defined in any one of claims 1-3.
8. The method for preparing the resin according to claim 7, characterized in that, The initiator is selected from one or more of alkali metals, alkyl metal reagents, Grignard reagents, and alkoxy metal reagents; And / or, the reaction solvent is selected from one or more of benzene, toluene, tetrahydrofuran, diethyl ether, isopropyl ether, methyl ethyl ether, n-propyl ether, heptane, octane, n-hexane, cyclohexane, and dioxane; And / or, the molar ratio of the monomer to the initiator is 20-60:1; And / or, the mass ratio of the monomer to the volume of the reaction solvent is 10-30 g: 100 mL; And / or, the anionic polymerization is carried out at a temperature of -80℃ to 0℃ for a time of 0.5 to 12 hours; And / or, the anionic polymerization is carried out under an inert atmosphere; And / or, the molar ratio of the monomer to the coupling reaction reagent is 40-200:1; And / or, the coupling reaction is carried out at a temperature of -80℃ to 0℃ for a time of 0.5 to 2 hours; And / or, the deprotection reagent used in the deprotection treatment is an organic acid and / or an inorganic acid; And / or, the temperature for the deprotection treatment is 50℃~60℃, and the time is 4~6h; And / or, the molar ratio of the monomer to the deprotecting agent used in the deprotection treatment is 150-200:1; And / or, the deprotection treatment is carried out in the presence of an alcohol solvent.
9. Use of the resin according to any one of claims 1-6 or the resin prepared by the preparation method according to claim 7 or 8 in the preparation of photoresist.
10. A photoresist, characterized in that, The resin comprising any one of the resins described in claims 1-6 or the resin prepared by the method described in claim 7 or 8, further comprising a photoacid-producing agent and a solvent.