A PET-based nano-ZnO antibacterial masterbatch, its preparation method and application
By combining high and low viscosity PET and surface-modifying nano-ZnO particles, the problem of uneven dispersion of nano-ZnO particles in PET matrix was solved, achieving uniform dispersion and stable processing of PET-based nano-ZnO antibacterial masterbatch, improving antibacterial and processing performance, and broadening the application range.
Patent Information
- Application Number
- CN202611320616.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-17
AI Technical Summary
In existing technologies, nano-ZnO particles are not evenly dispersed in the PET matrix, resulting in uneven melt flow properties of the masterbatch and insufficient processing performance, making it difficult to meet the needs of high-end spinning fields. Furthermore, existing improvement methods suffer from poor compatibility or complex processes that are difficult to scale up.
High-viscosity PET and low-viscosity PET are blended and nano-ZnO particles are treated with surface modifiers and then melt-blended using a twin-screw extruder to prepare PET-based nano-ZnO antibacterial masterbatch, ensuring uniform dispersion of nano-ZnO particles in the PET matrix.
This method achieves uniform dispersion of nano-ZnO particles in a PET matrix, improves the processing stability and antibacterial properties of the masterbatch, broadens its application range, is suitable for large-scale production, and avoids problems such as poor compatibility and complex processes.
Smart Images

Figure CN123107316A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of polymer functional masterbatch technology, specifically relating to a PET-based nano-ZnO antibacterial masterbatch, its preparation method, and its application. Background Technology
[0002] In the spinning process, antibacterial agents are typically introduced to impart antibacterial properties to PET fibers. In recent years, given considerations of environmental protection and human health, nano-ZnO particles, as an inorganic antibacterial agent, have gradually received widespread attention and have begun to be applied to the research and development of PET-based antibacterial masterbatches.
[0003] In existing technical solutions, PET with a single viscosity is generally used as the masterbatch matrix, and it is melt-blended and extruded with nano ZnO particles to prepare PET-based antibacterial masterbatch.
[0004] However, when the PET of a single viscosity is either low-viscosity or high-viscosity, it is difficult to achieve uniform dispersion of nano-ZnO particles in the PET matrix. The specific reasons are as follows: high-viscosity PET cannot allow nano-ZnO particles to be dispersed in the initial stage; although low-viscosity PET is conducive to the initial dispersion of nano-ZnO particles, it cannot maintain their stable distribution in the system after dispersion, and local enrichment or segregation is prone to occur.
[0005] The uneven dispersion of nano-ZnO particles in the PET matrix has multiple effects. It not only leads to uneven flow properties of the masterbatch melt, but also makes the preparation of high-concentration masterbatches difficult, thus limiting their effectiveness in functional applications such as antibacterial and antifungal properties.
[0006] When the PET with a single viscosity is low-viscosity PET, insufficient processing performance will also occur. This is because during the high-temperature melting process, nano-ZnO particles can easily cause a significant decrease in the viscosity of low-viscosity PET, leading to a series of problems such as insufficient melt strength, large processing fluctuations, and poor fiber spinnability. More importantly, due to the limitation of the decrease in masterbatch viscosity, its application range is usually limited to the production of conventional short fibers or filaments, making it difficult to meet the needs of PET industrial yarn preparation with higher requirements for melt viscosity and stability. This seriously restricts its promotion and application in the high-end spinning field.
[0007] The decrease in PET viscosity is mainly due to two factors: Firstly, the Lewis acid / base sites on the surface of nano-ZnO particles, in the presence of trace amounts of water or terminal carboxyl groups, promote the breakage of ester bonds, causing the PET chains to transform from long chains to short chains, reducing the average molecular weight and consequently decreasing the viscosity. Secondly, the dispersed nanoparticles reduce the friction or entanglement between polymer chains, making the system exhibit stronger shear-thinning properties, resulting in a more significant decrease in viscosity. Low-viscosity PET itself has short chains and less entanglement, making it more sensitive to further chain breakage, hence the larger decrease in viscosity.
[0008] To address the aforementioned issues, some processes have been attempted. For example, patent application CN102933654A, "Antibacterial Resin Composition Formed from Masterbatch," attempts to partially replace PET with polybutylene terephthalate (PBT) to improve flowability and dispersibility of the antibacterial material. However, PBT and PET differ in molecular structure, resulting in poor compatibility when blended. This leads to interfacial separation during spinning, affecting the evenness and dyeing uniformity of subsequent fibers, thus limiting its further application. Furthermore, patent CN109280345B, "A Composite Antibacterial Polyester Masterbatch and Its Preparation Method," employs a multi-stage liquid-phase thickening process to increase masterbatch viscosity. However, this process is complex, requires extremely high equipment precision, and is difficult to implement on a large scale in actual production, resulting in significant fluctuations in product quality.
[0009] In summary, there is an urgent need for a new method for preparing PET-based nano-ZnO antibacterial masterbatch that combines excellent processability and dispersibility with stable and easy-to-operate processes. Summary of the Invention
[0010] The purpose of this invention is to solve the problems existing in the prior art and to provide a PET-based nano-ZnO antibacterial masterbatch, its preparation method, and its application.
[0011] To achieve the above objectives, the technical solution adopted by the present invention is as follows:
[0012] A PET-based nano-ZnO antibacterial masterbatch includes a substrate and modified nano-ZnO particles dispersed therein.
[0013] The substrate is composed of high-viscosity PET and low-viscosity PET;
[0014] The intrinsic viscosity of high-viscosity PET is 0.80-1.20 dL / g, and the intrinsic viscosity of low-viscosity PET is 0.40-0.55 dL / g. The difference in intrinsic viscosity between high-viscosity PET and low-viscosity PET is 0.40-0.65 dL / g.
[0015] The mass ratio of high-viscosity PET to low-viscosity PET is 30-70:70-30;
[0016] Modified nano-ZnO particles are obtained by treating nano-ZnO particles with a surface modifier. During the treatment, the amount of surface modifier used is more than 1% of the mass of the nano-ZnO particles.
[0017] As a preferred technical solution:
[0018] In the PET-based nano-ZnO antibacterial masterbatch described above, the amount of surface modifier used during processing is less than 10% of the mass of the nano-ZnO particles.
[0019] The PET-based nano-ZnO antibacterial masterbatch described above uses one or more of the following as surface modifiers: silane coupling agent, phosphate ester, stearic acid, carboxylated polymer, and dopamine derivatives.
[0020] The PET-based nano-ZnO antibacterial masterbatch described above has nano-ZnO particles with a particle size of 20-80 nm. This particle size range falls within the commonly used industrial particle size range for nano-ZnO particles in polyester masterbatches. Within this range, the nano-ZnO particles can ensure a high specific surface area, thereby achieving effective antibacterial properties, while also facilitating thorough wetting and dispersion in the melt.
[0021] The PET-based nano-ZnO antibacterial masterbatch described above contains modified nano-ZnO particles at a mass content of 10%-40%. This range covers typical industrial applications, from conventional antibacterial masterbatches (10%-20% mass content) to high-efficiency or multifunctional antibacterial masterbatches (20%-40% mass content), meeting the antibacterial performance requirements of different fiber applications. 10%-40% is a mature and industrially viable range for nano-ZnO particle loading. This invention is not intended to be inventive; this addition range is merely a reasonable selection to ensure masterbatch performance and processability.
[0022] The PET-based nano-ZnO antibacterial masterbatch described above also includes additives dispersed in the substrate; the additives are one or more of fatty acid esters, polyethylene wax, amphiphilic polyester wax, amide wax and E-GMA-VA (ethylene-glycidyl methacrylate-vinyl acetate terpolymer); the mass content of the additives in the PET-based nano-ZnO antibacterial masterbatch is 0.5%-2%.
[0023] As described above, the PET-based nano-ZnO antibacterial masterbatch has a filtration pressure value of no more than 0.1 bar / g, indicating that the modified nano-ZnO particles have high dispersion uniformity. The actual intrinsic viscosity of the PET-based nano-ZnO antibacterial masterbatch is 85%-110% of the theoretical intrinsic viscosity. The theoretical intrinsic viscosity = mass percentage of high-viscosity PET in the substrate × intrinsic viscosity of high-viscosity PET + mass percentage of low-viscosity PET in the substrate × intrinsic viscosity of low-viscosity PET. Therefore, the intrinsic viscosity of the PET-based nano-ZnO antibacterial masterbatch decreases only slightly during processing.
[0024] This invention also provides a method for preparing PET-based nano-ZnO antibacterial masterbatch. First, multiple formulations of PET-based nano-ZnO antibacterial masterbatch are designed. Then, Monte Carlo simulation is used to screen out the formulation with the best dispersion uniformity of modified nano-ZnO particles. Finally, production and processing are carried out according to the formulation.
[0025] PET-based nano-ZnO antibacterial masterbatch includes a substrate and modified nano-ZnO particles dispersed therein;
[0026] The substrate is composed of high-viscosity PET and low-viscosity PET;
[0027] The intrinsic viscosity of high-viscosity PET is 0.80-1.20 dL / g, and the intrinsic viscosity of low-viscosity PET is 0.40-0.55 dL / g. The difference in intrinsic viscosity between high-viscosity PET and low-viscosity PET is 0.40-0.65 dL / g.
[0028] The mass ratio of high-viscosity PET to low-viscosity PET is 30-70:70-30;
[0029] Modified nano-ZnO particles are obtained by treating nano-ZnO particles with a surface modifier. During the treatment, the amount of surface modifier used is more than 1% of the mass of the nano-ZnO particles.
[0030] The variables in the formulation are the intrinsic viscosity of high-viscosity PET, the intrinsic viscosity of low-viscosity PET, and the mass ratio of high-viscosity PET to low-viscosity PET.
[0031] As a preferred technical solution:
[0032] The preparation method of the PET-based nano-ZnO antibacterial masterbatch described above involves the following process: after preparing modified nano-ZnO particles, they are mixed with high-viscosity PET, low-viscosity PET and additives to form a premix, and then the premix is melt-blended and granulated to obtain the PET-based nano-ZnO antibacterial masterbatch.
[0033] The preparation method of the PET-based nano-ZnO antibacterial masterbatch described above, wherein the preparation process of the modified nano-ZnO particles is as follows:
[0034] First, the nano-ZnO particles are dispersed in a solvent (preferably ethanol) and ultrasonically treated for 10-30 minutes to break up particle agglomeration. Then, a surface modifier is added, and the mixture is stirred at 60°C for 6-12 hours to promote the chemical bonding between the surface modifier and the hydroxyl groups on the surface of the nano-ZnO particles. To further improve the coating uniformity and dispersion stability, a high-shear dispersion treatment can be performed for 1-2 hours during or after the above reaction using a nano-homogenizer or sand mill. Finally, the resulting slurry is centrifuged and washed twice with ethanol, followed by drying. The drying method is spray drying (inlet air temperature 120-150°C) or vacuum drying (80°C, 6 hours) to obtain modified nano-ZnO particles.
[0035] The preparation method of the PET-based nano-ZnO antibacterial masterbatch described above involves the following steps: Modified nano-ZnO particles and additives are mixed at 800-1200 rpm for 5-10 minutes at 60-80℃ to form a pre-dispersion. After cooling to room temperature, high-viscosity PET and low-viscosity PET are added and mixed at 400-800 rpm for 3-5 minutes to obtain the premix.
[0036] The preparation method of PET-based nano-ZnO antibacterial masterbatch described above involves melt blending using a twin-screw extruder with vacuum degassing. The temperatures of zones one to ten of the twin-screw extruder are 170℃, 265℃, 265℃, 255℃, 250℃, 250℃, 235℃, 235℃, 250℃, and 260℃, respectively, and the screw speed is 150-300 rpm. The process parameters for melt blending can be adjusted within a reasonable range.
[0037] This invention also provides an application of a PET-based nano-ZnO antibacterial masterbatch as described above. The PET-based nano-ZnO antibacterial masterbatch is dried with PET chips (the purpose is to control the moisture content to be below 30ppm, the means are not limited, for example, it can be dried at 140℃ for 10h), and then mixed, screw extrusion blended, spinneret extruded, cooled and shaped, wound, and subjected to secondary stretching deformation to obtain antibacterial DTY.
[0038] The PET chips have an intrinsic viscosity of 0.6-1.2 dL / g, a spinning temperature of 275-295℃, a winding speed of 2800-3300 m / min, a total secondary stretching ratio of 1.2-2.5 times, preferably 1.5-2.5 times, a modified nano-ZnO particle mass content of 0.2%-2% in DTY, preferably 0.5-1.5%, and a DTY specification of 75-1200D / 24-192F, preferably 75-1100D / 48-192F.
[0039] DTY has a mildew resistance rating of 0-2, with an inhibition rate of 90.00%-99.99% against Escherichia coli, 90.00%-99.99% against Staphylococcus aureus, and 85.00%-99.99% against Candida albicans.
[0040] Invention principle:
[0041] This invention achieves uniform dispersion of modified ZnO nanoparticles in a PET matrix by blending high-viscosity PET with low-viscosity PET. Low-viscosity PET, with its shorter molecular chains and lower melt viscosity, exhibits stronger fluidity and faster wetting of the filling medium surface, making it easier to penetrate the gaps between modified ZnO nanoparticle agglomerates and quickly coat and break up the agglomerates. Therefore, during the extrusion stage, the modified ZnO nanoparticles are more easily and rapidly wetted and agglomerated, resulting in a more uniform distribution. High-viscosity PET maintains a stable distribution of the modified ZnO nanoparticles within the blended system after dispersion, preventing localized enrichment or segregation.
[0042] This invention combines high-viscosity PET with low-viscosity PET to solve the problem of insufficient processing performance. Because the modified nano-ZnO particles are uniformly dispersed in the PET matrix, it can avoid the formation of local high-concentration areas of modified nano-ZnO particles ("hot spots" where chain breakage is accelerated), thereby reducing chain breakage and decreasing the viscosity drop of the compound system.
[0043] Even with a significant decrease in viscosity of low-viscosity PET, high-viscosity PET can maintain the viscosity of the blended system within a controllable range. This is partly because high-viscosity PET has a higher chain entanglement density, so even if some chain breakage occurs, the viscosity decrease is relatively gradual. Furthermore, the blended system contains both long chains (providing skeletal strength) and short chains (enhancing wetting and dispersion). From a polymer rheological perspective, systems with a wide molecular weight distribution respond more smoothly to molecular weight decreases than systems with a single molecular weight. Therefore, even if chain breakage continues, it is unlikely to cause an "instantaneous viscosity collapse," resulting in a significantly wider processing window and a more "resistant" production process.
[0044] In summary, the role of low-viscosity PET is to promote the rapid wetting and uniform dispersion of modified nano-ZnO particles in the melt, significantly reducing the risk of agglomeration. High-viscosity PET has two roles: one is to maintain the stable distribution of modified nano-ZnO particles in the compound system after dispersion, avoiding local enrichment or segregation; the other is to compensate for the viscosity loss of the compound system when the viscosity of low-viscosity PET drops significantly.
[0045] This invention controls the intrinsic viscosity of high-viscosity PET to be 0.80-1.20 dL / g, while simultaneously controlling the intrinsic viscosity of low-viscosity PET to be 0.40-0.55 dL / g. This is a prerequisite for ensuring that high-viscosity and low-viscosity PET can perform the aforementioned functions. This invention also controls the intrinsic viscosity difference between high-viscosity and low-viscosity PET to be 0.40-0.65 dL / g. If the intrinsic viscosity difference between high-viscosity and low-viscosity PET is too small, an effective viscosity gradient structure cannot be formed between the high-viscosity and low-viscosity PET, resulting in insufficient driving force for the migration of modified nano-ZnO particles in the melt and a decrease in dispersion uniformity. If the intrinsic viscosity difference between high-viscosity and low-viscosity PET is too large, the compensating effect of high-viscosity PET on the viscosity loss of the compound system is weakened, and the actual intrinsic viscosity retention rate of the masterbatch is significantly reduced.
[0046] This invention controls the mass ratio of high-viscosity PET to low-viscosity PET to be 30-70:70-30 to achieve a balance between processing fluidity and final viscosity support. If the proportion of high-viscosity PET is too low, the stable distribution of modified nano-ZnO particles in the compound system cannot be maintained, nor can the viscosity loss of the compound system be effectively compensated; conversely, if the proportion of high-viscosity PET is too high, the melt fluidity of the compound system is insufficient, and the dispersion of modified nano-ZnO particles is difficult.
[0047] This invention uses nano-ZnO particles treated with a surface modifier. During treatment, the amount of surface modifier used is more than 1% of the mass of the nano-ZnO particles. If the nano-ZnO particles are not modified or are insufficiently modified, they will have high surface energy and strong agglomeration, making it difficult for low-viscosity PET to completely wet and break up the agglomerates, resulting in local enrichment of nano-ZnO particles and exacerbating the breakage of PET molecular chains.
[0048] Beneficial effects:
[0049] (1) This invention simulates the dispersion behavior of modified nano ZnO particles in the melt using Monte Carlo simulation, which can screen and optimize the intrinsic viscosity and compounding ratio of high and low viscosity chips, providing guidance for the development of high content masterbatch, shortening the R&D cycle and improving product development efficiency.
[0050] (2) This invention combines high and low viscosity PET to take into account melt strength and fluidity, and solves the problem of large viscosity drop and poor spinnability after adding nano ZnO particles to a single PET matrix, so that the melt exhibits good stability in the spinning process of different specifications of fibers.
[0051] (3) In this invention, nano ZnO particles are fully dispersed through surface modification and twin-screw high shearing action. Even at a high concentration of 40wt%, they can still be uniformly distributed in the PET matrix, with no obvious agglomeration of particles, which significantly improves the functional effect of the material.
[0052] (4) The modified nano-ZnO particles in the masterbatch of the present invention can reach 10-40 wt%, and the modified nano-ZnO particles still maintain good dispersibility. The addition amount of masterbatch at 2-5 wt% can endow fibers and products with excellent antibacterial and antifungal functions. At the same time, since the masterbatch system maintains high melt viscosity and good processing stability, in addition to conventional short fibers and filaments, it can also be used for the production of PET industrial yarn with higher melt viscosity requirements, thus broadening the application range.
[0053] (5) This invention uses PET as the matrix, which avoids problems such as poor compatibility caused by using different matrix PBT, and avoids the thickening process. While maintaining the uniformity of fiber evenness and dyeing performance, it greatly reduces the production cost and is suitable for large-scale industrial applications. Attached Figure Description
[0054] Figure 1 This is a SEM image of the DTY obtained in Example 1 of the present invention;
[0055] Figure 2 This is a SEM image of the DTY obtained in Comparative Example 6 of the present invention;
[0056] Figure 3 This is a SEM image of the DTY obtained in Example 2 of the present invention;
[0057] Figure 4 This is a simulation diagram of the distribution of modified nano-ZnO particles in the masterbatch melt of Example 1 of the present invention;
[0058] Figure 5 This is a simulation diagram of the distribution of modified nano-ZnO particles in the melt of the masterbatch in Comparative Example 6 of this invention;
[0059] Figure 6 This is a simulation diagram of the distribution of modified nano-ZnO particles in the masterbatch melt of Example 2 of the present invention. Detailed Implementation
[0060] The present invention will be further described below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Furthermore, it should be understood that after reading the teachings of this invention, those skilled in the art can make various alterations or modifications to the invention, and these equivalent forms also fall within the scope defined by the appended claims.
[0061] The manufacturers and brands mentioned in the following embodiments are merely examples. The core of this invention lies in the technical solution itself, and it is not intended to limit specific manufacturers or brands. Products from other manufacturers and brands that meet the technical requirements and performance indicators specified in this invention can also meet the application requirements of this invention and are all feasible choices.
[0062] The test methods for the relevant performance indicators in the following embodiments and comparative examples are as follows:
[0063] Pressure filtration value: The PET-based nano-ZnO antibacterial masterbatches prepared in each example and comparative example were used as samples. The samples were then thoroughly mixed with PET substrate (Sanfangxiang bottle flakes, intrinsic viscosity 0.82 dL / g) at an effective mass fraction of 8% for the modified nano-ZnO particles, resulting in a total mixture mass of 1000g. The mixture was then extruded through a single-screw extruder using a 1400-mesh filter screen, and the extrusion pressure curve was recorded. The pressure filtration value was then calculated according to the formula... The filter press value (FPV, bar / g) was calculated; where P max P0 is the maximum pressure value (bar) of the pressure curve, and m is the initial pressure value (bar) of the curve. ZnO The mass (g) of the modified nano-ZnO particles in the mixture.
[0064] Intrinsic viscosity: The high-viscosity PET, low-viscosity PET and the prepared PET-based nano-ZnO antibacterial masterbatch in each example and comparative example were used as samples, and the intrinsic viscosity of the samples was tested in accordance with GBT 14190-2008 "Test Methods for Fiber Grade Polyester Chips (PET)".
[0065] Mildew resistance rating: The samples were tested for mildew resistance rating in accordance with GB / T 24346-2009 "Test of mildew resistance performance of textiles".
[0066] Inhibition rates against Escherichia coli, Staphylococcus aureus, and Candida albicans: The samples were tested for inhibition rates against Escherichia coli, Staphylococcus aureus, and Candida albicans in accordance with GB / T 20944.3-2008 "Evaluation of antimicrobial properties of textiles, Part 3: Vibration method".
[0067] Example 1
[0068] A method for preparing PET-based nano-ZnO antibacterial masterbatch, comprising the following steps:
[0069] (1) First, the nano-ZnO particles with an average particle size of 60 nm were dispersed in ethanol and ultrasonically dispersed for 30 min to break the agglomeration. Then, silane coupling agent KH550 (manufacturer: Evonik Industries AG, brand name: Dynasylan®AMEO) was added and reacted at 60 °C for 6 h. Then, the mixture was stirred at 60 °C for 1 h using a nano-homogenizer. After centrifugation, washing with ethanol twice, and drying, modified nano-ZnO particles were obtained. The amount of silane coupling agent KH550 was 1% of the mass of the nano-ZnO particles. The drying was carried out by vacuum drying (drying temperature: 80 °C, drying time: 6 h).
[0070] (2) At 70°C, the modified nano ZnO particles and the amphiphilic polyester wax (manufacturer: Lubrizol Corporation, USA, brand name: DP310) were mixed at 1200 rpm for 8 min to form a pre-dispersion. After cooling to 25°C, high-viscosity PET with an intrinsic viscosity of 1.0 dL / g and low-viscosity PET with an intrinsic viscosity of 0.45 dL / g were added and mixed at 800 rpm for 3 min to obtain the premix; wherein the mass ratio of high-viscosity PET to low-viscosity PET was 40:60.
[0071] (3) The premixed material was melt-blended using a twin-screw extruder and granulated under vacuum exhaust conditions to obtain PET-based nano ZnO antibacterial masterbatch; wherein the cooling water temperature during cooling and pelletizing was 40℃, the screw speed was 250rpm, and the vacuum degree during vacuum exhaust was -0.04MPa.
[0072] The final PET-based nano-ZnO antibacterial masterbatch includes a substrate, modified nano-ZnO particles dispersed therein, and amphiphilic polyester wax; the substrate is composed of high-viscosity PET and low-viscosity PET.
[0073] The PET-based nano-ZnO antibacterial masterbatch contains 20% modified nano-ZnO particles and 1% amphiphilic polyester wax.
[0074] The filtration pressure value of PET-based nano-ZnO antibacterial masterbatch is 0.08 bar / g; the actual intrinsic viscosity of PET-based nano-ZnO antibacterial masterbatch is 97% of the theoretical intrinsic viscosity. The theoretical intrinsic viscosity = mass percentage of high-viscosity PET in the substrate × intrinsic viscosity of high-viscosity PET + mass percentage of low-viscosity PET in the substrate × intrinsic viscosity of low-viscosity PET.
[0075] The application process of the PET-based nano-ZnO antibacterial masterbatch prepared above is as follows: the PET-based nano-ZnO antibacterial masterbatch and PET chips (intrinsic viscosity of 0.65 dL / g) are dried at 140℃ for 10 h, and then mixed, screw extruded and blended, spinneret extruded, cooled and shaped, wound, and subjected to secondary stretching deformation to obtain antibacterial DTY with specifications of 75D / 72F; wherein, the spinning temperature is 275℃, the winding speed is 3000 m / min, the total multiple of secondary stretching is 1.5 times, the mass content of modified nano-ZnO particles in DTY is 1%, and the mass ratio of PET-based nano-ZnO antibacterial masterbatch to PET chips is 5:95.
[0076] The final DTY had a mildew resistance level of 1, with an inhibition rate of 99.99% against Escherichia coli, 99.99% against Staphylococcus aureus, and 93% against Candida albicans.
[0077] Comparative Example 1
[0078] A method for preparing PET-based nano-ZnO antibacterial masterbatch is basically the same as in Example 1, except that the intrinsic viscosity of the high-viscosity PET used in step (2) is 0.80 dL / g.
[0079] The final PET-based nano-ZnO antibacterial masterbatch was basically the same as in Example 1, except that the filtration pressure value of the PET-based nano-ZnO antibacterial masterbatch was 0.60 bar / g.
[0080] The application of the PET-based nano-ZnO antibacterial masterbatch prepared above is basically the same as in Example 1, except that the PET-based nano-ZnO antibacterial masterbatch used is prepared in this comparative example.
[0081] The final DTY had a mildew resistance level of 3, an inhibition rate of 72% against Escherichia coli, an inhibition rate of 72% against Staphylococcus aureus, and an inhibition rate of 55% against Candida albicans.
[0082] Comparing Comparative Example 1 and Example 1, it can be seen that the PET-based nano-ZnO antibacterial masterbatch prepared in this comparative example is inferior to that of Example 1 in terms of dispersion uniformity and pressure filtration performance. The DTY prepared using it also shows a certain degree of decline in anti-mildew performance and antibacterial uniformity. This is because when the intrinsic viscosity difference between high and low viscosity PET is too small (less than 0.40 dL / g), an effective viscosity gradient structure cannot be formed between high and low viscosity PET. The migration driving force of modified nano-ZnO particles in the melt is insufficient, resulting in a decrease in dispersion uniformity and an increase in the pressure filtration value of the masterbatch. On this basis, the effective exposure of modified nano-ZnO particles in the fiber is insufficient, and functional blank areas with uneven distribution of antibacterial agent are formed on the fiber surface and near the surface layer. As a result, the final product has significantly deteriorated in terms of antibacterial uniformity and anti-mildew performance, and its overall performance is significantly lower than that of Example 1.
[0083] Comparative Example 2
[0084] A method for preparing PET-based nano-ZnO antibacterial masterbatch is basically the same as in Example 1, except that the intrinsic viscosity of the high-viscosity PET used in step (2) is 1.30 dL / g.
[0085] The final PET-based nano-ZnO antibacterial masterbatch was basically the same as in Example 1, except that the filtration pressure value of the PET-based nano-ZnO antibacterial masterbatch was 0.90 bar / g.
[0086] The application of the PET-based nano-ZnO antibacterial masterbatch prepared above is basically the same as in Example 1, except that the PET-based nano-ZnO antibacterial masterbatch used is prepared in this comparative example.
[0087] The final DTY had a mildew resistance level of 3, an inhibition rate of 70% against Escherichia coli, an inhibition rate of 70% against Staphylococcus aureus, and an inhibition rate of 65% against Candida albicans.
[0088] Comparing Comparative Example 2 with Example 1, it can be seen that the filtration pressure value of the PET-based nano-ZnO antibacterial masterbatch prepared in this comparative example is increased, and the anti-mildew grade and antibacterial rate of DTY prepared with it are reduced. This is because under the condition of excessively high intrinsic viscosity of high-viscosity PET, the melt viscosity of the system increases and the fluidity decreases, the dispersion efficiency of modified nano-ZnO particles decreases, resulting in an increase in filtration pressure value. Under this condition, although the modified nano-ZnO particles still exist in the fiber system, due to the deterioration of their dispersion state in the melt, it is difficult for them to migrate evenly and stably distribute on the fiber surface and near-surface during spinning and stretching, which limits the effective action area of the antibacterial active components, thereby weakening their inhibitory effect on microorganisms. Ultimately, this is reflected in the reduction of the antibacterial rate and anti-mildew grade of DTY compared to Example 1.
[0089] Comparative Example 3
[0090] A method for preparing PET-based nano-ZnO antibacterial masterbatch is basically the same as in Example 1, except that the mass ratio of high-viscosity PET to low-viscosity PET in step (2) is 25:75.
[0091] The final PET-based nano-ZnO antibacterial masterbatch was basically the same as in Example 1, except that: the filtration pressure value of the PET-based nano-ZnO antibacterial masterbatch was 0.60 bar / g; and the actual intrinsic viscosity of the PET-based nano-ZnO antibacterial masterbatch was 70% of the theoretical intrinsic viscosity.
[0092] The application of the PET-based nano-ZnO antibacterial masterbatch prepared above is basically the same as in Example 1, except that the PET-based nano-ZnO antibacterial masterbatch used is prepared in this comparative example.
[0093] The final DTY had a mildew resistance level of 2, an inhibition rate of 75% against Escherichia coli, an inhibition rate of 75% against Staphylococcus aureus, and an inhibition rate of 60% against Candida albicans.
[0094] Comparing Comparative Example 3 and Example 1, it can be seen that the PET-based nano-ZnO antibacterial masterbatch prepared in this comparative example has an increased filtration pressure value and a decreased actual intrinsic viscosity. The antifungal grade and antibacterial rate of DTY prepared with it are reduced. This is because the proportion of high-viscosity PET in this comparative example is insufficient, which cannot maintain the stable distribution of modified nano-ZnO particles in the compound system, nor can it effectively compensate for the viscosity loss of the compound system. This weakens the promoting effect of the viscosity gradient structure of the present invention on the dispersion of modified nano-ZnO particles, which in turn leads to an increase in the filtration pressure value and a decrease in the actual intrinsic viscosity of the antibacterial masterbatch. On this basis, the dispersibility of modified nano-ZnO particles deteriorates, thereby reducing the antibacterial rate and antifungal grade of DTY.
[0095] Comparative Example 4
[0096] A method for preparing PET-based nano-ZnO antibacterial masterbatch is basically the same as in Example 1, except that the mass ratio of high-viscosity PET to low-viscosity PET in step (2) is 80:20.
[0097] The final PET-based nano-ZnO antibacterial masterbatch was basically the same as in Example 1, except that the filtration pressure value of the PET-based nano-ZnO antibacterial masterbatch was 0.85 bar / g.
[0098] The application of the PET-based nano-ZnO antibacterial masterbatch prepared above is basically the same as in Example 1, except that the PET-based nano-ZnO antibacterial masterbatch used is prepared in this comparative example.
[0099] The final DTY had a mildew resistance level of 3, an inhibition rate of 70% against Escherichia coli, an inhibition rate of 65% against Staphylococcus aureus, and an inhibition rate of 55% against Candida albicans.
[0100] Comparing Comparative Example 4 and Example 1, it can be seen that the PET-based nano-ZnO antibacterial masterbatch prepared in this comparative example has an increased filtration pressure value, and the antifungal grade and antibacterial rate of the DTY prepared with it are reduced. This is because the high proportion of high-viscosity PET in this comparative example leads to insufficient melt flow of the compound system, weakening the dispersion efficiency of the modified nano-ZnO particles in the melt, and failing to achieve the viscosity gradient synergistic dispersion effect described in this invention, ultimately resulting in an increased filtration pressure value of the antibacterial masterbatch. In addition, due to the excessively high viscosity component during the masterbatch preparation process, the modified nano-ZnO particles have difficulty fully migrating in the melt and redistributing during the subsequent fiber forming process, resulting in insufficient effective coverage on the fiber surface and near-surface layer, limiting the effective area of the antibacterial active components, thereby weakening the effective contact between the modified nano-ZnO particles and microorganisms, ultimately reducing the antibacterial rate and antifungal grade of the prepared DTY.
[0101] Comparative Example 5
[0102] A method for preparing PET-based nano-ZnO antibacterial masterbatch is basically the same as in Example 1, except that the amount of surface modifier used in step (1) is 0.9% of the mass of the modified nano-ZnO particles.
[0103] The final PET-based nano-ZnO antibacterial masterbatch was basically the same as in Example 1, except that the filtration pressure value of the PET-based nano-ZnO antibacterial masterbatch was too high to be measured.
[0104] The application of the PET-based nano-ZnO antibacterial masterbatch prepared above is basically the same as in Example 1, except that the PET-based nano-ZnO antibacterial masterbatch used is prepared in this comparative example.
[0105] The final DTY had a mildew resistance level of 3, an inhibition rate of 65% against Escherichia coli, an inhibition rate of 65% against Staphylococcus aureus, and an inhibition rate of 40% against Candida albicans.
[0106] Comparing Comparative Example 5 with Example 1, it can be seen that the filtration pressure value of the PET-based nano-ZnO antibacterial masterbatch prepared in this comparative example is increased, and the anti-mildew grade and antibacterial rate of DTY prepared with it are reduced. This is because the amount of surface modifier used in this comparative example is small, the modification of nano-ZnO particles is insufficient, and the effective dispersion of modified nano-ZnO particles in the fiber is insufficient, resulting in an increase in the filtration pressure value of the antibacterial masterbatch, which in turn leads to a decrease in the antibacterial and anti-mildew properties of DTY prepared with it.
[0107] Comparative Example 6
[0108] A method for preparing PET-based nano-ZnO antibacterial masterbatch is basically the same as in Example 1, except that the high-viscosity PET and low-viscosity PET used in step (2) are replaced with equal mass of PET chips with a single intrinsic viscosity of 0.67 dL / g.
[0109] The final PET-based nano-ZnO antibacterial masterbatch was basically the same as in Example 1, except that: the filtration pressure value of the PET-based nano-ZnO antibacterial masterbatch was 1.05 bar / g; the actual intrinsic viscosity of the PET-based nano-ZnO antibacterial masterbatch was 0.38 dL / g, which was 56.72% of the theoretical intrinsic viscosity compared to the theoretical intrinsic viscosity (0.67 dL / g) in Example 1.
[0110] The application of the PET-based nano-ZnO antibacterial masterbatch prepared above is basically the same as in Example 1, except that the PET-based nano-ZnO antibacterial masterbatch used is prepared in this comparative example.
[0111] The final DTY had a mildew resistance level of 3, an inhibition rate of 50% against Escherichia coli, an inhibition rate of 55% against Staphylococcus aureus, and an inhibition rate of 40% against Candida albicans.
[0112] Comparing Comparative Example 6 and Example 1, it can be seen that the PET-based nano-ZnO antibacterial masterbatch prepared in this comparative example has an increased filtration pressure value and a decreased actual intrinsic viscosity. The anti-mildew grade and antibacterial rate of DTY prepared with it are reduced. This is because, without the formation of a high- and low-viscosity PET viscosity gradient structure, the migration and dispersion ability of modified nano-ZnO particles in the melt is significantly reduced, which increases the filtration pressure value and decreases the actual intrinsic viscosity of the prepared antibacterial masterbatch, thereby leading to a decrease in the anti-mildew grade and antibacterial rate of DTY prepared with it.
[0113] The SEM images of the DTYs obtained in Example 1 and Comparative Example 6 were compared, as follows: Figure 1 , Figure 2 As shown in the figure, the modified nano-ZnO particles in Example 1 have less agglomeration and are evenly distributed, achieving good coating and dispersion within the fiber cross-section; while in Comparative Example 6, the modified nano-ZnO particles show obvious agglomeration, with only sporadic distribution of modified nano-ZnO particles in some local areas within the fiber, indicating poor dispersibility and uneven distribution.
[0114] Example 2
[0115] A method for preparing PET-based nano-ZnO antibacterial masterbatch, comprising the following steps:
[0116] (1) First, the nano-ZnO particles with an average particle size of 60 nm were dispersed in ethanol and ultrasonically dispersed for 30 min to break the agglomeration. Then, silane coupling agent KH550 (manufacturer: Evonik Industries AG, brand name: Dynasylan®AMEO) was added and reacted at 60 °C for 8 h. Then, the mixture was stirred at 60 °C for 1.5 h using a nano-homogenizer. After centrifugation, washing with ethanol twice, and drying, modified nano-ZnO particles were obtained. The amount of silane coupling agent KH550 was 5% of the mass of the nano-ZnO particles. The drying was carried out by vacuum drying (drying temperature: 80 °C, drying time: 6 h).
[0117] (2) At 70°C, the modified nano ZnO particles and the amphiphilic polyester wax (manufacturer: Lubrizol Corporation, USA, brand name: DP310) were mixed at 1200 rpm for 8 min to form a pre-dispersion. After cooling to 25°C, high-viscosity PET with an intrinsic viscosity of 1.20 dL / g and low-viscosity PET with an intrinsic viscosity of 0.55 dL / g were added and mixed at 800 rpm for 5 min to obtain the premix; wherein the mass ratio of high-viscosity PET to low-viscosity PET was 60:40.
[0118] (3) The premixed material was melt-blended using a twin-screw extruder and granulated under vacuum exhaust conditions to obtain PET-based nano ZnO antibacterial masterbatch; wherein the cooling water temperature during cooling and pelletizing was 40℃, the screw speed was 150rpm, and the vacuum degree during vacuum exhaust was -0.04MPa.
[0119] The final PET-based nano-ZnO antibacterial masterbatch includes a substrate, modified nano-ZnO particles dispersed therein, and amphiphilic polyester wax; the substrate is composed of high-viscosity PET and low-viscosity PET.
[0120] The PET-based nano-ZnO antibacterial masterbatch contains 40% modified nano-ZnO particles and 1% amphiphilic polyester wax.
[0121] The filtration pressure value of PET-based nano-ZnO antibacterial masterbatch is 0.05 bar / g; the actual intrinsic viscosity of PET-based nano-ZnO antibacterial masterbatch is 108% of the theoretical intrinsic viscosity. The theoretical intrinsic viscosity = mass percentage of high-viscosity PET in the substrate × intrinsic viscosity of high-viscosity PET + mass percentage of low-viscosity PET in the substrate × intrinsic viscosity of low-viscosity PET.
[0122] The application process of the PET-based nano-ZnO antibacterial masterbatch prepared above is as follows: The PET-based nano-ZnO antibacterial masterbatch and PET chips (intrinsic viscosity 1.2 dL / g) are dried at 140℃ for 10 hours respectively, then sequentially mixed, extruded and blended using a screw extruder, extruded using a spinneret, cooled and shaped, wound, and subjected to secondary stretching deformation to obtain an antibacterial DTY with a density of 1100D / 192F (e.g., ...). Figure 3 As shown in the figure, the modified nano-ZnO particles can still be uniformly dispersed in the fiber prepared from the high-concentration masterbatch. The spinning temperature is 295℃, the winding speed is 3000m / min, the total multiple of secondary stretching is 2.5 times, the mass content of modified nano-ZnO particles in DTY is 1%, and the mass ratio of PET-based nano-ZnO antibacterial masterbatch to PET chips is 2.5:97.5.
[0123] The final DTY had a mold resistance rating of 0, an inhibition rate of 99.99% against Escherichia coli, 99.99% against Staphylococcus aureus, and 99.99% against Candida albicans.
[0124] Comparative Example 7
[0125] A method for preparing PET-based nano-ZnO antibacterial masterbatch is basically the same as in Example 2, except that the intrinsic viscosity of the low-viscosity PET used in step (2) is 0.60 dL / g.
[0126] The final PET-based nano-ZnO antibacterial masterbatch was basically the same as in Example 2, except that the filtration pressure value of the PET-based nano-ZnO antibacterial masterbatch was 0.50 bar / g.
[0127] The application of the PET-based nano-ZnO antibacterial masterbatch prepared above is basically the same as in Example 2, except that the PET-based nano-ZnO antibacterial masterbatch used is prepared in this comparative example.
[0128] The final DTY had a mildew resistance level of 2, an inhibition rate of 80% against Escherichia coli, an inhibition rate of 80% against Staphylococcus aureus, and an inhibition rate of 68% against Candida albicans.
[0129] Comparing Comparative Example 7 and Example 2, it can be seen that the filtration pressure value of the PET-based nano-ZnO antibacterial masterbatch prepared in this comparative example is increased, and the anti-mildew grade and antibacterial rate of DTY prepared with it are reduced. This is because the intrinsic viscosity of low-viscosity PET is too high, which leads to a significant decrease in the migration and dispersion ability of modified nano-ZnO particles in the melt, resulting in an increase in the filtration pressure value of the prepared antibacterial masterbatch, which in turn leads to a decrease in the anti-mildew grade and antibacterial rate of DTY prepared with it.
[0130] Example 3
[0131] A method for preparing PET-based nano-ZnO antibacterial masterbatch, comprising the following steps:
[0132] (1) First, the nano-ZnO particles with an average particle size of 30 nm were dispersed in ethanol and ultrasonically dispersed for 10 min to break the agglomeration. Then, dopamine (a surface modifier that uses dopamine as a precursor to form a polydopamine (PDA) coating layer by oxidation and self-polymerization under weakly alkaline conditions (adjusted to pH 8.5 by Tris buffer solution) was added and reacted at 60 °C for 10 h. Then, the mixture was stirred at 60 °C for 2 h using a nano-homogenizer. After centrifugation, washing with ethanol twice, and drying, modified nano-ZnO particles were obtained. The amount of dopamine was 10% of the mass of the nano-ZnO particles. The drying was done under vacuum (drying temperature was 80 °C, drying time was 6 h).
[0133] (2) At 80°C, the modified nano ZnO particles and fatty acid ester (manufacturer: Kao Corporation, Japan, brand name: EB-FF) were mixed at 800 rpm for 5 min to form a pre-dispersion. After cooling to 25°C, high-viscosity PET with an intrinsic viscosity of 0.8 dL / g and low-viscosity PET with an intrinsic viscosity of 0.40 dL / g were added and mixed at 400 rpm for 4 min to obtain the premix; wherein the mass ratio of high-viscosity PET to low-viscosity PET was 40:60.
[0134] (3) The premixed material was melt-blended using a twin-screw extruder and granulated under vacuum exhaust conditions to obtain PET-based nano ZnO antibacterial masterbatch; wherein the cooling water temperature during cooling and pelletizing was 40℃, the screw speed was 300rpm, and the vacuum degree during vacuum exhaust was -0.04MPa.
[0135] The final PET-based nano-ZnO antibacterial masterbatch includes a substrate, modified nano-ZnO particles dispersed therein, and fatty acid esters; the substrate is composed of high-viscosity PET and low-viscosity PET.
[0136] The modified nano-ZnO particles in the PET-based nano-ZnO antibacterial masterbatch contain 10% by mass, and the fatty acid ester content contains 0.5% by mass.
[0137] The filtration pressure value of PET-based nano-ZnO antibacterial masterbatch is 0.05 bar / g; the actual intrinsic viscosity of PET-based nano-ZnO antibacterial masterbatch is 95% of the theoretical intrinsic viscosity. The theoretical intrinsic viscosity = mass percentage of high-viscosity PET in the substrate × intrinsic viscosity of high-viscosity PET + mass percentage of low-viscosity PET in the substrate × intrinsic viscosity of low-viscosity PET.
[0138] The application process of the PET-based nano-ZnO antibacterial masterbatch prepared above is as follows: the PET-based nano-ZnO antibacterial masterbatch and PET chips (intrinsic viscosity of 0.65 dL / g) are dried at 140℃ for 10 h, and then mixed, extruded and blended by screw extrusion, extruded by spinneret, cooled and shaped, wound, and subjected to secondary stretching deformation to obtain antibacterial DTY with specifications of 150D / 48F; wherein, the spinning temperature is 275℃, the winding speed is 2800 m / min, the total multiple of secondary stretching is 1.5 times, the mass content of modified nano-ZnO particles in DTY is 0.5%, and the mass ratio of PET-based nano-ZnO antibacterial masterbatch to PET chips is 5:95.
[0139] The final DTY had a mildew resistance level of 2, an inhibition rate of 90% against Escherichia coli, an inhibition rate of 90% against Staphylococcus aureus, and an inhibition rate of 85% against Candida albicans.
[0140] Example 4
[0141] A method for preparing PET-based nano-ZnO antibacterial masterbatch, comprising the following steps:
[0142] (1) First, the nano-ZnO particles with an average particle size of 50 nm were dispersed in ethanol and ultrasonically dispersed for 20 min to break the agglomeration. Then, a carboxylated polymer (a polymer dispersant containing carboxyl functional groups, with a weight average molecular weight Mw of 10000 and an acid value of 120 mg KOH / g) was added and reacted at 60 °C for 8 h. Then, the mixture was stirred at 60 °C using a nano-homogenizer for 1.5 h. After centrifugation, washing with ethanol twice, and drying, modified nano-ZnO particles were obtained. The amount of carboxylated polymer was 3% of the mass of the nano-ZnO particles. The drying was done by spray drying (drying temperature of 120 °C and drying time of 1 h).
[0143] (2) At 60°C, the modified nano ZnO particles and polyethylene wax (manufacturer: Honeywell International, brand name: AC-6) were mixed at 1000 rpm for 10 min to form a pre-dispersion. After cooling to 25°C, high-viscosity PET with an intrinsic viscosity of 1.0 dL / g and low-viscosity PET with an intrinsic viscosity of 0.45 dL / g were added and mixed at 600 rpm for 5 min to obtain the premix; wherein the mass ratio of high-viscosity PET to low-viscosity PET was 30:70.
[0144] (3) The premixed material was melt-blended using a twin-screw extruder and granulated under vacuum exhaust conditions to obtain PET-based nano ZnO antibacterial masterbatch; wherein the cooling water temperature during cooling and pelletizing was 40℃, the screw speed was 200rpm, and the vacuum degree during vacuum exhaust was -0.04MPa.
[0145] The final PET-based nano-ZnO antibacterial masterbatch includes a substrate, modified nano-ZnO particles dispersed therein, and polyethylene wax; the substrate is composed of high-viscosity PET and low-viscosity PET.
[0146] The PET-based nano-ZnO antibacterial masterbatch contains 20% modified nano-ZnO particles and 2% polyethylene wax.
[0147] The filtration pressure value of PET-based nano-ZnO antibacterial masterbatch is 0.07 bar / g; the actual intrinsic viscosity of PET-based nano-ZnO antibacterial masterbatch is 85% of the theoretical intrinsic viscosity. The theoretical intrinsic viscosity = mass percentage of high-viscosity PET in the substrate × intrinsic viscosity of high-viscosity PET + mass percentage of low-viscosity PET in the substrate × intrinsic viscosity of low-viscosity PET.
[0148] The application process of the PET-based nano-ZnO antibacterial masterbatch prepared above is as follows: the PET-based nano-ZnO antibacterial masterbatch and PET chips (intrinsic viscosity of 0.8 dL / g) are dried at 140℃ for 10 h, and then mixed, extruded and blended by screw extrusion, extruded by spinneret, cooled and shaped, wound, and subjected to secondary stretching deformation to obtain antibacterial DTY with specifications of 300D / 96F; wherein, the spinning temperature is 280℃, the winding speed is 3000 m / min, the total multiple of secondary stretching is 2 times, the mass content of modified nano-ZnO particles in DTY is 1%, and the mass ratio of PET-based nano-ZnO antibacterial masterbatch to PET chips is 5:95.
[0149] The final DTY had a mildew resistance level of 1, with an inhibition rate of 99.99% against Escherichia coli, 99.99% against Staphylococcus aureus, and 92% against Candida albicans.
[0150] Example 5
[0151] A method for preparing PET-based nano-ZnO antibacterial masterbatch, comprising the following steps:
[0152] (1) First, the nano-ZnO particles with an average particle size of 70 nm were dispersed in ethanol and ultrasonically dispersed for 20 min to break the agglomeration. Then, a phosphate ester / stearic acid compound (a surface modifier system formed by compounding phosphate ester surfactant (manufacturer: Solvay Group, brand name: SOPROPHOR® 3D33) and zinc stearate (manufacturer: Changzhou Jinpulesi New Material Technology Co., Ltd., brand name: L-806) in a mass ratio of 1:1) was added. The mixture was reacted at 60 °C for 12 h, and then stirred at 60 °C using a nano-homogenizer for 1 h. After centrifugation, washing with ethanol twice, and drying, modified nano-ZnO particles were obtained. The amount of phosphate ester / stearic acid compound was 1% of the mass of the nano-ZnO particles. The drying was carried out by spray drying (drying temperature: 120 °C, drying time: 1 h).
[0153] (2) At 70°C, the modified nano ZnO particles and E-GMA-VA (manufacturer: Sumitomo Chemical Industries, Ltd., Japan, brand name: BF-2B) were mixed at 1000 rpm for 8 min to form a pre-dispersion. After cooling to 25°C, high-viscosity PET with an intrinsic viscosity of 1.0 dL / g and low-viscosity PET with an intrinsic viscosity of 0.45 dL / g were added and mixed at 600 rpm for 5 min to obtain the premix; wherein the mass ratio of high-viscosity PET to low-viscosity PET was 70:30.
[0154] (3) The premixed material was melt-blended using a twin-screw extruder and granulated under vacuum exhaust conditions to obtain PET-based nano ZnO antibacterial masterbatch; wherein the cooling water temperature during cooling and pelletizing was 40℃, the screw speed was 180rpm, and the vacuum degree during vacuum exhaust was -0.04MPa.
[0155] The final PET-based nano-ZnO antibacterial masterbatch includes a substrate, modified nano-ZnO particles dispersed therein, and E-GMA-VA; the substrate is composed of high-viscosity PET and low-viscosity PET.
[0156] The PET-based nano-ZnO antibacterial masterbatch contains 30% modified nano-ZnO particles and 1.2% E-GMA-VA.
[0157] The filtration pressure value of PET-based nano-ZnO antibacterial masterbatch is 0.1 bar / g; the actual intrinsic viscosity of PET-based nano-ZnO antibacterial masterbatch is 110% of the theoretical intrinsic viscosity. The theoretical intrinsic viscosity = mass percentage of high-viscosity PET in the substrate × intrinsic viscosity of high-viscosity PET + mass percentage of low-viscosity PET in the substrate × intrinsic viscosity of low-viscosity PET.
[0158] The application process of the PET-based nano-ZnO antibacterial masterbatch prepared above is as follows: the PET-based nano-ZnO antibacterial masterbatch and PET chips (intrinsic viscosity of 0.9 dL / g) are dried at 140℃ for 10 h, and then mixed, extruded and blended by screw extrusion, extruded by spinneret, cooled and shaped, wound, and subjected to secondary stretching deformation to obtain antibacterial DTY with specifications of 1100D / 192F; wherein, the spinning temperature is 295℃, the winding speed is 3300 m / min, the total multiple of secondary stretching is 2.5 times, the mass content of modified nano-ZnO particles in DTY is 1.5%, and the mass ratio of PET-based nano-ZnO antibacterial masterbatch to PET chips is 5:95.
[0159] The final DTY had a mold resistance rating of 0, an inhibition rate of 99.99% against Escherichia coli, an inhibition rate of 99.99% against Staphylococcus aureus, and an inhibition rate of 97% against Candida albicans.
[0160] The formulations of the PET-based nano-ZnO antibacterial masterbatches in Examples 1-5 were simulated using a two-dimensional single-site Larson bond length fluctuation model combined with the kinetic Monte Carlo method to simulate the dispersion behavior of modified nano-ZnO particles in the PET melt system. The simulation results were compared to obtain the formulation with the best dispersion uniformity of modified nano-ZnO particles. In actual processes, due to the screw combination design of the twin-screw extruder, the residence time of modified nano-ZnO particles in the shear block region is the longest, and the temperature setting in this region is relatively consistent. Therefore, the simulation mainly focuses on the flow and migration behavior of modified nano-ZnO particles in this region to simplify calculations and focus on key mechanisms.
[0161] During the simulation, each nano-ZnO particle is treated as a single particle, each particle occupies a lattice point, the allowed bond length square is 1 or 2, and each lattice point has 8 selectable motion sites; periodic boundary conditions are set in the X and Y directions (to simulate an infinite / continuous melt environment and avoid boundary enrichment or dilution effects caused by the finite simulation region) to eliminate finite boundary effects;
[0162] Considering the volume exclusion effect (any lattice point can only be occupied by one particle at a time) and prohibiting bond crossing behavior to conform to the physical constraints of polymer systems, the time unit is defined as the Monte Carlo step (MCs), which is the average time for each particle in the system to attempt to move once.
[0163] The migration probability of particles is jointly regulated by the local viscosity and temperature field of the system: when the temperature increases, the migration probability of particles increases; when the viscosity increases, the migration probability of particles decreases. This can intuitively reflect the influence of the system's processing conditions and raw material ratio on particle motion and dispersion state, as expressed below:
[0164] ;
[0165] In the formula, This represents the local viscosity at the location of the particle. Indicates local temperature. To set the temperature, The migration probability at the current position is represented by the value of the migration probability. By comparing the migration probability with the random number, it is determined whether the particle has migrated. If migration is successful, the particle coordinates and system properties are updated, and the aggregation situation is statistically analyzed before proceeding to the next simulation step. The next simulation step refers to the iterative process of calculating migration probabilities, determining random numbers, and updating the state of particles in the system after completing one particle migration determination and system state update. Through multiple iterations of the above steps, the particles gradually evolve in the constructed viscosity and temperature fields until the particle distribution in the system reaches a statistically stable state. The simulation results shown in the attached figure are a schematic representation of the spatial distribution of particles in the system after multiple Monte Carlo iterations, used to characterize the dispersion and aggregation behavior of modified nano-ZnO particles under different formulation conditions.
[0166] Pre-simulation parameter settings: System temperature (set according to the actual melting temperature during processing) was 533K; the calculation grid was 100×100, with a total of 10,000 grid points. This grid size referenced commonly used settings in existing literature on polymer / nanoparticle dispersion Monte Carlo simulations (two-dimensional grid, 10...). 4 (Grid size), used to control computational load while ensuring statistical representativeness; total number of attempts 1×10-1 6 -1×10 7 MCs, sampling interval 1000MCs, the same formula is independently repeated 30 times and the ensemble average is taken; the initial distribution will randomly and uniformly place particles, and some samples will be introduced with slight initial aggregation to evaluate the dispersing ability. This can avoid artificially introducing dispersion prior conditions and ensure that subsequent particle migration and dispersion behavior are completely dominated by model parameters.
[0167] The steps for calculating the corresponding number of grid points of modified nano-ZnO particles based on the mass fraction of modified nano-ZnO particles are as follows:
[0168] (a) First, calculate the volume fraction based on the mass fraction and density of the modified nano-ZnO particles and the density of the PET matrix. The calculation formula is as follows:
[0169]
[0170] In the formula, This indicates the mass fraction of modified nano-ZnO particles. This indicates the density of the modified nano-ZnO particles. Indicates the density of the PET matrix;
[0171] (b) Map volume fractions to grid points / occupancy;
[0172] In a two-dimensional lattice MC, the number of lattice points occupied by modified nano ZnO particles is equal to the volume fraction multiplied by the total number of lattice points, and the calculation formula is as follows: •Φ, where, Total grid points The number of lattice points represents the number of modified nano-ZnO particles.
[0173] The above simulation process considered volume exclusion effects and periodic boundary conditions to ensure the correspondence between the simulation results and the actual system. Simultaneously, through numerous independent simulations and ensemble averaging of the results, the dispersion trend of modified nano-ZnO particles under different blending ratios was obtained. Finally, the intrinsic viscosity and blending ratio of the high-viscosity PET and low-viscosity PET chips were selected, concluding that the formulation in Example 2 had the best uniformity of modified nano-ZnO particle dispersion (the distribution simulation of modified nano-ZnO particles in the masterbatch melt is as follows). Figure 6 As shown in the figure, the modified nano-ZnO particles still maintain good dispersion and migration ability in the high-content masterbatch system, indicating that the compound system has good dispersion stability. The DTY performance obtained by using it is also better than other embodiments, and the simulation results deviate little from the actual data.
[0174] The simulation results of the formulation in Example 1 were compared with those of the formulation in Comparative Example 6 (the simulation results of the distribution of modified nano-ZnO particles in the masterbatch melt were as follows). Figure 4 , Figure 5 As shown in the figure, in the high-viscosity PET and low-viscosity PET blend system, the particles are more evenly distributed near the interface, and the agglomeration rate (calculated by software, based on the size of modified nano-ZnO particles within the statistical region) decreases to 18%. This result is used to reflect the particle dispersion trend under different systems, rather than as an absolute quantitative result. In contrast, in the single-viscosity system (intrinsic viscosity of 0.67 dL / g), the local distribution of modified nano-ZnO particles varies greatly, and agglomeration is obvious, with a larger average agglomeration size. Therefore, in the high- and low-viscosity systems of Example 1, the modified nano-ZnO particles are uniformly dispersed in the polyester melt, while in the single-viscosity system of Comparative Example 6, the modified nano-ZnO particles are unevenly distributed, with local enrichment.
[0175] The above comparison shows that the high and low viscosity PET compound system can significantly inhibit the agglomeration of modified nano ZnO particles and achieve highly dispersed masterbatch. At the same time, the simulation method can reproduce the experimental results and provide a visual prediction for the formulation optimization before granulation.
Claims
1. A PET-based nano-ZnO antibacterial masterbatch, characterized in that, Including the substrate and the modified nano-ZnO particles dispersed therein; The substrate is composed of high-viscosity PET and low-viscosity PET; The intrinsic viscosity of high-viscosity PET is 0.80-1.20 dL / g, and the intrinsic viscosity of low-viscosity PET is 0.40-0.55 dL / g. The difference in intrinsic viscosity between high-viscosity PET and low-viscosity PET is 0.40-0.65 dL / g. The mass ratio of high-viscosity PET to low-viscosity PET is 30-70:70-30; Modified nano-ZnO particles are obtained by treating nano-ZnO particles with a surface modifier. During the treatment, the amount of surface modifier used is more than 1% of the mass of the nano-ZnO particles.
2. The PET-based nano-ZnO antibacterial masterbatch according to claim 1, characterized in that, During the treatment, the amount of surface modifier used is less than 10% of the mass of the nano ZnO particles.
3. The PET-based nano-ZnO antibacterial masterbatch according to claim 2, characterized in that, The surface modifier is one or more of the following: silane coupling agent, phosphate ester, stearic acid, carboxylated polymer and dopamine.
4. The PET-based nano-ZnO antibacterial masterbatch according to claim 1, characterized in that, The particle size of nano-ZnO particles is 20-80nm; in PET-based nano-ZnO antibacterial masterbatch, the mass content of modified nano-ZnO particles is 10%-40%.
5. The PET-based nano-ZnO antibacterial masterbatch according to claim 1, characterized in that, It also includes additives dispersed in the substrate; the additives are one or more of fatty acid esters, polyethylene wax, amphiphilic polyester wax, amide wax and E-GMA-VA; in PET-based nano ZnO antibacterial masterbatch, the mass content of the additives is 0.5%-2%.
6. A PET-based nano-ZnO antibacterial masterbatch according to any one of claims 1 to 5, characterized in that, The filter pressure value of PET-based nano-ZnO antibacterial masterbatch does not exceed 0.1 bar / g; the actual intrinsic viscosity of PET-based nano-ZnO antibacterial masterbatch is 85%-110% of the theoretical intrinsic viscosity. The theoretical intrinsic viscosity = mass percentage of high-viscosity PET in the substrate × intrinsic viscosity of high-viscosity PET + mass percentage of low-viscosity PET in the substrate × intrinsic viscosity of low-viscosity PET.
7. A method for preparing PET-based nano-ZnO antibacterial masterbatch, characterized in that, First, design multiple formulations for PET-based nano-ZnO antibacterial masterbatch, then use Monte Carlo simulation to screen out the formulation with the best dispersion uniformity of modified nano-ZnO particles, and then carry out production and processing according to the formulation. PET-based nano-ZnO antibacterial masterbatch includes a substrate and modified nano-ZnO particles dispersed therein; The substrate is composed of high-viscosity PET and low-viscosity PET; The intrinsic viscosity of high-viscosity PET is 0.80-1.20 dL / g, and the intrinsic viscosity of low-viscosity PET is 0.40-0.55 dL / g. The difference in intrinsic viscosity between high-viscosity PET and low-viscosity PET is 0.40-0.65 dL / g. The mass ratio of high-viscosity PET to low-viscosity PET is 30-70:70-30; Modified nano-ZnO particles are obtained by treating nano-ZnO particles with a surface modifier. During the treatment, the amount of surface modifier used is more than 1% of the mass of the nano-ZnO particles. The variables in the formulation are the intrinsic viscosity of high-viscosity PET, the intrinsic viscosity of low-viscosity PET, and the mass ratio of high-viscosity PET to low-viscosity PET.
8. The method for preparing a PET-based nano-ZnO antibacterial masterbatch according to claim 7, characterized in that, The production and processing process is as follows: after preparing modified nano-ZnO particles, they are mixed with high-viscosity PET, low-viscosity PET and additives to form a premix. The premix is then melt-blended and granulated to obtain PET-based nano-ZnO antibacterial masterbatch.
9. The application of a PET-based nano-ZnO antibacterial masterbatch as described in any one of claims 1 to 6, characterized in that, After drying PET-based nano-ZnO antibacterial masterbatch and PET chips, they are mixed, screw extruded and blended, spinneret extruded, cooled and shaped, wound and subjected to two-stage stretching deformation to obtain antibacterial DTY. The intrinsic viscosity of the PET chips is 0.6-1.2 dL / g, the spinning temperature is 275-295℃, the winding speed is 2800-3300m / min, the total multiple of secondary drawing is 1.2-2.5 times, the mass content of modified nano-ZnO particles in DTY is 0.2%-2%, and the specifications of DTY are 75-1200D / 24-192F. DTY has an anti-mildew rating of 0-2, an inhibition rate of 90%-99.99% against Escherichia coli, an inhibition rate of 90%-99.99% against Staphylococcus aureus, and an inhibition rate of 85%-99.99% against Candida albicans.
Citation Information
Patent Citations
Antibacterial resin composition derived from master batch, antibacterial fiber, antibacterial film, and method for producing antibacterial resin composition derived from master batch
CN102933654A
A composite antibacterial polyester masterbatch and its preparation method
CN109280345B