Preparation method of acrylate copolymer

By designing a three-stage temperature gradient that matches the half-life of azobisisobutyronitrile (AIBN), and by adding low-concentration initiators and gradient cooling, the problems of molecular weight reduction, distribution broadening, and difficulty in removing residual monomers in existing processes have been solved. This has enabled the preparation of acrylate copolymers with high molecular weight, narrow distribution, and low residual monomers, thus improving product performance and environmental friendliness.

CN123106979APending Publication Date: 2026-11-17ZHEJIANG RIJIU NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611505504.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-24
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing solvent-based acrylate copolymer solution polymerization processes cannot simultaneously achieve high molecular weight, narrow molecular weight distribution, and low residual monomer, resulting in decreased copolymer cohesive strength, uneven product performance, and environmental issues.

Method used

A three-stage temperature gradient was adopted, with the thermal decomposition half-life of azobisisobutyronitrile in ethyl acetate matched stepwise. The reaction time of each stage was linked to the total amount of free radicals released. Combined with the slow, long-term, uniform dropwise addition of a low-concentration, highly diluted initiator solution and the gradient cooling after polymerization, the concentration of free radicals and the molecular chain growth environment were controlled to achieve deep conversion of residual monomers.

Benefits of technology

Acrylic copolymers with high molecular weight (640,000 to 1,100,000), narrow molecular weight distribution (2.1 to 2.8), and low residual monomer (0.22% to 0.45%) are obtained, which improves the holding power of pressure-sensitive adhesives and the durability of coatings, and reduces odor and environmental risks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention discloses a method for preparing an acrylate copolymer, comprising: S10: mixing isooctyl acrylate, butyl acrylate, and hydroxyethyl acrylate and dissolving them in ethyl acetate to obtain a homogeneous reaction solution; preparing an initiator solution; S20: heating the reaction solution to 64.5~65.5℃ and maintaining the temperature, adding 0.02~0.05 parts of azobisisobutyronitrile, and polymerizing at the same temperature for 3~4 hours; S30: heating to 66.5~67.5℃ and maintaining the temperature, adding 0.01~0.02 parts of azobisisobutyronitrile, and polymerizing at the same temperature for 2~3 hours; S40: heating to 70.0~71.0℃ and maintaining the temperature, uniformly adding the initiator solution dropwise to the reaction system at a rate of 0.3~0.7 mL / min, and continuing the polymerizing reaction at the same temperature for 3~4 hours after the addition is complete, and then ending the reaction; S50: gradually cooling the reaction system and filtering to remove impurities. The method for preparing acrylate copolymers of the present invention achieves simultaneous control of free radical concentration, molecular chain growth environment and residual monomer depth transformation throughout the entire reaction process through the synergistic effect of optimized schemes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of polymer materials technology, and specifically relates to a method for preparing acrylate copolymers. Background Technology

[0002] Acrylic copolymers, with their excellent flexibility, adhesion, weather resistance, and film-forming properties, are widely used in pressure-sensitive adhesives, composite adhesives, functional coatings, and optical thin film coatings. Among them, solution polymerization is the mainstream process for preparing solvent-based acrylate copolymers, which has advantages such as uniform and stable system, low gel content, and simple post-processing.

[0003] Existing solution polymerization processes for solvent-based acrylate copolymers mainly fall into three categories: batch solution polymerization, semi-continuous dropwise solution polymerization, and high-temperature post-curing / initiator replenishment. Batch solution polymerization involves adding all monomers, solvents, and initiators to the reactor at once. To obtain high molecular weights, low initiator concentrations and low temperatures are used to suppress chain termination and chain transfer side reactions. However, these mild conditions result in low polymerization rates, making it difficult to exceed 99% monomer conversion, and leading to high residual monomer content in the system. Extending the holding time or increasing the temperature to enhance conversion exacerbates chain transfer and bimolecular termination, causing a significant decrease in molecular weight. Simultaneously, the high monomer concentration and rapid increase in system viscosity at the initial stage of the reaction result in a significant auto-acceleration effect, leading to large differences in molecular chain growth conditions between the early and later stages, resulting in a wide molecular weight distribution and poor uniformity of the product. Semi-continuous dropwise solution polymerization stabilizes free radical generation and polymerization rate by controlling the dropping rate of monomers or initiators, weakening the auto-acceleration effect and achieving a narrower molecular weight distribution. However, due to the gradient dropping characteristics, the instantaneous monomer concentration in the reactor remains low, reducing the effective collision probability of monomers and limiting the continuous growth of molecular chains. This results in a low molecular weight of the final product, making it difficult to meet the performance requirements of high cohesion and high durability materials. Furthermore, maintaining a low initiator concentration throughout the process leads to insufficient residual active free radicals in the later stages of the reaction, making deep monomer conversion difficult and leaving the residual monomer problem prominent. High-temperature curing / initiator replenishment processes activate residual monomers to continue the reaction by raising the temperature in the later stages of the reaction or adding highly active initiators to reduce residual monomers. However, higher temperatures exacerbate side reactions such as chain transfer and backbiting-β-splitting, causing long-chain free radicals to break down and generate short-chain molecules and large monomers. This not only significantly reduces the average molecular weight but also adds low molecular weight tails to the molecular weight distribution, broadening the originally controllable narrow distribution system again.

[0004] Several dispersed technical methods have been disclosed in the prior art, such as staged or multiple initiator replenishment, designing the replenishment timing according to the initiator half-life, programmed temperature rise, diluting the initiator with solvent before dropwise addition, pretreatment of monomers such as alkaline washing to remove polymerization inhibitors before polymerization, and nitrogen replacement for deoxygenation. Among these, the scheme of designing the replenishment timing according to the initiator half-life is mostly used in solvent-free or low-solvent polymerization routes. It has high operating temperatures, half-lives measured in minutes, and focuses on system viscosity rather than molecular weight, molecular weight distribution, and residual monomers as control targets. It cannot simultaneously achieve high molecular weight and narrow distribution, and it is also difficult to obtain low residual monomers. In the scheme of short-term rapid replenishment of initiator at a constant high temperature, the initiator decomposes quickly and the instantaneous concentration of free radicals is high. It is easy to form local over-initiation at the replenishment point, triggering side reactions such as chain transfer and backbiting-β cleavage, which leads to a decrease in molecular weight and broadening of distribution. The short-term rapid dropwise addition cannot form a continuous and uniform low-concentration free radical supply to the terminal residual monomers, and the residual monomers are not completely removed. None of the aforementioned existing technologies discloses a method for curing a narrow distribution by ending with a gradient cooling of no more than 5°C / 10min, nor do they disclose the linkage design between the three temperature steps and the initiator half-life, reaction time, and total amount of free radicals released.

[0005] It is evident that existing solvent-based solution polymerization processes for acrylate copolymers cannot simultaneously achieve the three key indicators of high molecular weight, narrow molecular weight distribution, and low residual monomer: insufficient molecular weight leads to decreased cohesive strength of the copolymer, affecting the holding power of the pressure-sensitive adhesive and the durability of the coating; an excessively wide molecular weight distribution results in uneven product performance, easily causing coating defects in high-precision applications such as optical films; excessive residual monomer leads to odor and environmental problems, and may also cause quality hazards such as precipitation and yellowing in subsequent applications. Existing processes must make trade-offs among these three indicators in actual production.

[0006] Therefore, in view of the above-mentioned technical problems, it is necessary to provide a method for preparing acrylate copolymers. Summary of the Invention

[0007] The purpose of this invention is to provide a method for preparing solvent-based acrylate copolymers that simultaneously achieves high molecular weight, narrow molecular weight distribution, and low residual monomer content, as well as a solution polymerization method for preparing the same copolymer, overcoming the shortcomings of existing processes that require trade-offs among these three key indicators. This invention also addresses process stability issues in existing segmented addition / high-temperature curing processes, such as molecular weight reduction, broadened distribution, difficulty in removing residual monomers due to localized over-initiation of the initiator, and broadened distribution and cloudy appearance caused by improper cooling.

[0008] To achieve the above objectives, the present invention provides a method for preparing an acrylate copolymer, comprising: S10: mixing 60-70 parts by mass of isooctyl acrylate, 12-25 parts by mass of butyl acrylate, and 3-8 parts by mass of hydroxyethyl acrylate, and dissolving them in 150-200 parts by mass of ethyl acetate to obtain a homogeneous reaction solution; preparing an initiator solution, wherein the initiator solution is obtained by dissolving at least 0.01-0.02 parts by mass of azobisisobutyronitrile in 35-42 parts by mass of ethyl acetate; S20: heating the reaction solution to 64.5-65.5°C and maintaining the temperature, adding 0.02-0.05 parts by mass of azobisisobutyronitrile, and performing a constant-temperature polymerization reaction for 3-4 hours to obtain a first reaction copolymer. S30: Heat the first reaction solution to 66.5~67.5℃ and maintain the temperature, add 0.01~0.02 parts of azobisisobutyronitrile, and polymerize at the same temperature for 2~3 hours to obtain the second reaction solution; S40: Heat the second reaction solution to 70.0~71.0℃ and maintain the temperature, add the initiator solution dropwise to the reaction system at a rate of 0.3~0.7mL / min, and continue the polymerization reaction at 70.0~71.0℃ for 3~4 hours after the addition is complete, and then stop the reaction; S50: After the reaction is completed, control the cooling rate to not exceed 5℃ / 10min, cool the reaction system to room temperature, filter to remove impurities, and obtain the acrylate copolymer solution.

[0009] In one embodiment, the acrylate copolymer has a weight-average molecular weight of 640,000 to 1,100,000, a molecular weight dispersion of 2.1 to 2.8, and a residual monomer content of 0.22% to 0.45%.

[0010] In one embodiment, in S50, the cooling is a gradient cooling: from 70.0~71.0℃ to 50℃, the cooling process in this stage is controlled within 41~60min; then to 40℃, the cooling process in this stage is controlled within 30~60min; finally to room temperature, the cooling rate is 1~5℃ / 10min.

[0011] In one embodiment, the initiator solution in S40 is added at a constant rate for 60-120 minutes, allowing the terminal residual monomer to slowly complete chain growth under low free radical concentration.

[0012] In one embodiment, the azobisisobutyronitrile in S20 and / or S30 is first dissolved in 5 to 10 times its mass of ethyl acetate to form a uniform initiator mother liquor, and then added to the reaction solution in a single injection or in a thin stream over 30 to 90 seconds to improve the uniformity of initiator dispersion in the gradually thickening solution polymerization system.

[0013] In one embodiment, a monomer pretreatment step S60 is included before S10: isooctyl acrylate, butyl acrylate, and hydroxyethyl acrylate are washed with a 5% (w / w) sodium hydroxide aqueous solution to remove polymerization inhibitors, rinsed with deionized water until neutral, and dehydrated and dried. Specifically, each monomer is mixed with a 5% (w / w) sodium hydroxide aqueous solution at a volume ratio of 1:1, stirred and washed at room temperature for 10-20 minutes, and washed 1-3 times in total; after separating the aqueous phase, it is rinsed with deionized water until the pH of the aqueous phase is 6.5-7.5; after standing and dehydrating at room temperature for 10-20 hours, it is sealed and stored away from light, and used within 60-72 hours.

[0014] In one embodiment, after S10 and before S20, there is an oxygen removal step S70: high-purity nitrogen is introduced into the reaction solution to replace the air and dissolved oxygen for 20-40 minutes, and the reaction system is kept in a slightly positive pressure sealed state after the aeration is completed.

[0015] In one embodiment, stirring is also maintained in S20 and / or S30 and / or S40: the stirring speed is 150~250 rpm.

[0016] In one embodiment, S50 uses a precision filter with a 150-300 mesh screen connected in series to filter the material.

[0017] In one embodiment, in S10, 1 to 15 parts of the modified monomer are added and mixed with isooctyl acrylate, butyl acrylate, and hydroxyethyl acrylate, and then dissolved in ethyl acetate to obtain a homogeneous reaction solution. The modified monomer is at least one of methyl methacrylate, lauryl acrylate, and glycidyl methacrylate.

[0018] Compared with existing technologies, the preparation method of the acrylate copolymer of the present invention achieves simultaneous control of free radical concentration, molecular chain growth environment and residual monomer depth transformation throughout the entire reaction process through the synergistic effects of three-stage temperature steps matched with the thermal decomposition half-life of azobisisobutyronitrile in ethyl acetate, the linkage design of reaction time in each stage with the total amount of free radical release, the slow and long-term uniform dropwise addition of low-concentration, highly diluted initiator solution at the end of the reaction, and gradient cooling after polymerization. Specifically:

[0019] First, the present invention uses a three-stage stepped heating and segmented addition of initiator to make the total supply of free radicals present in a step-like, continuous, and low-peak distribution along the reaction process, which is different from the one-time high-concentration supply of the intermittent method and the pulsed short-time supply of the high-temperature curing method. The free radical generation and monomer consumption are dynamically coupled, chain termination and chain transfer are suppressed, and the molecular chain can grow fully, which is conducive to obtaining high molecular weight copolymers. The test results show that the weight average molecular weight of the obtained acrylate copolymer can reach 640,000 to 1,100,000.

[0020] Secondly, the present invention avoids automatic acceleration effect and temperature drift by using three-stage constant temperature, avoids local over-initiation of the initiator by uniform low-concentration droplet addition at the end of the reaction, and avoids phase separation caused by sudden aggregation of polymer chains by gradient cooling, which is beneficial to stabilize the molecular weight dispersion at 2.1~2.8.

[0021] Third, in the third stage of this invention, a low-concentration, highly diluted initiator solution matched with a high temperature and short half-life is slowly and uniformly added dropwise to continuously and uniformly replenish the residual monomers at the end, thereby achieving deep conversion of the residual monomers. Test results show that the content of residual monomers can be as low as 0.22%~0.45%.

[0022] Fourth, the initiator mother liquor replenishment, monomer alkaline washing pretreatment and nitrogen deoxygenation together eliminate the hidden dangers of gelation, bubbles and batch differences of monomers, which is conducive to obtaining a uniform, transparent polymer solution with good batch consistency. Detailed Implementation

[0023] To enable those skilled in the art to better understand the technical solutions in this disclosure, the technical solutions of this invention will be clearly and completely described below in conjunction with the embodiments disclosed herein. Obviously, the described embodiments are only some embodiments of this disclosure, and not all embodiments. Based on the embodiments in this disclosure, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of this disclosure.

[0024] Abbreviations and Key Terms

[0025] AIBN (2,2′-Azobis(2-methylpropionitrile)): A commonly used oil-soluble azo thermal initiator in this field. When heated, it homogenizes to generate nitrogen gas and 2-cyano-2-propyl free radicals, which initiate free radical polymerization.

[0026] HEA: Hydroxyethyl acrylate (2-hydroxyethyl acrylate).

[0027] MEHQ: p-Methoxyphenol (4-methoxyphenol), a commonly used polymerization inhibitor for industrial acrylate monomers.

[0028] PDI: Molecular weight dispersion (Mw / Mn).

[0029] Mw: weight-average molecular weight; Mn: number-average molecular weight.

[0030] T 1 / 2 Thermal decomposition half-life, which is the time required for the initiator to decompose to half of its initial concentration.

[0031] This invention provides a method for preparing an acrylate copolymer, comprising: S10: mixing 60-70 parts by mass of isooctyl acrylate, 12-25 parts by mass of butyl acrylate, and 3-8 parts by mass of hydroxyethyl acrylate, and dissolving them in 150-200 parts by mass of ethyl acetate to obtain a homogeneous reaction solution; preparing an initiator solution, wherein the initiator solution is obtained by dissolving at least 0.01-0.02 parts by mass of azobisisobutyronitrile in 35-42 parts by mass of ethyl acetate; S20: heating the reaction solution to 64.5-65.5℃ and maintaining the temperature, adding 0.02-0.05 parts by mass of azobisisobutyronitrile, and performing a constant-temperature polymerization reaction for 3-4 hours to obtain a first reaction solution; S S30: Heat the first reaction solution to 66.5~67.5℃ and maintain the temperature, add 0.01~0.02 parts of azobisisobutyronitrile, and polymerize at the same temperature for 2~3 hours to obtain the second reaction solution; S40: Heat the second reaction solution to 70.0~71.0℃ and maintain the temperature, add the initiator solution dropwise to the reaction system at a rate of 0.3~0.7mL / min, and continue the polymerization reaction at 70.0~71.0℃ for 3~4 hours after the addition is complete, and then stop the reaction; S50: After the reaction is completed, control the cooling rate to not exceed 5℃ / 10min, cool the reaction system to room temperature, filter to remove impurities, and obtain the acrylate copolymer solution. Preferably, the cooling is a gradient cooling: from 70.0~71.0℃ to 50℃, the cooling process in this stage is controlled within 41~60min; then to 40℃, the cooling process in this stage is controlled within 30~60min; finally to room temperature, the cooling rate is 1~5℃ / 10min.

[0032] The thermal decomposition half-life of azobisisobutyronitrile (AIB) in ethyl acetate decreases progressively with increasing temperature, while the decomposition rate increases progressively. The thermal decomposition half-life Tazobisisobutyronitrile in ethyl acetate was determined to be... 1 / 2 The thermal decomposition half-life is as follows: approximately 4.5~5.5 h at 64.5~65.5℃, approximately 3.5~4.5 h at 66.5~67.5℃, and approximately 2.0~3.0 h at 70.0~71.0℃. The thermal decomposition half-life can be determined using UV-Vis spectrophotometry: the absorbance of an ethyl acetate solution of azobisisobutyronitrile (AIBN) at approximately 240 nm is tracked over time, and the time required for the absorbance to decrease to half of its initial value is taken as the thermal decomposition half-life.

[0033] The reaction temperature, isothermal time, and initiator drop rate in each stage of the present invention are all designed to match the above-mentioned thermal decomposition half-life of azobisisobutyronitrile in ethyl acetate.

[0034] The first stage (S20, 64.5~65.5℃, isothermal polymerization for 3~4h): At this temperature, the half-life of azobisisobutyronitrile (AIBN) is relatively long, the initiator decomposes slowly, and free radicals are released stably at a low rate. The low and stable free radical concentration can suppress auto-acceleration effects and chain transfer side reactions, allowing the molecular chains to grow fully with a low termination probability, forming a high molecular weight, low branching polymer backbone. The system is exothermic and the temperature control is stable, which can avoid early burst polymerization that leads to a broadened molecular weight distribution, laying the molecular weight foundation for high cohesive performance throughout the polymerization process.

[0035] The second stage (S30, 66.5~67.5℃, isothermal polymerization for 2~3h): The temperature is gradually increased to a range with a suitable half-life, and a second initiator is added. Before the risk of chain transfer due to temperature increase increases significantly, the newly added initiator continuously replenishes the active free radicals, compensating for the lack of free radicals caused by the decrease in the supply capacity of the residual initiator in the first stage, so that the system can maintain a sufficient polymerization rate and conversion rate. The staged addition avoids the sudden increase in free radical concentration caused by a single large addition of initiator, and can continuously improve the monomer conversion rate without destroying the molecular chain structure or broadening the molecular weight distribution. This allows the free radical supply curve and the monomer consumption curve to be dynamically coupled, preparing for the deep conversion in the third stage.

[0036] The third stage (S40, 70.0~71.0℃, slow dropwise addition of initiator solution, isothermal polymerization for 3~4h): The temperature is further increased to a range with a shorter half-life, utilizing a more efficient initiator decomposition rate to continuously activate trace amounts of residual monomers in the system, achieving deep conversion of residual monomers. Traditional late-stage curing dropwise addition processes often involve dissolving the initiator in a small amount of solvent and then rapidly adding it dropwise. Once the initiator enters the high-viscosity system, it easily accumulates locally and releases a large number of free radicals instantaneously, leading to side reactions such as chain transfer and bite-β cleavage. This results in a decrease in polymer molecular weight and a broadening of the molecular weight distribution, while residual monomers are difficult to completely remove. In the third stage of this invention, 0.01-0.02 parts of azobisisobutyronitrile are thoroughly diluted with 35-42 parts of ethyl acetate to form a low-concentration, highly dispersible initiator solution. This solution is then added dropwise at a low rate of 0.3-0.7 mL / min, ensuring the generation of free radicals in trace amounts, uniformly, and continuously, achieving a uniform supply across the entire system. This method matches the half-life at 70.0-71.0 °C, allowing the terminal residual monomers to slowly complete chain growth at low free radical concentrations. This is beneficial for increasing the overall molecular weight of the polymer and achieving deep conversion of residual monomers. It also suppresses side reactions such as chain transfer and bite-β cleavage at higher temperatures, maintaining a high molecular weight and narrow molecular weight distribution while ensuring low residual monomers. Furthermore, sufficient dilution solvent improves the diffusion and miscibility of the initiator in high-viscosity systems, avoiding problems such as gel particles and system inhomogeneity caused by local over-initiation. This is beneficial for improving the uniformity, transparency, and process stability of the polymer solution.

[0037] After the reaction, the high molecular weight acrylate molecules exhibit strong entanglement. Rapid cooling can cause sudden aggregation of the molecular chains and localized phase separation, directly leading to a wider molecular weight distribution and a cloudy product appearance. This invention limits the cooling rate to no more than 5°C / 10 min, allowing the polymer chains to gradually relax and disperse uniformly in the solvent, solidifying the molecular chain structure and further consolidating the narrow distribution characteristics. Simultaneously, slow cooling avoids thermal stress concentration in the system, which helps improve the consistency of batch product performance.

[0038] Raw material specifications

[0039] The raw material specifications used in each embodiment and comparative example include: all acrylate monomers are industrial grade, with the original manufacturer adding the polymerization inhibitor p-methoxyphenol; azobisisobutyronitrile (AIBN) is analytical grade, purified by recrystallization from methanol, with a purity of not less than 99.0%, stored at room temperature in a sealed container away from light, and used immediately; ethyl acetate is analytical grade or industrial grade, with a moisture content not exceeding 0.05%, and used after drying with 4A molecular sieves; high-purity nitrogen has a purity of not less than 99.999%; deionized water has a resistivity of not less than 18.2 MΩ·cm; sodium hydroxide is analytical grade and used to prepare the washing alkali solution. Each part in the formulation is based on a mass of 1 g.

[0040] Test methods

[0041] (1) Solid content: According to GB / T1725-2007, weigh 2g of sample and dry it in a 105℃ drying oven for 2h, cool it and weigh it to calculate the solid content.

[0042] (2) Weight average molecular weight and molecular weight dispersion: The weight average molecular weight and molecular weight dispersion were determined by gel permeation chromatography (GPC) with a Styragel HR3+HR4 tandem column, tetrahydrofuran (THF) as the mobile phase, a flow rate of 1.0 mL / min, a test temperature of 30 °C, and narrow distribution polystyrene standard as the standard sample.

[0043] (3) Residual monomer content: The content was determined by gas chromatography (GC) equipped with an FID detector. The chromatographic column was a weakly polar capillary column, and the carrier gas was high-purity nitrogen. The total residual amount of isooctyl acrylate, butyl acrylate and hydroxyethyl acrylate was quantitatively determined by external standard method.

[0044] Group 1

[0045] Example 1

[0046] The preparation method of the acrylate copolymer in this embodiment includes the following steps:

[0047] S60: Prepare a 5% (w / w) sodium hydroxide dilute aqueous solution as the washing solution; mix each monomer with the washing solution at a volume ratio of 1:1, and wash with magnetic stirring at room temperature for 15 minutes each time, for a total of 2 washes; separate the lower aqueous phase, and repeatedly rinse the organic phase with deionized water, stirring for 8 minutes each time, until the pH of the aqueous phase is 7.0; transfer the washed monomers to a dry container and let them stand at room temperature for 15 hours to dehydrate; after dehydration, seal and store the monomers in the dark, and put them into use within 60-72 hours.

[0048] S10: By mass, 65 parts of isooctyl acrylate, 20 parts of butyl acrylate, and 5 parts of hydroxyethyl acrylate are mixed and dissolved in 180 parts of ethyl acetate in a reaction vessel. The mixture is stirred at 200 rpm for 30 minutes to obtain a homogeneous reaction solution.

[0049] S70: High-purity nitrogen gas is introduced into the reaction solution to replace the air and dissolved oxygen. The aeration time is 30 minutes. After the aeration is completed, the reaction system is kept under a slightly positive pressure and sealed.

[0050] S20: Slowly heat the reaction solution to 65°C and keep it at a constant temperature. Add 0.03 parts of azobisisobutyronitrile and polymerize at a constant temperature for 3.5 hours.

[0051] S30: Continue heating to 67℃ and maintain the temperature, add 0.015 parts of azobisisobutyronitrile, and continue the polymerization reaction at the constant temperature for 2.5h.

[0052] S40: Further heat to 70.5℃ and maintain constant temperature. Add the initiator solution dropwise to the reaction solution at a rate of 0.5 mL / min. After the addition is complete, continue the polymerization reaction at constant temperature for 3.5 h. The initiator solution is obtained by completely dissolving 0.015 parts of azobisisobutyronitrile in 35 parts of ethyl acetate and adding it dropwise at a constant rate for 70 min.

[0053] S50: After the reaction is completed, room temperature circulating cooling water is introduced into the jacket of the reactor, and the cooling rate of the reaction solution in the reactor is controlled at 5℃ / 10min. The reaction solution is gradually cooled to room temperature. The bottom outlet of the reactor is opened, and a 200-mesh filter is used in series with a precision filter to filter the material and remove trace insoluble impurities to obtain an acrylate copolymer solution.

[0054] The acrylate copolymer obtained in this embodiment has a weight-average molecular weight in the range of 640,000 to 1,100,000, a molecular weight dispersion in the range of 2.1 to 2.8, and a residual monomer content in the range of 0.22% to 0.45%. All three indicators meet the engineering requirements for high molecular weight resins for pressure-sensitive adhesives.

[0055] Example 2

[0056] The only difference between this embodiment and Example 1 is that: in S60, the single washing time is 20 minutes, and the washing is done once, rinsing until the pH of the aqueous phase is 6.5, and dehydration is carried out for 10 hours; in S10, 60 parts by mass of isooctyl acrylate, 12 parts by mass of butyl acrylate, and 3 parts by mass of hydroxyethyl acrylate are dissolved in 150 parts by mass of ethyl acetate, and the stirring speed is 150 rpm; in S70, aeration is carried out for 20 minutes; in S20, the temperature is raised to 64.5°C and kept constant, and 0.02 parts by mass of azobisisobutyronitrile are added, and polymerization is carried out at a constant temperature. The reaction should proceed for 3 hours; for S30, the temperature is raised to 66.5℃ and kept constant, and 0.01 parts of azobisisobutyronitrile are added, and the polymerization reaction is carried out at a constant temperature for 2 hours; for S40, the temperature is raised to 70.0℃ and kept constant, and the initiator solution is added dropwise at a rate of 0.3 mL / min. After the addition is completed, the polymerization reaction is continued at a constant temperature for 3 hours. The initiator solution is obtained by dissolving 0.01 parts of azobisisobutyronitrile in 36 parts of ethyl acetate, and the dropwise addition time is 120 min; for S50, a 150-mesh filter is used to filter the material through a series of precision filters.

[0057] In this embodiment, a low total initiator amount (0.04 parts) and a minimum monomer feed (60 / 12 / 3) were used. In the third stage, the monomer was added at an ultra-slow rate of 0.3 mL / min for a long time of 120 min. The weight-average molecular weight, molecular weight dispersion and residual monomer content of the resulting copolymer all met the aforementioned requirements. Extending the dropping window and matching the half-life is beneficial to further reduce residual monomer without damaging the molecular weight.

[0058] Example 3

[0059] The only difference between this embodiment and Example 1 is that: in S60, each wash lasts 10 minutes, and a total of 3 washes are performed, rinsing until the pH of the aqueous phase is 7.5, and dehydration lasts for 20 hours; in S10, 70 parts by weight of isooctyl acrylate, 25 parts by weight of butyl acrylate, and 8 parts by weight of hydroxyethyl acrylate are dissolved in 200 parts by weight of ethyl acetate, and the stirring speed is 250 rpm; in S70, aeration is carried out for 40 minutes; in S20, the temperature is raised to 65.5°C and kept constant, and 0.05 parts by weight of azobisisobutyronitrile are added, followed by constant-temperature polymerization. The reaction was carried out for 4 hours; S30 was heated to 67.5℃ and kept at a constant temperature, and 0.02 parts of azobisisobutyronitrile were added, and the polymerization reaction was carried out at a constant temperature for 3 hours; S40 was heated to 71.0℃ and kept at a constant temperature, and the initiator solution was added dropwise at a rate of 0.7 mL / min. After the addition was completed, the polymerization reaction was continued at a constant temperature for 4 hours. The initiator solution was obtained by dissolving 0.02 parts of azobisisobutyronitrile in 42 parts of ethyl acetate, and the dropwise addition time was 60 min; S50 was filtered by a 250-mesh filter in series with a precision filter.

[0060] This embodiment uses the maximum monomer feed (70 / 25 / 8) and a relatively long reaction time in each stage. The resulting copolymer has a molecular weight dispersion of about 2.1 and a residual monomer content of about 0.22%, which is the scheme with the narrowest distribution and the lowest residual monomer content in the embodiment group. The higher hydroxyethyl acrylate content (8 parts) also provides more hydroxyl crosslinking points for subsequent crosslinking applications.

[0061] Example 4

[0062] The only difference between this embodiment and Example 1 is that: in S10, the modified monomer methyl methacrylate (MMA) is added to participate in the polymerization. The modified monomer is 6 parts by mass, and after being mixed with isooctyl acrylate, butyl acrylate and hydroxyethyl acrylate, it is dissolved in ethyl acetate to obtain a homogeneous reaction solution.

[0063] Methyl methacrylate is a hard monomer. Its introduction can improve the glass transition temperature and cohesive strength of the copolymer, making it suitable for pressure-sensitive adhesives or coatings that require higher holding power and temperature resistance. The copolymer composition of methyl methacrylate with soft monomers isooctyl acrylate and butyl acrylate can be adjusted by adjusting the amount to balance the initial tack and holding power.

[0064] Example 5

[0065] The only difference between this embodiment and Example 1 is that: in S10, the modified monomer lauryl acrylate (LA) is added to participate in the polymerization. The modified monomer is 5 parts by mass, and after being mixed with isooctyl acrylate, butyl acrylate and hydroxyethyl acrylate, it is dissolved in ethyl acetate to obtain a homogeneous reaction solution.

[0066] Lauryl acrylate is a long-chain soft monomer with highly flexible side chains and high steric hindrance. It can reduce the glass transition temperature, improve initial tack and wettability, and inhibit chain transfer and excessive intermolecular entanglement through its hydrophobic long chains. The copolymer obtained in Example 5 has a weight-average molecular weight of about 1.1 million, which is the highest in the example group, indicating that the process of the present invention is universally applicable to a variety of monomer systems.

[0067] Example 6

[0068] The only difference between this embodiment and Example 1 is that: in S10, the modified monomer glycidyl methacrylate (GMA) is added to participate in the polymerization. The modified monomer is 3 parts by mass, and after being mixed with isooctyl acrylate, butyl acrylate and hydroxyethyl acrylate, it is dissolved in ethyl acetate to obtain a homogeneous reaction solution.

[0069] Glycidyl methacrylate contains epoxy groups, which can undergo cross-linking reactions with amino and carboxyl groups after coating and film formation, thereby improving the cohesive strength, solvent resistance and heat resistance of the adhesive layer. It can be used in pressure-sensitive adhesives or protective film systems that require cross-linking and curing.

[0070] Example 7

[0071] The only difference between this embodiment and Embodiment 1 is that steps S60 and S70 are omitted.

[0072] Example 8

[0073] The only difference between this embodiment and Embodiment 1 is that step S60 is omitted.

[0074] Example 9

[0075] The only difference between this embodiment and Embodiment 1 is that step S70 is omitted.

[0076] Example 10

[0077] The only difference between this embodiment and Embodiment 1 is that step S70 involves nitrogen deoxygenation for 20 minutes.

[0078] Example 11

[0079] The only difference between this embodiment and Embodiment 1 is that step S70 involves nitrogen deoxygenation for 40 minutes.

[0080] Comparative Example 1

[0081] The preparation method of the acrylate copolymer in this comparative example includes the following steps:

[0082] S10: By mass, 65 parts of isooctyl acrylate, 20 parts of butyl acrylate, and 5 parts of hydroxyethyl acrylate are mixed and dissolved in 180 parts of ethyl acetate in a reaction vessel. The mixture is stirred at 200 rpm for 30 minutes to obtain a homogeneous reaction solution.

[0083] S70: High-purity nitrogen gas is introduced into the reaction solution to replace the air and dissolved oxygen. The aeration time is 30 minutes. After the aeration is completed, the reaction system is kept under a slightly positive pressure and sealed.

[0084] S20: Slowly heat the reaction solution to 60°C and keep it at a constant temperature. Add 0.03 parts of azobisisobutyronitrile and polymerize at a constant temperature for 3.5 hours.

[0085] S30: Continue heating to 65℃ and maintain the temperature, add 0.015 parts of azobisisobutyronitrile, and continue the polymerization reaction at the constant temperature for 2.5h.

[0086] S40: Further heat to 70℃ and maintain the temperature, add the initiator solution dropwise to the reaction solution at a rate of 0.5 mL / min, and continue the polymerization reaction at a constant temperature for 3.5 h after the addition is complete; the initiator solution is obtained by completely dissolving 0.015 parts of azobisisobutyronitrile in 10 parts of ethyl acetate, and the dropwise addition time is 20 min.

[0087] S50: After the reaction is completed, room temperature circulating cooling water is introduced into the jacket of the reactor to control the reaction solution in the reactor to drop to room temperature rapidly at a cooling rate of more than 10℃ / 10min. The bottom outlet of the reactor is opened, and the material is filtered by a 200-mesh filter in series with a precision filter to remove trace amounts of insoluble impurities and obtain an acrylate copolymer solution.

[0088] Comparative Example 1 is a control scheme that deviates from the principle of half-life matching: the temperature in the first stage is only 60℃ and the temperature in the second stage is only 65℃. The decomposition of azobisisobutyronitrile is too slow and the supply of free radicals is insufficient, resulting in a low molecular weight starting point. In the third stage, the initiator is diluted with only 10 parts of ethyl acetate and added rapidly over 20 minutes. The low dilution and rapid addition lead to local enrichment of the initiator and instantaneous release of a large number of free radicals, triggering side reactions such as chain transfer and backbiting-β cleavage, which reduces the molecular weight. Moreover, the free radicals are quickly depleted and cannot continuously activate the residual monomers. With the addition of rapid cooling, the molecular weight distribution is further broadened.

[0089] Table 1 shows the comparison results of the test data corresponding to each embodiment and comparative example in Group 1:

[0090] Table 1

[0091]

[0092] Effect Analysis

[0093] Test results show that the weight-average molecular weights of the acrylate copolymers obtained in Examples 1-6 are all distributed between 640,000 and 1,100,000, meeting the requirement of not less than 600,000. Example 5 reaches approximately 1,100,000, while Comparative Example 1 is only about 360,000, far below the lower limit. The molecular weight dispersion is between 2.1 and 2.8, meeting the requirement of not exceeding 3.0. Example 3 is as low as about 2.1, while Comparative Example 1 is as high as about 4.2. The residual monomer content is between 0.22% and 0.45%, meeting the requirement of not exceeding 0.50%. Example 3 is as low as about 0.22%, while Comparative Example 1 is as high as about 1.56%. The above data are obtained based on the test methods (gel permeation chromatography and gas chromatography) described in the specific embodiments of this invention, and do not extend to other test conditions not disclosed in the prior art of this invention.

[0094] The parameters of Comparative Example 1 deviated from the half-life matching principle: the first stage temperature was only 60℃, the decomposition of azobisisobutyronitrile was too slow, the supply of free radicals was insufficient, and the starting molecular weight was too low; the second stage temperature was only 65℃, and the addition of initiator could not effectively decompose the initiator, resulting in limited improvement in conversion rate; in the third stage, only 10 parts of ethyl acetate were used to dilute the initiator and the addition was only 20 minutes. The low dilution and rapid addition caused the initiator to be locally enriched and release a large number of free radicals instantly. On the one hand, this triggered side reactions such as chain transfer and bite-β cleavage, which reduced the molecular weight; on the other hand, the free radicals were quickly consumed and could not be continuously activated to activate the residual monomers. At the same time, the rapid cooling further aggravated the broadening of the molecular weight distribution. The superposition of the above multiple factors led to the comprehensive deterioration of Comparative Example 1 in terms of molecular weight, distribution width, and residual monomers. This shows that the overall synergy of the three temperature steps and half-life matching, the slow addition of low concentration and large dilution at the end and the gradient cooling is necessary for the technical effect of this invention.

[0095] From an application perspective, high molecular weight (weight average molecular weight 640,000~1,100,000) corresponds to higher cohesive strength, which is beneficial to improving the holding power and shear resistance of pressure-sensitive adhesives; narrow distribution (molecular weight dispersion 2.1~2.8) ensures consistent molecular chain behavior within a batch, resulting in uniform coating and film formation, which can reduce coating defects and haze in optical films and other applications; low residual monomer (0.22%~0.45%) reduces the risk of odor, precipitation and yellowing from the source, meeting the requirements of environmental protection and optical applications.

[0096] Group 2

[0097] E1-1: The only difference between this embodiment and Embodiment 1 is that: the constant temperature in S20 is 64.5℃ and the reaction time is 3h; the constant temperature in S30 is 66.5℃ and the reaction time is 2h; the constant temperature in S40 is 70.0℃ and the reaction time is 3h.

[0098] E1-2: The only difference between this embodiment and embodiment 1 is that the constant temperature in S20 is 65.5℃ and the reaction time is 4h; the constant temperature in S30 is 67.5℃ and the reaction time is 3h; and the constant temperature in S40 is 71.0℃ and the reaction time is 4h.

[0099] E1-3: The only difference between this embodiment and Embodiment 1 is that the reaction time in S20 is 3 hours; the reaction time in S30 is 2 hours; and the reaction time in S40 is 3 hours.

[0100] D1-1: The only difference between this comparative example and Example 1 is that the polymerization was carried out at a constant temperature of 65°C throughout, AIBN was added all at once in total, and the total constant temperature reaction time was the same as in Example 1.

[0101] D1-2: The only difference between this comparative example and Example 1 is that: S40: The temperature is further increased to 70.5℃ and kept constant. The initiator solution is added dropwise to the reaction solution at a rate of 0.5 mL / min. After the addition is complete, the polymerization reaction is continued at a constant temperature for 3.5 h. The initiator solution is obtained by completely dissolving 0.03 parts of azobisisobutyronitrile in 35 parts of ethyl acetate. The dropwise addition time is 70 min.

[0102] D1-3: The only difference between this comparative example and Example 1 is that the constant temperature in S20 is 62°C; the constant temperature in S30 is 64°C; and the constant temperature in S40 is 68°C.

[0103] D1-4: The only difference between this comparative example and Example 1 is that the constant temperature in S20 is 75°C; the constant temperature in S30 is 80°C; and the constant temperature in S40 is 85°C.

[0104] Table 2 shows the comparison results of the test data corresponding to each embodiment and comparative example in Group 2:

[0105] Table 2

[0106]

[0107] Group 3

[0108] E2-1: The only difference between this embodiment and Example 1 is that in S40, 36 parts of ethyl acetate were used to prepare the initiator solution, the dropping rate was 0.3 mL / min, and the dropping time was 120 min;

[0109] E2-2: The only difference between this example and Example 1 is that in S40, 38 parts of ethyl acetate were used to prepare the initiator solution, the dropping rate was 0.6 mL / min, and the dropping time was about 63 min;

[0110] D2-1: The only difference between this comparative example and Example 1 is that 30 parts of ethyl acetate were used to prepare the initiator solution in S40;

[0111] D2-2: The only difference between this comparative example and Example 1 is that no AIBN is added dropwise in S40, but an equal amount is added at once;

[0112] D2-3: The only difference between this comparative example and Example 1 is that the dropping rate in S40 is increased to 3 mL / min;

[0113] D2-4: The only difference between this comparative example and Example 1 is that 50 parts of ethyl acetate were used to prepare the initiator solution in S40;

[0114] Table 3 shows the comparison results of the test data corresponding to each embodiment and comparative example in Group 3:

[0115] Table 3

[0116]

[0117] Group 4

[0118] E3-1: The only difference between this embodiment and Embodiment 1 is that the cooling rate in S50 is 4℃ / 10min;

[0119] E3-2: The only difference between this embodiment and Embodiment 1 is that the cooling rate in S50 is 1℃ / 10min;

[0120] E3-3: The only difference between this embodiment and embodiment 1 is that gradient cooling is used in S50: from 70.5℃ to 50℃ at a cooling rate of 3.42℃ / 10min; then to 40℃ at a cooling rate of 1.7℃ / 10min; and finally to room temperature at a cooling rate of 1℃ / 10min.

[0121] E3-4: The only difference between this embodiment and embodiment 1 is that gradient cooling is used in S50: from 70.5℃ to 50℃ at a cooling rate of 5℃ / 10min; then to 40℃ at a cooling rate of 3.3℃ / 10min; and finally to room temperature at a cooling rate of 5℃ / 10min.

[0122] E3-5: The only difference between this embodiment and embodiment 1 is that gradient cooling is used in S50: from 70.5℃ to 50℃ at a cooling rate of 5℃ / 10min; then to 40℃ at a cooling rate of 2.5℃ / 10min; and finally to room temperature at a cooling rate of 3℃ / 10min.

[0123] D3-1: The only difference between this comparative example and Example 1 is that the cooling rate in S50 is 8°C / 10min for all processes.

[0124] D3-2: The only difference between this comparative example and Example 1 is that the cooling rate in S50 is 0.5℃ / 10min for the entire process;

[0125] D3-3: The only difference between this comparative example and Example 1 is that in S50, the polymerization ends without temperature control and the material is discharged directly at high temperature.

[0126] Table 4 shows the comparison results of the test data corresponding to each embodiment and comparative example in Group 4:

[0127] Table 4

[0128]

[0129] It will be apparent to those skilled in the art that this disclosure is not limited to the details of the exemplary embodiments described above, and that this disclosure can be implemented in other specific forms without departing from the spirit or essential characteristics of this disclosure. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of this disclosure is defined by the appended claims rather than the foregoing description. Thus, it is intended that all variations falling within the meaning and scope of equivalents of the claims be included within this disclosure.

[0130] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.

Claims

1. A method for preparing an acrylate copolymer, comprising: S10: Based on the mass fraction of monomers, 60-70 parts of isooctyl acrylate, 12-25 parts of butyl acrylate, and 3-8 parts of hydroxyethyl acrylate are mixed and dissolved in 150-200 parts of ethyl acetate to obtain a homogeneous reaction solution. Prepare an initiator solution, which is obtained by dissolving at least 0.01 to 0.02 parts of azobisisobutyronitrile in 35 to 42 parts of ethyl acetate; S20: Heat the reaction solution to 64.5~65.5℃ and keep it at a constant temperature, add 0.02~0.05 parts of azobisisobutyronitrile, and polymerize at a constant temperature for 3~4 hours to obtain the first reaction solution; S30: Heat the first reaction solution to 66.5~67.5℃ and keep it at a constant temperature, add 0.01~0.02 parts of azobisisobutyronitrile, and polymerize at a constant temperature for 2~3 hours to obtain the second reaction solution; S40: Heat the second reaction solution to 70.0~71.0℃ and keep it at a constant temperature. Add the initiator solution dropwise to the reaction system at a rate of 0.3~0.7mL / min. After the addition is complete, continue the polymerization reaction at a constant temperature of 70.0~71.0℃ for 3~4 hours and then stop the reaction. S50: After the reaction is complete, control the cooling rate to not exceed 5℃ / 10min, cool the reaction system to room temperature, filter to remove impurities, and obtain an acrylate copolymer solution.

2. The method for preparing the acrylate copolymer according to claim 1, characterized in that, In S50, the cooling is a gradient cooling: from 70.0~71.0℃ to 50℃, the cooling process in this stage is controlled within 41~60min; then to 40℃, the cooling process in this stage is controlled within 30~60min; finally to room temperature, the cooling rate is 1~5℃ / 10min.

3. The method for preparing the acrylate copolymer according to claim 1, characterized in that, In S40, the initiator solution is added at a constant rate for 60-120 minutes.

4. The method for preparing the acrylate copolymer according to claim 1, characterized in that, In S20 and / or S30, the azobisisobutyronitrile is first dissolved in 5 to 10 times its mass of ethyl acetate to form a homogeneous initiator mother liquor, and then added in a single injection or in a thin stream over 30 to 90 seconds.

5. The method for preparing the acrylate copolymer according to claim 1, characterized in that, Before S10, there is also a monomer pretreatment step S60: isooctyl acrylate, butyl acrylate and hydroxyethyl acrylate are washed with a 5% sodium hydroxide aqueous solution to remove the polymerization inhibitor, rinsed with deionized water until neutral and dehydrated and dried.

6. The method for preparing the acrylate copolymer according to claim 5, characterized in that, In S60, each monomer is mixed with a 5% sodium hydroxide aqueous solution at a volume ratio of 1:1, and washed at room temperature with stirring for 10-20 minutes, for a total of 1-3 times. After separating the aqueous phase, the organic phase is rinsed with deionized water until the pH of the aqueous phase after rinsing is 6.5-7.

5. After standing at room temperature for 10-20 hours to dehydrate, the mixture is sealed and stored away from light, and put into use within 60-72 hours.

7. The method for preparing the acrylate copolymer according to claim 1, characterized in that, After S10 and before S20, there is also a deoxygenation step S70: high-purity nitrogen is introduced into the reaction solution to replace the air and dissolved oxygen. The aeration time is 20-40 minutes. After the aeration is completed, the reaction system is kept in a slightly positive pressure sealed state.

8. The method for preparing the acrylate copolymer according to claim 1, characterized in that, Stirring is also maintained in S20 and / or S30 and / or S40 at a speed of 150-250 rpm.

9. The method for preparing the acrylate copolymer according to claim 1, characterized in that, In S10, 1 to 15 parts of a modified monomer are added to the monomer, which is mixed with isooctyl acrylate, butyl acrylate, and hydroxyethyl acrylate and then dissolved in ethyl acetate to obtain a homogeneous reaction solution; the modified monomer is at least one of methyl methacrylate, lauryl acrylate, and glycidyl methacrylate.

10. The method for preparing the acrylate copolymer according to claim 1, characterized in that, In S50, the filtration and impurity removal is carried out by using a precision filter with a 150-300 mesh screen in series.