Production method of ultrafine activated heavy calcium carbonate for adhesives
By performing stepwise modification of heavy calcium carbonate and using silane coupling agents and porous silica-based nanocomposites, the problems of agglomeration and uneven dispersion of ultrafine heavy calcium carbonate in organic adhesives were solved, significantly improving the adhesive strength, compressive strength and water resistance of the adhesives, and realizing the production of high-performance adhesives.
Patent Information
- Application Number
- CN202611324121.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-17
AI Technical Summary
In the existing technology, ultrafine heavy calcium carbonate powder is prone to agglomeration, uneven dispersion, high oil absorption value and poor compatibility with resin in organic adhesive resin systems, resulting in limited improvement in the bonding strength and compressive strength of adhesives, making it difficult to meet the performance requirements of high-end structural adhesives and high-strength sealants.
By performing stepwise modification of heavy calcium carbonate, chemical grafting with silane coupling agent KH-550, inorganic dispersion, and molten stearic acid coating are used to form a stable organic-inorganic interface layer. Combined with porous silica-based nanocomposite materials, the interparticle connection and interfacial bonding are enhanced, forming a three-dimensional network structure and improving the mechanical properties of the adhesive.
It significantly improves the adhesive's bonding strength and compressive strength, prevents delamination and oil separation, extends shelf life, and enhances the adhesive layer's water resistance and toughness, as well as its stiffness and resistance to deformation.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of heavy calcium carbonate production technology, specifically a method for producing ultrafine activated heavy calcium carbonate for adhesives. Background Technology
[0002] Heavy calcium carbonate is a commonly used inorganic filler powder in the adhesive industry. It features good chemical stability, high whiteness, and excellent mechanical filling properties, effectively reducing adhesive production costs while improving adhesive layer hardness and bonding performance. However, ordinary ultrafine heavy calcium carbonate powder has a hydrophilic and oleophobic surface with numerous hydroxyl active sites. Directly filling it into organic adhesive resin systems can easily lead to problems such as powder agglomeration, uneven dispersion, excessively high oil absorption, and poor resin compatibility.
[0003] For example, Chinese patent CN109705795A discloses a two-component polyurethane adhesive and its preparation method. The modified heavy calcium carbonate used in this adhesive is heavy calcium carbonate with a surface coated with a polyoxyethylene-type nonionic surfactant and hydrophilic and oleophilic additives. This can improve the adhesion between the heavy calcium carbonate and the mixed polyol, prevent the oil in the polyurethane adhesive from penetrating into the interior of the fiberglass board, and improve the anti-permeation performance of the polyurethane adhesive on the magnesium oxide board. However, this method is only a physical coating. The surfactant is free in the adhesive layer, forming flexible defect sites and destroying the epoxy resin cross-linking network. This results in a slight increase in the tensile strength of the adhesive body. Although it can also play a certain reinforcing role as a carrier, the reinforcing ability is limited and cannot significantly improve the bonding strength and compressive strength of the adhesive. It is difficult to meet the high-performance requirements of high-end structural adhesives and high-strength sealants.
[0004] Therefore, developing a high-strength reinforced ultrafine active heavy calcium carbonate production method that can simultaneously improve the adhesive bonding and compression properties of adhesives is a technical problem that urgently needs to be solved in this field. Summary of the Invention
[0005] In view of the problems existing in the prior art, the purpose of this invention is to provide a method for producing ultrafine active heavy calcium carbonate for adhesives.
[0006] To achieve the above objectives, the present invention provides the following technical solution: The production method of ultrafine activated heavy calcium carbonate for adhesives specifically includes the following steps: 1) Select high-purity heavy calcium carbonate coarse material, crush and screen it, and pass it through a 100-mesh sieve to obtain heavy calcium carbonate fine material; 2) Mix the fine heavy calcium carbonate with deionized water to make a slurry, adjust the solid content of the slurry to 65-75%, add a dispersant, grind and then add water to dilute and adjust the mixture to obtain a heavy calcium carbonate slurry. 3) A stepwise modification process is adopted. The heavy calcium carbonate slurry is placed in a reactor. Under stirring, a silane coupling agent solution is sprayed into the slurry. After stirring, an inorganic dispersion is added. After stirring, preheated molten stearic acid is sprayed into the reactor. The amounts of the silane coupling agent solution, inorganic dispersion, and molten stearic acid are 1-2%, 2-5%, and 2.3-2.8% of the total mass of heavy calcium carbonate in the heavy calcium carbonate slurry, respectively. 4) The above slurry is fed into a low-temperature airflow drying device. After drying, it is dispersed and classified by airflow to obtain ultrafine active heavy calcium carbonate.
[0007] As a further preferred embodiment of the present invention, in step 1), the high-purity heavy calcium carbonate crude material is a high-purity calcite raw material with a dry basis calcium carbonate content ≥96%, Fe2O3≤0.02%, SiO2≤1%, MgO≤1%, Al2O3≤0.01%, and whiteness ≥96.2%; In step 2), the dispersant is a polyacrylate dispersant, and the amount added is 0.1-0.3% of the mass of the heavy calcium carbonate fines. In step 3), the heavy calcium carbonate slurry has a solid content of 15-18%, and the slurry powder particle size D50 is 3.5-4.5μm and D97≤10μm; In step 3), the temperature inside the reactor is 70-75℃, and the stirring speed is 800-1000 r / min; In step 3), the preheated molten stearic acid is preheated at a temperature of 75-78°C. In step 4), the drying equipment has an inlet air temperature controlled at 110-130℃ and an outlet air temperature of 60-80℃.
[0008] As a further preferred embodiment of the present invention, the silane coupling agent solution is obtained by adding 1.5-2.5 parts of silane coupling agent KH-550 to 7-10 parts of anhydrous ethanol and 0.8-1.2 parts of deionized water, and then stirring and hydrolyzing. The inorganic dispersion is obtained by dispersing 2-3 parts of fumed silica and 3-5 parts of porous silica-based nanocomposite material in 20-40 parts of an ethanol solution prepared by anhydrous ethanol and deionized water at a volume ratio of 95:5, and then dispersing them evenly in an ice-water bath. The molten stearic acid, by weight, is obtained by heating 2.5-3.5 parts of stearic acid in a sealed melting vessel to 70-75°C until completely melted.
[0009] As a further preferred embodiment of the present invention, the porous silica-based nanocomposite material is prepared by the following method: 1) Add porous silica to an ethanol solution, disperse it evenly, centrifuge it, dry it to constant weight, and then treat it with oxygen plasma for 3-4 minutes to obtain pretreated porous silica; 2) The rod-shaped composite nanomaterials were added to an ethanol solution and dispersed evenly in an ice-water bath to obtain a suspension; 3) Add the pretreated porous silica to the suspension at a solid-liquid ratio of 1g:(80-150)mL, stir thoroughly, and then transfer it to a vacuum impregnation tank. Maintain the vacuum at -0.07 to -0.09MPa for 30-50 minutes. After depressurizing to atmospheric pressure, continue stirring thoroughly. After centrifugation, dry to constant weight and treat in a nitrogen atmosphere for 2-3 hours. After treatment, allow it to cool naturally to room temperature.
[0010] Furthermore, in step 1), the porous silica has a particle size of 300-400 nm and a pore size of 50-60 nm; In step 1), the ethanol solution is prepared by mixing anhydrous ethanol and deionized water at a volume ratio of 95:5. In step 1), the ratio of porous silica to ethanol solution is (2-5) g: (400-900) mL; In step 2), the ratio of rod-shaped composite nanomaterials to ethanol solution in the suspension is (0.8-1.5) g : (350-500) mL; In step 3), the processing temperature is 220-230℃, and the heating rate is 1-2℃ / min.
[0011] As a further preferred embodiment of the present invention, the rod-shaped composite nanomaterial is prepared by the following method: 1) After ultrasonic cleaning and drying, the porous rod-shaped nanomaterials are treated with oxygen plasma for 3-4 minutes, then immersed in zinc acetate ethanol solution, dispersed evenly, centrifuged, dried, and heat-treated in air atmosphere for 1-2 hours, and then cooled naturally to obtain pretreated porous rod-shaped nanomaterials. 2) Add zinc nitrate hexahydrate and hexamethylenetetramine to deionized water in sequence, stir thoroughly at room temperature, and obtain the precursor growth solution after complete dissolution; 3) The pretreated porous rod-shaped nanomaterials are added to the precursor growth solution, and after thorough stirring and ultrasonic dispersion, they are transferred to a reaction vessel and reacted for 8-10 hours. 4) After the reaction is complete, the material is centrifuged, washed, dried, and treated under a nitrogen atmosphere for 2-3 hours. After treatment, it is naturally cooled to room temperature to obtain rod-shaped composite nanomaterials.
[0012] Furthermore, in step 1), the concentration of the zinc acetate ethanol solution is 0.005-0.01 mol / L; In step 1), the heat treatment is performed at a temperature of 350-360℃, with a heating rate of 3-5℃ / min. In step 2), the ratio of zinc nitrate hexahydrate, hexamethylenetetramine, and deionized water in the precursor growth solution is (2.2-4.0) g: (1.4-2.5) g: (300-500) mL.
[0013] Furthermore, in step 3), the solid-liquid ratio of the pretreated porous rod-shaped nanomaterial and the precursor growth solution is 1g:(30-50)mL; In step 3), the reaction is carried out at a temperature of 80-90℃, with a heating rate of 2-3℃ / min. In step 4), the processing temperature is 200-210℃, and the heating rate is 1-2℃ / min.
[0014] As a further preferred embodiment of the present invention, the porous rod-shaped nanomaterial is prepared by the following method: 1) Dissolve nickel nitrate hexahydrate in deionized water to obtain a nickel salt solution, and dissolve sodium oxalate and hexamethylenetetramine in deionized water to obtain a mixed solution; 2) Add the nickel salt solution to an equal volume of the mixture, stir continuously at room temperature for 4-6 hours, centrifuge after the reaction is complete, wash and dry the precipitate to obtain the micro-nano rod precursor; 3) Treat the micro-nano rod precursor under a nitrogen atmosphere for 4-6 hours. After the treatment is completed, allow it to cool naturally to room temperature to obtain porous rod-shaped nanomaterials.
[0015] Furthermore, in step 1), the ratio of nickel nitrate hexahydrate to deionized water in the nickel salt solution is (2-5) g: (250-350) mL; In step 1), the ratio of sodium oxalate, hexamethylenetetramine, and deionized water in the mixture is (1.3-2.5) g : (1.4-2.8) g : (250-350) mL; In step 2), the stirring reaction is carried out at a speed of 400-500 r / min; In step 3), the processing temperature is 350-380℃, and the heating rate is 1-3℃ / min.
[0016] Compared with the prior art, the beneficial effects of the present invention are: In this invention, heavy calcium carbonate is activated and modified, then chemically grafted with an inner layer of silane coupling agent KH-550, fixed with an intermediate layer of inorganic filler, and hydrophobically coated with an outer layer of stearic acid. This chemical grafting reduces the hydrophilic hydroxyl groups on the surface of ultrafine calcium carbonate particles, making the powder less prone to agglomeration in organic adhesive matrices such as epoxy resin, polyurethane, MS glue, and butyl glue. Simultaneously, one end of the KH550 aminosilane condenses and grafts with the hydroxyl groups on the calcium carbonate surface, while the other end's amino group can chemically react with epoxy groups, isocyanate groups, and siloxane groups in the adhesive resin, forming a stable organic-inorganic interface layer. This avoids interfacial voids between the filler and the resin, improving the overall bonding system. In terms of bulk mechanical properties, the fumed silica in the middle layer, rich in silanol groups on its surface, forms a three-dimensional silica network structure with particles linked by hydrogen bonds. This network thickens the adhesive, prevents sagging, and prevents collapse. Furthermore, the silanol groups on the surface of the fumed silica can form strong interactions with polymer molecular chains, such as hydrogen bonds or van der Waals forces, resulting in a tight bond and reinforcing effect, further improving the mechanical properties of the adhesive. Additionally, the uniformly coated stearic acid on the outer layer forms a hydrophobic barrier, reducing the adsorption and locking of plasticizers and low-molecular-weight additives by calcium carbonate particles, inhibiting plasticizer migration and precipitation, making the adhesive less prone to separation and oil separation during storage, and extending the product's shelf life.
[0017] Meanwhile, to further enhance the effect of heavy calcium carbonate in adhesives and improve their mechanical properties, this invention synthesizes micro / nanor rod precursors via room-temperature precipitation and obtains porous rod-shaped nanomaterials through calcination in a nitrogen atmosphere. The porous rod-shaped nanomaterials are then cleaned to remove air bubbles and create active nucleation sites, ensuring the zinc source precursor fully penetrates the pores. Oxygen plasma treatment increases the surface hydroxyl content, which is beneficial for the adhesion of subsequent nanowires. After preparing a ZnO seed layer on its surface, it is immersed in a zinc source precursor growth solution, and stirring allows for the absorption of zinc ions. Initial adsorption is performed, followed by ultrasonic cavitation to forcefully expel residual trace amounts of air from the pores. This drives the zinc source ions to fully wet and fill the entire porous channel, achieving saturated adsorption within the pores. This ensures that subsequent ZnO nanowire growth begins inside the pores and extends to the outside. Subsequent isothermal treatment ensures the nanowires are firmly bonded, resulting in a structurally stable rod-shaped composite nanomaterial. Then, using porous silica as a carrier, vacuum impregnation allows the rod-shaped composite nanomaterial to infiltrate the carrier, forming a framework support structure within it. This yields a porous silica-based nanocomposite material, which, along with fumed silica, serves as an inorganic filler. The porous silica-based nanocomposite material contains numerous outward-extending ZnO nanowires that can embed into the adhesive layer. During adhesive curing, the polymer resin chains entwine and wrap around the nanowire surface, forming a dual interface of physical interlocking and chemical interaction, greatly enhancing the interfacial bonding strength and thus significantly improving the adhesive strength. Furthermore, when microcracks generated in the adhesive layer under external force propagate, the nanowires can act as a bridge on the crack surface, bridging both sides of the crack, consuming more fracture energy, and preventing rapid crack propagation. Moreover, the rod-shaped composite nanowires embedded within the porous silica-based nanocomposite material further contribute to this effect. The material itself has a mesoporous structure that can accommodate minute deformations and buffer interfacial stress, thereby achieving a toughening effect and improving the toughness of the adhesive. Moreover, the porous silica-based nanocomposite material fixed on the surface of calcium carbonate is uniformly dispersed inside the adhesive. It can not only form a large number of discontinuous inorganic barrier phases, preventing water vapor from penetrating the inorganic particles in a straight line, thus significantly lengthening the penetration path and reducing the water vapor diffusion rate, but also the composite material itself has a high specific surface area and strong adsorption capacity. It can also actively adsorb and lock those trace water molecules or small volatile molecules that may have already penetrated in, confining them in the pores, thereby significantly improving the water resistance of the adhesive layer. Meanwhile, the skeletal support structure formed inside the porous silica-based nanocomposite material can effectively enhance the stiffness of the composite material, just like miniature steel bars, and improve its ability to withstand compressive loads. When the adhesive layer as a whole is subjected to compressive force, the pressure can be efficiently transferred from the softer polymer matrix to the hard porous silica-based nanocomposite material through the interface. Since the stiffness of the porous silica-based nanocomposite material is much higher than that of the polymer, it can withstand most of the compressive load, improve the adhesive layer's resistance to deformation, and thus enhance the compressive strength of the adhesive layer. This allows the adhesive to achieve both high adhesive strength and high compressive strength. Detailed Implementation
[0018] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0019] In this embodiment of the invention, the heavy calcium carbonate crude material is a high-purity calcite raw material with a dry basis calcium carbonate content of 96%, Fe2O3 0.02%, SiO2 1%, MgO 1%, Al2O3 0.01%, and whiteness of 96.2%. The dispersant is sodium polyacrylate, and the amount added is 0.1% of the mass of the heavy calcium carbonate fines. Heavy calcium carbonate slurry, with a particle size D50 of 3.5-4.5μm and D97≤10μm.
[0020] In this embodiment of the invention, the ethanol solution is prepared by mixing anhydrous ethanol and deionized water at a volume ratio of 95:5; Porous silica with a particle size of 300-400 nm and a pore size of 50-60 nm.
[0021] Example 1 The production method of ultrafine activated heavy calcium carbonate for adhesives specifically includes the following steps: S1 Raw Material Pretreatment: Select high-purity heavy calcium carbonate coarse material, crush and screen it through a 100-mesh sieve to obtain heavy calcium carbonate fine material; S2 wet ultrafine grinding: Heavy calcium carbonate fines are mixed with deionized water to make a slurry, the solid content of the slurry is adjusted to 65%, a dispersant is added, and after grinding, water is added to dilute and adjust the slurry to obtain a heavy calcium carbonate slurry with a solid content of 15%. S3 composite modification: S3-1) According to the weight parts, add 1.5 parts of silane coupling agent KH-550, 7 parts of anhydrous ethanol and 0.8 parts of deionized water, stir and hydrolyze at room temperature for 15 minutes to obtain silane coupling agent solution. S3-2) Disperse 2 parts of fumed silica and 3 parts of porous silica-based nanocomposite material in 20 parts of ethanol solution, and ultrasonically disperse in an ice-water bath at 100W for 10 min to obtain an inorganic dispersion. S3-3) 2.5 parts of stearic acid were placed in a sealed melting vessel and heated to 70°C until completely melted to obtain molten stearic acid. Then, heavy calcium carbonate slurry was placed in a reaction vessel, and the system was kept at a constant temperature of 70°C. The stirring speed was set to 800 r / min. Silane coupling agent solution was sprayed into the slurry by atomization, and the mixture was stirred at a constant temperature for 50 min to complete the silane grafting reaction. Then, inorganic dispersion was slowly added, and the mixture was stirred at a constant temperature for 40 min to fix the fumed silica and porous silica-based nanocomposite material on the surface of heavy calcium carbonate. Finally, molten stearic acid preheated to 75°C was sprayed into the system by atomization, and the mixture was stirred for 50 min to form a coating layer on the surface of heavy calcium carbonate. The amount of silane coupling agent solution used is 1% of the total mass of heavy calcium carbonate in the heavy calcium carbonate slurry; The amount of inorganic dispersion is 2% of the total mass of heavy calcium carbonate in the heavy calcium carbonate slurry; The amount of molten stearic acid used is 2.3% of the total mass of heavy calcium carbonate in the heavy calcium carbonate slurry; S4 Low-Temperature Drying Refining: The above slurry is fed into a low-temperature airflow drying device, with the inlet air temperature controlled at 110℃ and the outlet air temperature at 60℃. After drying, it is cooled to room temperature, sealed and packaged to obtain the finished product of ultrafine active heavy calcium carbonate for adhesives.
[0022] The preparation method of porous silica-based nanocomposite materials is as follows: 1) Dissolve 2g of nickel nitrate hexahydrate in 250mL of deionized water to obtain a nickel salt solution. Dissolve 1.3g of sodium oxalate and 1.4g of hexamethylenetetramine in 250mL of deionized water to obtain a mixed solution. Add the nickel salt solution to an equal volume of the mixed solution. Stir the mixture at 400r / min at room temperature for 4 hours. After the reaction is complete, centrifuge the product and wash it with anhydrous ethanol and deionized water alternately 5 times. Then dry it to constant weight to obtain a micro-nano rod precursor. Then heat the micro-nano rod precursor to 350℃ at a rate of 1℃ / min under a nitrogen atmosphere and keep it at that temperature for 4 hours. After the treatment is complete, cool it to room temperature naturally to obtain porous rod-shaped nanomaterials. 2) The porous rod-shaped nanomaterials were added to deionized water and ultrasonically cleaned for 10 min at 100 W. Then, the ultrasonic cleaning was continued for 10 min with anhydrous ethanol. The cleaned powder was dried in an oven at 60 °C for 6 h. After being treated with oxygen plasma for 3 min, it was immersed in a 0.005 mol / L zinc acetate ethanol solution and ultrasonically dispersed for 10 min at 200 W. After centrifugation, it was dried at 70 °C and then heat-treated at 3 °C / min to 350 °C in air atmosphere for 1 h. After natural cooling, the pretreated porous rod-shaped nanomaterials were obtained. 2.2 g of zinc nitrate hexahydrate and 1.4 g of hexamethylenetetramine were added to 300 mL of deionized water. The mixture was magnetically stirred at room temperature for 30 min at a stirring speed of 400 r / min. After complete dissolution, the precursor growth solution was obtained. 3) The pretreated porous rod-shaped nanomaterials were added to the precursor growth solution at a solid-liquid ratio of 1g:30mL. After mechanical stirring at 200r / min for 20min, the mixture was ultrasonically treated at 200W for 20min. Then, it was transferred to a reaction vessel and heated to 80℃ at a rate of 2℃ / min. The reaction was kept at this temperature for 8h. After the reaction was completed, the mixture was centrifuged and washed 5 times alternately with anhydrous ethanol and deionized water. After drying to constant weight, the mixture was heated to 200℃ at a rate of 1℃ / min under a nitrogen atmosphere and kept at this temperature for 2h. After the treatment was completed, the mixture was naturally cooled to room temperature to obtain the rod-shaped composite nanomaterials. 4) Add 2g of porous silica to 400mL of ethanol solution, sonicate at 100W for 20min at room temperature, centrifuge, dry at 60℃ for 6h, and then treat with oxygen plasma for 3min to obtain pretreated porous silica. Add 0.8g of rod-shaped composite nanomaterials to 350mL of ethanol solution, sonicate at 100W for 20min in an ice-water bath, and then stir at 100r / min for 10min to obtain a suspension. Then, according to a solid-liquid ratio of 1g:8... 0 mL of pretreated porous silica was added to the suspension. After stirring at 200 r / min for 10 min, the mixture was transferred to a vacuum impregnation tank and maintained under a vacuum of -0.07 MPa for 30 min. After slowly depressurizing to atmospheric pressure, stirring was continued for 2 h. After centrifugation, the mixture was dried to constant weight and heated to 220 °C at a rate of 1 °C / min in a nitrogen atmosphere. The temperature was maintained for 2 h. After the treatment was completed, the mixture was allowed to cool naturally to room temperature to obtain the desired porous silica-based nanocomposite material.
[0023] Example 2 The production method of ultrafine activated heavy calcium carbonate for adhesives specifically includes the following steps: S1 Raw Material Pretreatment: Select high-purity heavy calcium carbonate coarse material, crush and screen it through a 100-mesh sieve to obtain heavy calcium carbonate fine material; S2 wet ultrafine grinding: Heavy calcium carbonate fines are mixed with deionized water to make a slurry, the solid content of the slurry is adjusted to 70%, a dispersant is added, and after grinding, water is added to dilute and adjust the slurry to obtain a heavy calcium carbonate slurry with a solid content of 16%. S3 composite modification: S3-1) According to the weight parts, add 2 parts of silane coupling agent KH-550, 8 parts of anhydrous ethanol and 0.9 parts of deionized water, stir and hydrolyze at room temperature for 16 minutes to obtain silane coupling agent solution. S3-2) 2.5 parts of fumed silica and 4 parts of porous silica-based nanocomposite material were dispersed in 30 parts of ethanol solution and ultrasonically dispersed in an ice-water bath at 150W for 12 min to obtain an inorganic dispersion. S3-3) Three parts of stearic acid were placed in a sealed melting vessel and heated to 72°C until completely melted to obtain molten stearic acid. Then, heavy calcium carbonate slurry was placed in a reaction vessel, and the system temperature was maintained at 72°C. The stirring speed was set to 900 r / min. Silane coupling agent solution was uniformly atomized and sprayed into the slurry. The mixture was stirred at a constant temperature for 55 min to complete the silane grafting reaction. Then, inorganic dispersion was slowly added, and the mixture was stirred at a constant temperature for 45 min to fix fumed silica and porous silica-based nanocomposite materials on the surface of heavy calcium carbonate. Finally, molten stearic acid preheated to 76°C was uniformly atomized and sprayed into the system. The mixture was stirred for 55 min to form a coating layer on the surface of heavy calcium carbonate. The amount of silane coupling agent solution used is 1.5% of the total mass of heavy calcium carbonate in the heavy calcium carbonate slurry; The amount of inorganic dispersion is 3% of the total mass of heavy calcium carbonate in the heavy calcium carbonate slurry; The amount of molten stearic acid used is 2.5% of the total mass of heavy calcium carbonate in the heavy calcium carbonate slurry; S4 Low-Temperature Drying Refining: The above slurry is fed into a low-temperature airflow drying device, with the inlet air temperature controlled at 120℃ and the outlet air temperature at 70℃. After drying, it is cooled to room temperature, sealed and packaged to obtain the finished product of ultrafine active heavy calcium carbonate for adhesives.
[0024] The preparation method of porous silica-based nanocomposites is as follows: 1) Dissolve 3g of nickel nitrate hexahydrate in 300mL of deionized water to obtain a nickel salt solution. Then dissolve 2.1g of sodium oxalate and 2.3g of hexamethylenetetramine in 300mL of deionized water to obtain a mixed solution. Slowly add the nickel salt solution to an equal volume of the mixed solution. At room temperature, stir continuously at 450r / min for 5 hours. After the reaction is completed, centrifuge and separate the precipitate. Wash the precipitate with anhydrous ethanol and deionized water alternately 5 times and dry it to constant weight to obtain a micro-nano rod precursor. Then heat the micro-nano rod precursor to 360℃ at a rate of 2℃ / min under a nitrogen atmosphere and keep it at that temperature for 5 hours. After the treatment is completed, cool it naturally to room temperature to obtain porous rod-shaped nanomaterials. 2) The porous rod-shaped nanomaterials were added to deionized water and ultrasonically cleaned for 12 min at 150 W. Then, the ultrasonic cleaning was continued for 12 min with anhydrous ethanol. The cleaned powder was dried in an oven at 65 °C for 7 h. After being treated with oxygen plasma for 4 min, it was immersed in a 0.008 mol / L zinc acetate ethanol solution and ultrasonically dispersed for 10 min at 250 W. After centrifugation, it was dried at 75 °C and placed in a tube furnace. Under an air atmosphere, the temperature was increased to 355 °C at 4 °C / min and kept constant for 1.5 h. After natural cooling, the pretreated porous rod-shaped nanomaterials were obtained. 3 g of zinc nitrate hexahydrate and 1.9 g of hexamethylenetetramine were added to 400 mL of deionized water. The mixture was magnetically stirred at room temperature for 40 min at a stirring speed of 450 r / min. After complete dissolution, the precursor growth solution was obtained. 3) The pretreated porous rod-shaped nanomaterials were added to the precursor growth solution at a solid-liquid ratio of 1g:40mL. After mechanical stirring at 250r / min for 25min, the mixture was ultrasonically treated at 250W for 25min. Then, it was transferred to a reaction vessel and heated to 85℃ at a rate of 3℃ / min. The reaction was kept at this temperature for 9h. After the reaction was completed, the mixture was centrifuged and washed 5 times alternately with anhydrous ethanol and deionized water. After drying to constant weight, the mixture was heated to 205℃ at a rate of 2℃ / min under a nitrogen atmosphere and kept at this temperature for 2.5h. After the treatment was completed, the mixture was naturally cooled to room temperature to obtain the rod-shaped composite nanomaterials. 4) Add 3g of porous silica to 500mL of ethanol solution, sonicate at 150W for 25min at room temperature, centrifuge, dry at 65℃ for 7h, and then treat with oxygen plasma for 4min to obtain pretreated porous silica. Add 1.2g of rod-shaped composite nanomaterials to 400mL of ethanol solution, sonicate at 150W for 25min in an ice-water bath, and then stir at 150r / min for 15min to obtain a suspension. Then, according to a solid-liquid ratio of 1g:120m L. Pretreated porous silica was added to the suspension and stirred at 250 r / min for 15 min. Then, it was transferred to a vacuum impregnation tank and maintained under a vacuum of -0.08 MPa for 40 min. After slowly depressurizing to atmospheric pressure, stirring was continued for 2.5 h. After centrifugation, it was dried to constant weight and heated to 225 °C at a rate of 2 °C / min in a nitrogen atmosphere. The temperature was kept constant for 2.5 h. After the treatment was completed, it was naturally cooled to room temperature to obtain the desired porous silica-based nanocomposite material.
[0025] Example 3 The production method of ultrafine activated heavy calcium carbonate for adhesives specifically includes the following steps: S1 Raw Material Pretreatment: Select high-purity heavy calcium carbonate coarse material, crush and screen it through a 100-mesh sieve to obtain heavy calcium carbonate fine material; S2 wet ultrafine grinding: Heavy calcium carbonate fines are mixed with deionized water to make a slurry, the solid content of the slurry is adjusted to 75%, a dispersant is added, and after grinding, water is added to dilute and adjust the slurry to obtain a heavy calcium carbonate slurry with a solid content of 18%. S3 composite modification: S3-1) According to the weight parts, add 2.5 parts of silane coupling agent KH-550, 10 parts of anhydrous ethanol and 1.2 parts of deionized water, stir and hydrolyze at room temperature for 20 minutes to obtain silane coupling agent solution. S3-2) Disperse 3 parts of fumed silica and 5 parts of porous silica-based nanocomposite material in 40 parts of ethanol solution, and ultrasonically disperse in an ice-water bath at 200W for 15 min to obtain an inorganic dispersion. S3-3) 3.5 parts of stearic acid were placed in a sealed melting vessel and heated to 75°C until completely melted to obtain molten stearic acid. Then, heavy calcium carbonate slurry was placed in a reaction vessel, and the system was kept at a constant temperature of 75°C. The stirring speed was set to 1000 r / min. Silane coupling agent solution was uniformly atomized and sprayed into the slurry. The mixture was stirred at a constant temperature for 60 min to complete the silane grafting reaction. Then, inorganic dispersion was slowly added, and the mixture was stirred at a constant temperature for 50 min to fix the fumed silica and porous silica-based nanocomposite material on the surface of heavy calcium carbonate. Finally, molten stearic acid preheated to 78°C was uniformly atomized and sprayed into the system. The mixture was stirred for 60 min to form a coating layer on the surface of heavy calcium carbonate. The amount of silane coupling agent solution used is 2% of the total mass of heavy calcium carbonate in the heavy calcium carbonate slurry; The amount of inorganic dispersion is 5% of the total mass of heavy calcium carbonate in the heavy calcium carbonate slurry; The amount of molten stearic acid used is 2.8% of the total mass of heavy calcium carbonate in the heavy calcium carbonate slurry; S4 Low-Temperature Drying Refining: The above slurry is fed into a low-temperature airflow drying device, with the inlet air temperature controlled at 130℃ and the outlet air temperature at 80℃. After drying, it is cooled to room temperature, sealed and packaged to obtain the finished product of ultrafine active heavy calcium carbonate for adhesives.
[0026] The preparation method of porous silica-based nanocomposites is as follows: 1) Dissolve 5g of nickel nitrate hexahydrate in 350mL of deionized water to obtain a nickel salt solution. Then dissolve 2.5g of sodium oxalate and 2.8g of hexamethylenetetramine in 350mL of deionized water to obtain a mixed solution. Slowly add the nickel salt solution to an equal volume of the mixed solution. At room temperature, stir continuously at 500r / min for 6h. After the reaction is completed, centrifuge and separate the precipitate. Wash the precipitate with anhydrous ethanol and deionized water alternately 5 times and dry it to constant weight to obtain a micro-nano rod precursor. Then heat the micro-nano rod precursor to 380℃ at a rate of 3℃ / min under a nitrogen atmosphere and keep it at that temperature for 6h. After the treatment is completed, cool it naturally to room temperature to obtain porous rod-shaped nanomaterials. 2) The porous rod-shaped nanomaterials were added to deionized water and ultrasonically cleaned for 15 min at 200 W. Then, the ultrasonic cleaning was continued for 15 min with anhydrous ethanol. The cleaned powder was dried in an oven at 70 °C for 8 h. After being treated with oxygen plasma for 4 min, it was immersed in a 0.01 mol / L zinc acetate ethanol solution and ultrasonically dispersed at 300 W for 15 min. After centrifugation, it was dried at 80 °C and placed in a tube furnace. Under an air atmosphere, the temperature was increased to 360 °C at 5 °C / min and kept constant for 2 h. After natural cooling, the pretreated porous rod-shaped nanomaterials were obtained. 4.0 g of zinc nitrate hexahydrate and 2.5 g of hexamethylenetetramine were added to 500 mL of deionized water. The mixture was magnetically stirred at 500 r / min at room temperature for 50 min. After complete dissolution, the precursor growth solution was obtained. 3) The pretreated porous rod-shaped nanomaterials were added to the precursor growth solution at a solid-liquid ratio of 1g:50mL. After mechanical stirring at 300r / min for 30min, the mixture was ultrasonically treated at 300W for 30min. Then, it was transferred to a reaction vessel and heated to 90℃ at a rate of 3℃ / min. The reaction was kept at this temperature for 10h. After the reaction was completed, the mixture was centrifuged and washed 5 times alternately with anhydrous ethanol and deionized water. After drying to constant weight, the mixture was heated to 210℃ at a rate of 2℃ / min under a nitrogen atmosphere and kept at this temperature for 3h. After the treatment was completed, the mixture was naturally cooled to room temperature to obtain the rod-shaped composite nanomaterials. 4) Add 5g of porous silica to 900mL of ethanol solution, sonicate at 200W for 30min at room temperature, centrifuge, dry at 70℃ for 8h, and then treat with oxygen plasma for 4min to obtain pretreated porous silica. Add 1.5g of rod-shaped composite nanomaterials to 500mL of ethanol solution, sonicate at 200W for 30min in an ice-water bath, and then stir at 200r / min for 20min to obtain a suspension. Then, according to a solid-liquid ratio of 1g:15... 0 mL of pretreated porous silica was added to the suspension and stirred at 300 r / min for 20 min. The mixture was then transferred to a vacuum impregnation tank and maintained under a vacuum of -0.09 MPa for 50 min. After slowly depressurizing to atmospheric pressure, stirring was continued for 3 h. After centrifugation, the mixture was dried to constant weight and heated to 230 °C at a rate of 2 °C / min in a nitrogen atmosphere. The temperature was maintained for 3 h. After the treatment was completed, the mixture was allowed to cool naturally to room temperature to obtain the desired porous silica-based nanocomposite material.
[0027] Comparative Example 1: This comparative example is basically the same as Example 1, except that the porous silica-based nanocomposite material is replaced with an equal mass of fumed silica.
[0028] Comparative Example 2: This comparative example is basically the same as Example 1, except that step 1) is omitted in the preparation of the porous silica-based nanocomposite material. The specific method is as follows: 1) Add 2.2g of zinc nitrate hexahydrate and 1.4g of hexamethylenetetramine to 300mL of deionized water. Stir magnetically for 30min at room temperature at a stirring speed of 400r / min. After complete dissolution, the precursor growth solution is obtained. Then, transfer it to a reaction vessel and heat it to 80℃ at a rate of 2℃ / min. React at this temperature for 8h. After the reaction is completed, centrifuge the mixture and wash it 5 times with anhydrous ethanol and deionized water alternately. Dry it to constant weight and then heat it to 200℃ at a rate of 1℃ / min under a nitrogen atmosphere. React at this temperature for 2h. After treatment, allow it to cool naturally to room temperature to obtain nanowires. 2) Add 2g of porous silica to 400mL of ethanol solution, sonicate at 100W for 20min at room temperature, centrifuge, dry at 60℃ for 6h, and then treat with oxygen plasma for 3min to obtain pretreated porous silica. Add 0.8g of nanowires to 350mL of ethanol solution, sonicate at 100W for 20min in an ice-water bath, and then stir at 100r / min for 10min to obtain a suspension. Then, add the pretreated porous silica to the suspension at a solid-liquid ratio of 1g:80mL, stir at 200r / min for 10min, transfer to a vacuum impregnation tank, maintain a vacuum of -0.07MPa for 30min, slowly depressurize to atmospheric pressure, continue stirring for 2h, centrifuge, dry to constant weight, heat to 220℃ at a rate of 1℃ / min in a nitrogen atmosphere, and maintain the temperature for 2h. After the treatment is completed, allow it to cool naturally to room temperature.
[0029] Comparative Example 3: This comparative example is basically the same as Example 1, except that steps 2)-3) are omitted in the preparation of the porous silica-based nanocomposite material. The specific method is as follows: 1) Dissolve 2g of nickel nitrate hexahydrate in 250mL of deionized water to obtain a nickel salt solution. Dissolve 1.3g of sodium oxalate and 1.4g of hexamethylenetetramine in 250mL of deionized water to obtain a mixed solution. Add the nickel salt solution to an equal volume of the mixed solution. Stir the mixture at 400r / min at room temperature for 4 hours. After the reaction is complete, centrifuge the product and wash it with anhydrous ethanol and deionized water alternately 5 times. Then dry it to constant weight to obtain a micro-nano rod precursor. Then heat the micro-nano rod precursor to 350℃ at a rate of 1℃ / min under a nitrogen atmosphere and keep it at that temperature for 4 hours. After the treatment is complete, cool it to room temperature naturally to obtain porous rod-shaped nanomaterials. 2) Add 2g of porous silica to 400mL of ethanol solution, sonicate at 100W for 20min at room temperature, centrifuge, dry at 60℃ for 6h, and then treat with oxygen plasma for 3min to obtain pretreated porous silica. Add 0.8g of porous rod-shaped nanomaterials to 350mL of ethanol solution, sonicate at 100W for 20min in an ice-water bath, and then stir at 100r / min for 10min to obtain a suspension. Then, add the pretreated porous silica to the suspension at a solid-liquid ratio of 1g:80mL, stir at 200r / min for 10min, transfer to a vacuum impregnation tank, maintain a vacuum of -0.07MPa for 30min, slowly depressurize to atmospheric pressure, continue stirring for 2h, centrifuge, dry to constant weight, heat to 220℃ at a rate of 1℃ / min in a nitrogen atmosphere, and maintain the temperature for 2h. After the treatment is completed, allow it to cool naturally to room temperature.
[0030] Comparative Example 4: This comparative example is basically the same as Example 1, except that step 4 is omitted in the preparation of the porous silica-based nanocomposite material, that is, rod-shaped composite nanomaterials are used instead of porous silica-based nanocomposite materials.
[0031] Comparative Example 5: This comparative example is basically the same as Example 1, except that in the preparation of the porous silica-based nanocomposite material, steps 2)-4) are omitted, that is, porous rod-shaped nanomaterials are used instead of porous silica-based nanocomposite materials.
[0032] Test experiment: The ultrafine active heavy calcium carbonate provided in Examples 1-3 and Comparative Examples 1-5 were used as fillers and applied to two-component epoxy resin adhesives. The preparation of component A of the two-component epoxy resin adhesive was as follows: 35 parts by weight of bisphenol A type epoxy resin (Phoenix E51) were placed in a container, and 10 parts by weight of bisphenol F type epoxy resin (Nanya 170) and 5 parts by weight of alicyclic epoxy resin 2021p type epoxy resin were added to obtain a liquid substance. The liquid substance was stirred at 1000 r / min for 10 min. Then, 50 parts by weight of heavy calcium carbonate filler, 5 parts by weight of plasticizer, and 5% by weight of silane coupling agent KH550 (accounting for 5% of the total mass of the three types of epoxy resins) were weighed. The mixture was stirred for another 10 min and then placed in an oven to dry at 100°C for 1 h to obtain a solid substance. The solid and liquid substances were then mixed evenly at a solid-liquid ratio of 50:50 until there was no obvious stratification to obtain component A. Preparation of component B: Take 20 parts of triethylenetetramine, 10 parts of polyetheramine D400 curing agent, 10 parts of phenolic amine (Liansheng LSC203) and 30 parts of polyamide 651 into a dry container, stir and mix at 1000 r / min for 25 min until the color is consistent and there is no obvious layering, to obtain component B; When using, mix component A and component B in a mass ratio of 100:30 until the color is uniform, then apply it to the item for bonding.
[0033] Maximum compressive load, compressive modulus: tested according to ASTM D695-26 standard.
[0034] Elongation: Tested according to GB / T2567-2021 standard.
[0035] Bond strength: Tested in accordance with GB / T 7124-2008 standard.
[0036] Shear strength of punch press: tested according to ASTM D732-24 (2024) standard.
[0037] Hardness: Tested according to GB / T 3854-2017 standard.
[0038] Water resistance: After bonding the two-component epoxy resin adhesive to the item (steel), the bonding strength P1 is measured according to GB / T 7124-2008 standard. Then, after immersing in water for 72 hours and draining the water, the bonding strength P2 is measured again. The bonding strength retention rate after immersion is calculated as follows: bonding strength P2 after immersion / bonding strength P1 before immersion × 100%.
[0039] The test results are shown in Table 1.
[0040] Table 1
[0041] As shown in Table 1, the ultrafine active heavy calcium carbonate in the embodiments of the present invention, when used as a filler in a two-component epoxy resin adhesive, exhibits excellent bonding strength, compressive strength, toughness, and water resistance. In particular, it has high compressive strength, strong toughness, and excellent bonding strength. Furthermore, after long-term immersion in water, its bonding strength retention rate is high, which can meet normal use requirements. In contrast, the adhesives in Comparative Examples 1-5, since they did not use the ultrafine active heavy calcium carbonate of this application, have inferior overall performance compared to the embodiments.
[0042] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to the specific implementations described. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention. The invention is limited only by the claims and their full scope and equivalents.
Claims
1. A process for the production of ultrafine reactive ground calcium carbonate for adhesives, characterized in that, Specifically, the steps include the following: 1) Select high-purity heavy calcium carbonate coarse material, crush and screen it, and pass it through a 100-mesh sieve to obtain heavy calcium carbonate fine material; 2) Mix the fine heavy calcium carbonate with deionized water to make a slurry, adjust the solid content of the slurry to 65-75%, add a dispersant, grind and then add water to dilute and adjust the mixture to obtain a heavy calcium carbonate slurry. 3) A stepwise modification process is adopted. The heavy calcium carbonate slurry is placed in a reactor. Under stirring, a silane coupling agent solution is sprayed into the slurry. After stirring, an inorganic dispersion is added. After stirring, preheated molten stearic acid is sprayed into the reactor. The amounts of the silane coupling agent solution, inorganic dispersion, and molten stearic acid are 1-2%, 2-5%, and 2.3-2.8% of the total mass of heavy calcium carbonate in the heavy calcium carbonate slurry, respectively. 4) The above slurry is fed into a low-temperature airflow drying device. After drying, it is dispersed and classified by airflow to obtain ultrafine active heavy calcium carbonate.
2. The production method of the ultrafine active ground calcium carbonate for adhesives according to claim 1, characterized by, In step 1), the high-purity heavy calcium carbonate crude material is high-purity calcite raw material with a dry basis calcium carbonate content ≥96%, Fe2O3≤0.02%, SiO2≤1%, MgO≤1%, Al2O3≤0.01%, and whiteness ≥96.2%. In step 2), the dispersant is a polyacrylate dispersant, and the amount added is 0.1-0.3% of the mass of the heavy calcium carbonate fines. In step 3), the heavy calcium carbonate slurry has a solid content of 15-18%, and the slurry powder particle size D50 is 3.5-4.5μm and D97≤10μm; In step 3), the temperature inside the reactor is 70-75℃, and the stirring speed is 800-1000 r / min; In step 3), the preheated molten stearic acid is preheated at a temperature of 75-78°C. In step 4), the drying equipment has an inlet air temperature controlled at 110-130℃ and an outlet air temperature of 60-80℃.
3. The method of producing ultrafine active ground calcium carbonate for adhesives according to claim 1, characterized by, The silane coupling agent solution is obtained by adding 1.5-2.5 parts of silane coupling agent KH-550 to 7-10 parts of anhydrous ethanol and 0.8-1.2 parts of deionized water, and then stirring and hydrolyzing. The inorganic dispersion is obtained by dispersing 2-3 parts of fumed silica and 3-5 parts of porous silica-based nanocomposite material in 20-40 parts of an ethanol solution prepared by anhydrous ethanol and deionized water at a volume ratio of 95:5, and then dispersing them evenly in an ice-water bath. The molten stearic acid, by weight, is obtained by heating 2.5-3.5 parts of stearic acid in a sealed melting vessel to 70-75°C until completely melted.
4. The production method of the ultrafine active ground calcium carbonate for adhesives according to claim 3, characterized by, The porous silica-based nanocomposite material is prepared by the following method: 1) Add porous silica to an ethanol solution, disperse it evenly, centrifuge it, dry it to constant weight, and then treat it with oxygen plasma for 3-4 minutes to obtain pretreated porous silica; 2) The rod-shaped composite nanomaterials were added to an ethanol solution and dispersed evenly in an ice-water bath to obtain a suspension; 3) Add the pretreated porous silica to the suspension at a solid-liquid ratio of 1g:(80-150)mL, stir thoroughly, and then transfer it to a vacuum impregnation tank. Maintain the vacuum at -0.07 to -0.09MPa for 30-50 minutes. After depressurizing to atmospheric pressure, continue stirring thoroughly. After centrifugation, dry to constant weight and treat in a nitrogen atmosphere for 2-3 hours. After treatment, allow it to cool naturally to room temperature.
5. The method for producing ultrafine activated heavy calcium carbonate for adhesives according to claim 4, characterized in that, In step 1), the porous silica has a particle size of 300-400 nm and a pore size of 50-60 nm. In step 1), the ethanol solution is prepared by mixing anhydrous ethanol and deionized water at a volume ratio of 95:
5. In step 1), the ratio of porous silica to ethanol solution is (2-5) g: (400-900) mL; In step 2), the ratio of rod-shaped composite nanomaterials to ethanol solution in the suspension is (0.8-1.5) g : (350-500) mL; In step 3), the processing temperature is 220-230℃, and the heating rate is 1-2℃ / min.
6. The method for producing ultrafine activated heavy calcium carbonate for adhesives according to claim 4, characterized in that, The rod-shaped composite nanomaterial is prepared by the following method: 1) After ultrasonic cleaning and drying, the porous rod-shaped nanomaterials are treated with oxygen plasma for 3-4 minutes, then immersed in zinc acetate ethanol solution, dispersed evenly, centrifuged, dried, and heat-treated in air atmosphere for 1-2 hours, and then cooled naturally to obtain pretreated porous rod-shaped nanomaterials. 2) Add zinc nitrate hexahydrate and hexamethylenetetramine to deionized water in sequence, stir thoroughly at room temperature, and obtain the precursor growth solution after complete dissolution; 3) The pretreated porous rod-shaped nanomaterials are added to the precursor growth solution, and after thorough stirring and ultrasonic dispersion, they are transferred to a reaction vessel and reacted for 8-10 hours. 4) After the reaction is complete, the material is centrifuged, washed, dried, and treated under a nitrogen atmosphere for 2-3 hours. After treatment, it is naturally cooled to room temperature to obtain rod-shaped composite nanomaterials.
7. The method of producing ultrafine active ground calcium carbonate for adhesives according to claim 6, characterized by, In step 1), the concentration of the zinc acetate ethanol solution is 0.005-0.01 mol / L; In step 1), the heat treatment is performed at a temperature of 350-360℃, with a heating rate of 3-5℃ / min. In step 2), the ratio of zinc nitrate hexahydrate, hexamethylenetetramine, and deionized water in the precursor growth solution is (2.2-4.0) g: (1.4-2.5) g: (300-500) mL.
8. The method of producing ultrafine active ground calcium carbonate for adhesives according to claim 6, characterized by, In step 3), the solid-liquid ratio of the pretreated porous rod-shaped nanomaterial and the precursor growth solution is 1g:(30-50)mL; In step 3), the reaction is carried out at a temperature of 80-90℃, with a heating rate of 2-3℃ / min. In step 4), the processing temperature is 200-210℃, and the heating rate is 1-2℃ / min.
9. The method of producing ultrafine active ground calcium carbonate for adhesives according to claim 6, characterized by, The porous rod-shaped nanomaterial is prepared by the following method: 1) Dissolve nickel nitrate hexahydrate in deionized water to obtain a nickel salt solution, and dissolve sodium oxalate and hexamethylenetetramine in deionized water to obtain a mixed solution; 2) Add the nickel salt solution to an equal volume of the mixture, stir continuously at room temperature for 4-6 hours, centrifuge after the reaction is complete, wash and dry the precipitate to obtain the micro-nano rod precursor; 3) Treat the micro-nano rod precursor under a nitrogen atmosphere for 4-6 hours. After the treatment is completed, allow it to cool naturally to room temperature to obtain porous rod-shaped nanomaterials.
10. The method of producing ultrafine active ground calcium carbonate for adhesives according to claim 9, characterized by, In step 1), the ratio of nickel nitrate hexahydrate to deionized water in the nickel salt solution is (2-5) g: (250-350) mL; In step 1), the ratio of sodium oxalate, hexamethylenetetramine, and deionized water in the mixture is (1.3-2.5) g : (1.4-2.8) g : (250-350) mL; In step 2), the stirring reaction is carried out at a speed of 400-500 r / min; In step 3), the processing temperature is 350-380℃, and the heating rate is 1-3℃ / min.
Citation Information
Patent Citations
Two-component polyurethane adhesive and preparation method thereof
CN109705795A