A narrow-distribution, low-ash foundry wax pure monomer resin and its preparation method
By introducing monomer dimers and BF3-alkyl acrylate complexation catalytic system, combined with precise low-temperature polymerization and multi-stage refining processes, the catalytic activity and ash content problems of styrene-based pure monomer resins were solved, achieving pure monomer resins with narrow molecular distribution and low ash content, thus improving the performance and environmental friendliness of casting wax.
Patent Information
- Application Number
- CN202611622700.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-20
- Publication Date
- 2026-11-17
AI Technical Summary
In existing technologies, styrene-based pure monomer resins have high catalytic activity, but catalyst residues are difficult to completely remove, resulting in high ash content, numerous side reactions, strong pungent odor, and excessive VOC emissions. This leads to decreased compatibility with base materials such as paraffin wax, limiting their application in high-end precision casting waxes.
By employing a complex catalytic system of monomer dimers and BF3 with alkyl acrylates, and leveraging the active polymerization characteristics of slow initiation, fast growth, and minimal transfer, combined with precise low-temperature polymerization and multi-stage refining processes, including termination, countercurrent washing, adsorption impurity removal, gradient devolatilization, and nitrogen stripping, a pure monomer resin with narrow molecular weight distribution and low ash content is formed.
It achieves a narrow molecular weight distribution, ash content below 0.009%, no irritating odor, excellent paraffin compatibility, meets environmental protection requirements, improves the dimensional accuracy and surface quality of casting wax, and has a significant cost advantage.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of pure monomer resin technology, specifically to a narrow-distribution, low-ash casting wax pure monomer resin and its preparation method. Background Technology
[0002] Pure monomer resins typically refer to low-molecular-weight aromatic hydrocarbon resins obtained through cationic polymerization using styrene monomers as the main raw material. Due to their light color, moderate softening point, and good compatibility with various waxes and polymer materials, they are widely used in adhesives, coatings, inks, and casting waxes. In the field of precision casting waxes, pure monomer resins, as key components for thickening, hardening, and shrinkage regulation, play a decisive role in the dimensional accuracy, surface finish, ash residue, and dewaxing performance of casting wax molds.
[0003] Precision casting (investment casting) has extremely stringent requirements for the ash content of foundry wax. Excessive ash content can lead to defects such as inclusions and pitting on the casting surface, directly affecting the surface quality and dimensional accuracy of the casting. Furthermore, during the mixing, waxing, and dewaxing processes of foundry wax, the resin used must have excellent compatibility with base materials such as paraffin wax, EVA, and rosin, and must not exhibit layering, precipitation, or turbidity. In addition, with increasingly stringent environmental protection requirements, low odor and low VOC emissions have become essential indicators for foundry wax materials.
[0004] Currently, the industrial production of styrene-based pure monomer resins typically employs a Lewis acid-catalyzed cationic polymerization process, with BF3 diethyl ether complex as a typical catalytic system. However, existing technologies generally suffer from the following drawbacks: First, the raw material monomers used are highly reactive, and the BF3 diethyl ether complex exhibits strong Lewis acidity, resulting in intense exothermic catalysis and making the reaction difficult to control; second, catalyst residues are difficult to completely remove, leading to high ash content in the product; third, the polymerization process involves numerous side reactions, generating large amounts of low-molecular-weight oligomers, resulting in a strong pungent odor, excessive VOC emissions, and poor environmental friendliness in both production and use; fourth, the high content of oligomers and polar impurities reduces the compatibility of the resin with base materials such as paraffin wax and EVA, limiting its application in high-end casting waxes.
[0005] Therefore, there is an urgent need to develop a pure monomer resin with a narrow molecular weight distribution, extremely low ash content, no irritating odor, and excellent compatibility with paraffin wax, as well as its preparation method, to meet the application needs of the high-end precision casting wax field. Summary of the Invention
[0006] To address the problems in the prior art, the first aspect of this invention provides a pure monomer resin for casting wax with narrow distribution and low ash content. The raw materials for preparation include polymeric monomers, polymeric monomer dimers, BF3, alkyl acrylates, composite terminators, adsorbents, and solvents.
[0007] This invention reduces the reactivity of the raw materials by introducing monomer dimers into them, thereby achieving a narrow molecular weight distribution. Simultaneously, it employs BF3 and alkyl acrylate as a catalyst system. The carbonyl oxygen atom of the alkyl acrylate forms a coordinate bond with the empty orbital of BF3, reducing the Lewis acidity of BF3, making the catalytic active center more stable, and extending its lifetime. This achieves the characteristics of slow initiation, rapid growth, and minimal transfer in active polymerization, thus narrowing the molecular weight distribution from the reaction mechanism level. Furthermore, it buffers the strongly exothermic complexation, avoiding localized explosive polymerization and a surge in side reactions.
[0008] In some embodiments, the raw materials for preparing the narrow-distribution, low-ash casting wax-specific pure monomer resin, by weight, include: 70-140 parts of polymer monomer Monomer dimer: 5-30 parts Solvent 180~220 parts BF30.8~1.0 parts Alkyl acrylate 0.6~0.8 parts 8-12 parts of compound terminating agent 8-12 parts of adsorbent.
[0009] In some embodiments, the alkyl acrylate includes one or more of methyl acrylate, ethyl acrylate, propyl acrylate, and butyl acrylate.
[0010] In some embodiments, the mass ratio of BF3 to alkyl acrylate is (0.8~1.0):(0.6~0.8). As an example, the mass ratio of BF3 to alkyl acrylate can be 0.8:0.8, 0.9:0.7, 1.0:0.6, or any value within the range of (0.8~1.0):(0.6~0.8).
[0011] In some embodiments, the composite terminator is a mixture of methanol and ammonia, with a volume ratio of methanol to ammonia of (7~10):1. As an example, the volume ratio of methanol to ammonia can be 7:1, 8:1, 9:1, 10:1, or any value within the range of (7~10):1. Ammonia provides an alkaline environment to neutralize the acidity remaining in BF3, while methanol acts as a terminator to react with the active chain. Together, they achieve a dual mechanism of "acid-base neutralization + free radical termination," preventing residual catalyst from triggering subsequent oxidation or decomposition reactions.
[0012] In some embodiments, the pure monomer resin satisfies at least one of the following characteristics: (1) The polymer monomer includes at least one of styrene and α-methylstyrene; (2) The polymeric monomer dimer includes at least one of α-methylstyrene-styrene dimer, styrene dimer, and α-methylstyrene dimer; (3) The solvent includes at least one of n-hexane, cyclohexane, ethylbenzene, and xylene.
[0013] In some embodiments, the adsorbent comprises activated alumina. This application uses activated alumina as an adsorbent, whose high specific surface area and microporous structure selectively adsorb catalyst residues and polar byproducts, blocking the formation of ash precursors and ensuring high product purity.
[0014] A second aspect of this invention provides a method for preparing a narrow-distribution, low-ash casting wax-specific pure monomer resin, comprising at least the following steps: S1. BF3 is coordinated with alkyl acrylate to obtain a complex catalyst; S2. Adjust the temperature of the complexing catalyst to 3~5℃, add the polymeric monomer and the polymeric monomer dimer by segmented dropwise addition, keep the reaction at the temperature after the dropwise addition is completed, and then successively perform the termination reaction, water washing extraction, adsorption purification, vacuum devolatilization, nitrogen stripping treatment, and cooling granulation to obtain pure monomer resin.
[0015] In some embodiments, S1 includes: cooling the solvent to -5~0°C under nitrogen protection, introducing BF3 gas, stirring to dissolve, adding alkyl acrylate dropwise, and continuing to stir the reaction to obtain a complex catalyst.
[0016] Optionally, the stirring reaction time is 25 to 35 minutes. As an example, the stirring reaction time can be 25 minutes, 30 minutes, 35 minutes, or any value within the range of 25 to 35 minutes.
[0017] The complex catalyst obtained in this invention is subjected to 11 B-NMR characterization showed that the boron chemical shift shifted from 0 ppm to -2.5 ppm, confirming the formation of the complex.
[0018] In some embodiments, the segmented addition method includes: adding 25-35% of the total mass of the monomer and monomer dimer in the first 2 hours, adding 45-55% of the total mass of the monomer and monomer dimer in the middle 4 hours, and adding the remaining monomer and monomer dimer in the last 2 hours.
[0019] In some embodiments, the S2 adopts a jacketed double heat exchange structure with an inner coil, and is equipped with a -15℃ ethylene glycol refrigeration unit, with a heat exchange area designed at 150kcal / (L·h); three temperature sensors are installed in the reactor at the top, middle and bottom of the reactor, and the monomer dropping rate and chilled water flow rate are automatically adjusted when the temperature deviation exceeds ±0.5℃.
[0020] This invention employs a precise low-temperature polymerization range of 3~5℃, and uses a three-stage gradient droplet addition of monomers to strictly control the matching of the exothermic rate and the heat exchange rate, effectively avoiding local overheating and explosive polymerization, and reducing the generation of low molecular weight impurities.
[0021] In some implementations, S2 satisfies at least one of the following features: (1) The termination reaction includes: after the heat preservation reaction is completed, adding a composite terminator to the reaction system and stirring for 20-30 minutes to terminate the reaction; (2) The water washing extraction is performed by countercurrent washing with deionized water at 45~55℃ 3~4 times; (3) The conditions for adsorption purification are: adsorption at 70~90℃ for 1.5~2.5h followed by filtration; (4) The decompression devolatilization adopts a two-stage devolatilization process. The first-stage devolatilization conditions are: 200℃, -0.095MPa, and the second-stage devolatilization conditions are: 230℃, -0.099MPa. (5) The nitrogen stripping treatment is to pass nitrogen gas at 200~300℃ for 25~35 minutes after devolatilization.
[0022] This invention constructs a five-stage closed-loop refining system: termination, countercurrent water washing, adsorption and impurity removal, gradient devolatilization, and nitrogen stripping. The methanol / ammonia composite termination completely inactivates the catalyst and neutralizes acidic residues; water washing removes most of the catalytic salts; activated alumina deeply adsorbs trace amounts of catalyst and impurities; two-stage vacuum devolatilization removes solvents and oligomers; and high-temperature nitrogen stripping completely removes volatile odor substances, ultimately achieving ultra-low ash content and odorless product quality.
[0023] Beneficial effects 1. This invention adds dimers of polymeric monomers to the raw materials to suppress the initial activity of the reaction. At the same time, it adopts a BF3-methyl acrylate complex catalytic system to precisely reduce the Lewis acidity of BF3, making the catalytic active center more stable. The lifespan of the active center is extended by more than 3 times compared with the traditional BF3 diethyl ether complex, effectively reducing chain transfer side reactions, achieving controllable polymerization characteristics, and reducing the polydispersity coefficient of the product to below 1.7, significantly improving the uniformity of resin performance, and ensuring the stability of casting wax shrinkage and casting dimensional accuracy.
[0024] 2. This invention uses a precise low-temperature polymerization range of 3~5℃, and adds monomers in a three-stage gradient process to strictly control the matching of the exothermic rate and the heat exchange rate, effectively avoiding local overheating and explosive polymerization, reducing the generation of low molecular weight impurities, and the product has an ash content of ≤0.009% and a softening point that is stable at 75~80℃.
[0025] 3. This invention constructs a five-stage closed-loop refining system. The methanol / ammonia water composite termination can completely inactivate the catalyst and neutralize acidic residues. Activated alumina deeply adsorbs trace impurities. Secondary devolatilization + nitrogen stripping removes solvents and oligomers in stages. The final product has an ash content of less than 0.009%, no irritating odor, excellent paraffin compatibility, meets VOCs environmental protection requirements, and can effectively avoid residual ash and porosity defects in castings.
[0026] 4. The process parameters of this invention are controllable, the process loop is complete, and the raw materials are all commonly used industrial products that are easy to purchase. Compared with traditional processes, the product yield is increased by more than 7.3%, no additional decolorization and deodorization process is required, the mass production yield is high, and it has significant cost advantages and prospects for large-scale application. Detailed Implementation
[0027] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are only for explaining the invention and are not intended to limit the invention. Experimental methods not specifying specific conditions in the embodiments were performed under conventional conditions or conditions recommended by the manufacturer. Reagents or instruments whose manufacturers are not specified are all commercially available conventional products.
[0028] Example 1 The first aspect of this example provides a narrow-distribution, low-ash casting wax-specific pure monomer resin, the raw materials for which are prepared by weight include: 30 parts styrene 70 parts of α-methylstyrene 10 parts of styrene dimer 200 parts of n-hexane BF31.0 copies 0.6 parts alkyl acrylate 10 parts of compound terminating agent 10 parts of adsorbent.
[0029] The alkyl acrylate is methyl acrylate.
[0030] The composite terminator is a mixture of methanol and ammonia, with a volume ratio of methanol to ammonia of 9:1.
[0031] The adsorbent is activated alumina (Φ3-5mm), sourced from Jiangxi 863 Industrial Co., Ltd.
[0032] The styrene dimer has the CAS number 25247-68-1 and comes from Hubei Guangao Biotechnology Co., Ltd.
[0033] The second aspect of this example provides a method for preparing a narrow-distribution, low-ash casting wax-specific pure monomer resin, comprising the following steps: S1. Under nitrogen protection, the solvent is cooled to -5°C, BF3 gas is introduced, and after stirring to dissolve, alkyl acrylate is added dropwise. The reaction is continued for 30 min to obtain the complex catalyst. S2. Styrene, α-methylstyrene, and styrene dimer are mixed evenly to obtain a mixture; the temperature of the complexing catalyst is adjusted to 4°C, and the mixture is added in stages: 30% of the total mass of the mixture is added in the first 2 hours, 50% of the total mass of the mixture is added in the middle 4 hours, and the remaining mixture is added in the last 2 hours; after the addition is completed, the mixture is kept at 4°C for 2 hours, and then subjected to the following processes in sequence: termination reaction, water washing and extraction, adsorption purification, vacuum devolatilization, and nitrogen stripping, followed by cooling and granulation to obtain pure monomer resin.
[0034] The termination reaction includes: after the heat preservation reaction is completed, adding a composite terminator to the reaction system and stirring for 30 minutes to terminate the reaction and obtain a reaction solution.
[0035] The water washing extraction process involves washing the reaction solution three times countercurrently with deionized water at 50°C, with a water-to-reaction-solution volume ratio of 1:1 each time. After standing and phase separation, the aqueous phase is discarded and the oil phase is retained.
[0036] The conditions for adsorption purification are as follows: active alumina is added to the oil phase, and the mixture is stirred and adsorbed at 80°C for 2 hours, followed by filtration to obtain the filtrate.
[0037] The vacuum devolatilization includes: performing two-stage devolatilization on the filtrate. The first-stage devolatilization conditions are: 200℃, -0.095MPa, and 20min. The second-stage devolatilization conditions are: 230℃, -0.099MPa, and 20min.
[0038] The nitrogen stripping treatment involves passing nitrogen gas at 250°C for 30 minutes after devolatilization.
[0039] Example 2 The first aspect of this example provides a narrow-distribution, low-ash casting wax-specific pure monomer resin, the raw materials for which are prepared by weight include: 30 parts styrene 70 parts of α-methylstyrene 10 parts of styrene dimer 200 parts of solvent BF 30.8 portions 0.8 parts alkyl acrylate 10 parts of compound terminating agent 10 parts of activated alumina adsorbent.
[0040] The solvent is n-hexane.
[0041] The alkyl acrylate is methyl acrylate.
[0042] The composite terminator is a mixture of methanol and ammonia, with a volume ratio of methanol to ammonia of 9:1.
[0043] The second aspect of this example provides a method for preparing a narrow-distribution, low-ash casting wax-specific pure monomer resin, comprising the following steps: S1. Under nitrogen protection, the solvent is cooled to -5°C, BF3 gas is introduced, and after stirring to dissolve, alkyl acrylate is added dropwise. The reaction is continued for 30 min to obtain the complex catalyst. S2. Styrene, α-methylstyrene, and styrene dimer are mixed evenly to obtain a mixture; the temperature of the complexing catalyst is adjusted to 4°C, and the mixture is added in stages: 30% of the total mass of the mixture is added in the first 2 hours, 50% of the total mass of the mixture is added in the middle 4 hours, and the remaining mixture is added in the last 2 hours; after the addition is completed, the mixture is kept at 4°C for 2 hours, and then subjected to the following processes in sequence: termination reaction, water washing and extraction, adsorption purification, vacuum devolatilization, and nitrogen stripping, followed by cooling and granulation to obtain pure monomer resin.
[0044] The termination reaction includes: after the heat preservation reaction is completed, adding a composite terminator to the reaction system and stirring for 30 minutes to terminate the reaction and obtain a reaction solution.
[0045] The water washing extraction process involves washing the reaction solution three times countercurrently with deionized water at 50°C, with a water-to-reaction-solution volume ratio of 1:1 each time. After standing and phase separation, the aqueous phase is discarded and the oil phase is retained.
[0046] The conditions for adsorption purification are as follows: active alumina is added to the oil phase, and the mixture is stirred and adsorbed at 80°C for 2 hours, followed by filtration to obtain the filtrate.
[0047] The vacuum devolatilization includes: performing two-stage devolatilization on the filtrate. The first-stage devolatilization conditions are: 200℃, -0.095MPa, and 20min; the second-stage devolatilization conditions are: 230℃, -0.099MPa, and 20min.
[0048] The nitrogen stripping treatment involves passing nitrogen gas at 250°C for 30 minutes after devolatilization.
[0049] Example 3 The specific implementation method in this example is the same as in Example 1, except that the preparation method of the narrow-distribution, low-ash casting wax-specific pure monomer resin includes the following steps: S1. Under nitrogen protection, the solvent is cooled to -5°C, BF3 gas is introduced, and after stirring to dissolve, alkyl acrylate is added dropwise. The reaction is continued for 30 min to obtain the complex catalyst. S2. Styrene, α-methylstyrene, and styrene dimer are mixed evenly to obtain a mixture; the temperature of the complexing catalyst is adjusted to 3°C, and the mixture is added in stages: 30% of the total mass of the mixture is added in the first 3 hours, 50% of the total mass of the mixture is added in the middle 5 hours, and the remaining mixture is added in the last 2 hours; after the addition is completed, the mixture is kept at 3°C for 2 hours, and then subjected to the following processes in sequence: termination reaction, water washing and extraction, adsorption purification, vacuum devolatilization, and nitrogen stripping, followed by cooling and granulation to obtain pure monomer resin.
[0050] Comparative Example 1 This example provides a pure monomer resin, the raw materials for which, by weight, are: 100 parts of styrene 200 parts of n-hexane 1.5 parts of BF3 diethyl ether complex 10 parts of methanol terminator.
[0051] The BF3 diethyl ether complex was obtained from Shandong Heyi Gas Co., Ltd., and contained 48% boron trifluoride.
[0052] Prepared according to the preparation method disclosed in US Patent Application US4075404A.
[0053] Comparative Example 2 The specific implementation method of this example is the same as that of Example 1, except that BF3 and alkyl acrylate are replaced with BF3 diethyl ether complex catalyst. In this example, BF3 diethyl ether complex is directly used for polymerization at 4°C. The reaction rate is too fast in the early stage and the temperature runs away to above 15°C. The pure monomer resin obtained has a polydispersity index (D) of 2.23, which is no different from the traditional process.
[0054] Comparative Example 3 The specific implementation method in this example is the same as in Example 1, except that, by weight, the raw materials include: 100 parts of styrene 200 parts of n-hexane BF31.0 copies 0.6 parts alkyl acrylate 10 parts of compound terminating agent Three parts of activated alumina adsorbent.
[0055] In this case, the amount of activated alumina used was insufficient, and the ash content of the final pure monomer resin was 0.023%, which did not meet the low ash content requirement. Furthermore, the product turned yellow after being stored for one month.
[0056] Comparative Example 4 The specific implementation method of this example is the same as that of Example 1, except that the temperature in S2 is 10°C.
[0057] In this example, the pure monomer resin D (polydispersity index) value increased to 1.92, and the odor level decreased to level 2 (slight odor).
[0058] Comparative Example 5 The specific implementation method in this example is the same as in Example 1, except that the amount of styrene dimer in the raw materials is 3 parts.
[0059] In this example, the pure monomer resin D (polydispersity index) value increased to 1.81, and the odor level decreased to level 2 (slight odor).
[0060] Comparative Example 6 The specific implementation method in this example is the same as in Example 1, except that, by weight, the raw materials include: 30 parts styrene 70 parts of α-methylstyrene 10 parts of styrene dimer 200 parts of solvent BF31.0 copies 1.4 parts alkyl acrylate 10 parts of compound terminating agent 10 parts of activated alumina adsorbent.
[0061] In this example, the pure monomer resin prepared had a D (polydispersity index) value of 1.85 and a softening point of 95°C.
[0062] Performance testing The pure monomer resins prepared in Examples 1-3 and Comparative Example 1 were subjected to the following tests: 1. Molecular weight and molecular weight distribution test (GPC test): Gel permeation chromatography was used with tetrahydrofuran (THF) as the mobile phase, the flow rate was set to 1.0 mL / min, the column temperature was kept constant at 35℃, and calibration was performed using standard polystyrene standard. The resin to be tested was prepared as a 0.5% THF dilute solution, filtered through a 0.22 μm organic filter membrane and then injected for testing. The instrument automatically integrated and calculated the number-average molecular weight Mn, weight-average molecular weight Mw, and polydispersity coefficient D (Mw / Mn).
[0063] 2. Softening point: Strictly in accordance with GB / T 4507-2014 "Determination of softening point of bitumen - ring and ball method", the resin was completely melted and poured into a standard ring mold. After cooling and shaping at room temperature, the surface was smoothed and placed in a constant temperature glycerol bath. The temperature was increased at a uniform rate of 5℃ / min, and the temperature at the moment of resin dripping was recorded. Each group of samples was tested in parallel 3 times, and the arithmetic mean was taken as the final result.
[0064] 3. Ash content: Performed according to the method specified in GB / T 2295. Accurately weigh 10.0g of the dried resin sample to constant weight and place it in a pre-weighed ceramic crucible; first, slowly carbonize it at low temperature until there is no black smoke or open flame, then transfer it to a muffle furnace at 800℃ and calcine at a constant temperature for 2 hours. After naturally cooling to room temperature, weigh it and calculate the percentage of the residue mass to the initial mass of the sample, which is the ash content of the sample.
[0065] 4. Odor Rating: The industry-standard closed-container sensory rating method is adopted. 50g of dry resin sample is sealed in a 1L closed light-proof container and baked at 80℃ for 2 hours. Five professional evaluators conduct the rating under the same environment and standard. The rating standards are as follows: Level 1 = No odor; Level 2 = Slight odorless; Level 3 = Slight perceptible odor; Level 4 = Obvious irritating odor; Level 5 = Strong and pungent odor.
[0066] 5. Paraffin compatibility: Mix the resin to be tested with industrial refined paraffin at a mass ratio of 1:1, heat at 120℃ until completely melted and stir at a uniform speed for 30 minutes until the system is homogeneous; allow it to cool naturally to room temperature, and record whether there are any adverse phenomena such as turbidity, layering, waxy precipitation, crystallization, or sedimentation.
[0067] 6. Product yield: The yield calculation formula is: (Final mass of dried resin after purification and impurity removal / Total mass of monomers fed) × 100%; the calculation process excludes the mass of solvents, catalysts, additives, and salt impurities, accurately corresponding to the actual yield in industrial production.
[0068] Table 1
[0069] As can be seen from the data in the table above: Comparative Example 1 uses a traditional BF3 diethyl ether complex, which is directly added to n-hexane at room temperature; the polymerization temperature is controlled within the range of 15~30℃, and the monomer is added in batches at once without segmented gradient addition; after the reaction is completed, it is simply terminated with pure methanol, and the product is directly discharged after a single depressurization solvent removal process, without countercurrent water washing, adsorption purification, or nitrogen stripping. Compared with the traditional process of Comparative Example 1, the polydispersity coefficient D of the pure monomer resin obtained in the three examples of this invention is controlled below 1.7, with the lowest reaching 1.60, which is much lower than 2.19 of Comparative Example 1; the ash content is ≤0.009%, which is an order of magnitude lower than 0.072% of Comparative Example 1; the odor level is all level 1 (odorless), while that of Comparative Example 1 is level 4 (irritating odor); it is completely transparent and compatible with paraffin without precipitation; the product yield is 91.8%~92.7%, which is more than 7 percentage points higher than 84.5% of Comparative Example 1.
[0070] The above provides a detailed description of a narrow-distribution, low-ash casting wax-specific pure monomer resin and its preparation method provided by the present invention. It should be noted that the above description of the embodiments is only for the purpose of helping to understand the method and core idea of the present invention. The series of detailed descriptions listed in the present invention are only specific descriptions of feasible implementation methods of the present technology. They are not intended to limit the scope of protection of this application. All equivalent implementation methods or modifications made without departing from the spirit of the present application should be included within the scope of protection of this application.
Claims
1. A pure monomer resin for narrow-distribution, low-ash foundry wax, characterized in that, The raw materials for preparation, by weight, include: 70-140 parts of polymer monomer Monomer dimer: 5-30 parts Solvent 180~220 parts BF30.8~1.0 parts Alkyl acrylate 0.6~0.8 parts 8-12 parts of compound terminating agent 8-12 parts of adsorbent; The preparation method of the narrow-distribution, low-ash casting wax-specific pure monomer resin includes at least the following steps: S1. BF3 is coordinated with alkyl acrylate to obtain a complex catalyst; S2. Adjust the temperature of the complexing catalyst to 3~5℃, add the polymeric monomer and the polymeric monomer dimer by segmented dropwise addition, keep the reaction at the temperature after the dropwise addition is completed, and then successively perform the termination reaction, water washing extraction, adsorption purification, vacuum devolatilization, nitrogen stripping treatment, and cooling granulation to obtain pure monomer resin.
2. The narrow-distribution, low-ash casting wax-specific pure monomer resin according to claim 1, characterized in that, The alkyl acrylate includes one or more of methyl acrylate, ethyl acrylate, propyl acrylate, and butyl acrylate.
3. The narrow-distribution, low-ash casting wax-specific pure monomer resin according to claim 1, characterized in that, The composite terminating agent is a mixture of methanol and ammonia, with a volume ratio of methanol to ammonia of (7~10):
1.
4. The narrow-distribution, low-ash casting wax-specific pure monomer resin according to claim 1, characterized in that, The adsorbent includes activated alumina.
5. The narrow-distribution, low-ash casting wax-specific pure monomer resin according to claim 1, characterized in that, The pure monomer resin satisfies at least one of the following characteristics: (1) The polymer monomer includes at least one of styrene and α-methylstyrene; (2) The polymeric monomer dimer includes at least one of α-methylstyrene-styrene dimer, styrene dimer, and α-methylstyrene dimer; (3) The solvent includes at least one of n-hexane, cyclohexane, ethylbenzene, and xylene.
6. The narrow-distribution, low-ash casting wax-specific pure monomer resin according to claim 1, characterized in that, S1 includes: cooling the solvent to -5~0℃ under nitrogen protection, introducing BF3 gas, stirring to dissolve, adding alkyl acrylate dropwise, and continuing to stir the reaction to obtain a complex catalyst.
7. The narrow-distribution, low-ash casting wax-specific pure monomer resin according to claim 1, characterized in that, The segmented dripping method includes: adding 25-35% of the total mass of the monomer and monomer dimer in the first 2 hours, adding 45-55% of the total mass of the monomer and monomer dimer in the middle 4 hours, and adding the remaining monomer and monomer dimer in the last 2 hours.
8. The narrow-distribution, low-ash casting wax-specific pure monomer resin according to claim 1, characterized in that, S2 satisfies at least one of the following characteristics: (1) The termination reaction includes: after the heat preservation reaction is completed, adding a composite terminator to the reaction system and stirring for 20-30 minutes to terminate the reaction; (2) The water washing extraction is performed by countercurrent washing with deionized water at 45~55℃ 3~4 times; (3) The conditions for adsorption purification are: adsorption at 70~90℃ for 1.5~2.5h followed by filtration; (4) The decompression devolatilization adopts a two-stage devolatilization process. The first-stage devolatilization conditions are: 200℃, -0.095MPa, and the second-stage devolatilization conditions are: 230℃, -0.099MPa. (5) The nitrogen stripping treatment is to pass nitrogen gas at 200~300℃ for 25~35 minutes after devolatilization.
Citation Information
Patent Citations
Copolymers of alpha-methylstyrene and styrene and uses thereof
US4075404A