A water-based high-alloy steel high-temperature casting blank anti-oxidation coating, a preparation method and application thereof

By forming a liquid glass phase and microcrack sources on high-alloy steel billets using water-based coatings, the problem of coating removal at high temperatures is solved, achieving efficient high-temperature anti-oxidation and easy removal effects, which is suitable for the large-scale production of high-alloy steel billets.

CN123107423APending Publication Date: 2026-11-17ANGANG STEEL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611357284.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-03
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing high-temperature anti-oxidation coatings are difficult to form a dense protective film on high-alloy steel billets at high temperatures and are prone to damaging the substrate. Furthermore, the coatings are difficult to remove effectively before rolling, which cannot meet the needs of large-scale production.

Method used

Water-based coatings composed of glass powder, mullite powder, zirconium oxide powder, and liquid colloids achieve coating adhesion and easy removal by forming a liquid glass phase and microcrack sources at high temperatures.

Benefits of technology

It effectively isolates oxygen at high temperatures, is easy to remove without damaging the substrate, and is suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107423A_ABST
    Figure CN123107423A_ABST
Patent Text Reader

Abstract

The application discloses a kind of water-based high-alloy steel high-temperature casting blank anti-oxidation coating and its preparation method and application.The coating is composed of glass powder, mullite powder, zirconia powder, liquid colloid and deionized water;Among them: the mass ratio of glass powder, mullite powder, zirconia powder is (3~5):(3~4):(1~2);The liquid colloid is composed of (2~4):1 of sodium hexametaphosphate aqueous solution and nano alumina sol;The liquid colloid accounts for 10%~20% of the total mass of glass powder, mullite powder, zirconia powder;The deionized water accounts for 10%~15% of the total mass of glass powder, mullite powder, zirconia powder.The glass powder, mullite powder, combined aluminum sol in the coating form a liquid glass phase under the action of high temperature, which can adhere to the surface of the casting blank to isolate the casting blank from the contact with gas;In addition, zirconia particles are dispersed in the glass phase, which play the role of micro-crack source when the glass phase is forced to cool, which is beneficial to the removal of the coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of high-temperature anti-oxidation coating technology, and more particularly to a water-based high-alloy steel high-temperature cast billet anti-oxidation coating, its preparation method, and its application. Background Technology

[0002] In the high-temperature metallurgical production of alloy steel, from the completion of casting to the cooling stage, the surface of the billet is prone to oxidation reaction with oxygen and water vapor in the air, generating iron oxide scale. This not only causes the surface quality of the billet to deteriorate, resulting in defects such as oxidation burn-off, cracks, and inclusions, but also affects the uniformity of composition due to the oxide layer, reducing the final performance of products with high surface purity requirements such as silicon steel and high-temperature alloys.

[0003] For high-alloy steel billets with a total alloy element content exceeding 10%, the presence of large amounts of chromium, aluminum, silicon, and other alloying elements with a strong affinity for oxygen leads to selective oxidation at the oxide layer-matrix interface during oxidation. This results in extremely dense spinel-structured phases or dense oxide films, such as FeO·Cr2O3 and FeO·Al2O3. This results in an extremely thin and highly dense oxide layer, lacking natural crack pathways for detachment. Furthermore, the oxide layer exhibits extremely strong metallurgical bonding with the matrix, even anchoring the oxide scale firmly to the matrix through the oxide pinning effect generated by internal oxidation. This makes it extremely difficult to remove the oxide layer from high-alloy steel billets using traditional methods. Conventional high-pressure water descaling is insufficient to break down and peel off this firmly bonded and seamless dense oxide film; mechanical grinding or shot blasting, due to the extremely thin oxide layer, easily damages the matrix during removal and has low processing efficiency, making it unsuitable for large-scale continuous production.

[0004] To address the aforementioned issues, the industry primarily employs two solutions: one is to develop more powerful removal equipment, and the other is to apply protection to the cast billet before heating to inhibit the formation of oxide scale at its source. The latter, due to its fundamental nature, has become the focus of research, leading to the development of high-temperature cast billet anti-oxidation coatings. The core requirement is the rapid formation of a dense and strongly adhering protective film under the high-temperature environment (typically 800-1200℃) experienced by the cast billet, effectively isolating it from contact with the substrate by atmospheres such as oxygen and nitrogen. Simultaneously, the coating must possess good high-temperature resistance and thermal shock stability, without undergoing harmful chemical reactions with the cast billet substrate, and be easily removed in subsequent processing steps without adversely affecting the final product performance. For example, patent CN201911411545.0 discloses a high-temperature resistant anti-oxidation coating, its preparation method, and its application. The high-temperature resistant anti-oxidation coating comprises the following raw material components in parts by weight: 5-10 parts quicklime, 5-15 parts refractory clay, 10-25 parts iron oxide scale, and 50-80 parts water. This technical solution utilizes the synergistic effect of refractory clay, quicklime, and iron oxide scale to not only give the coating excellent brushing or spraying performance but also excellent high-temperature chemical stability. The resulting dense coating isolates the steel billet from the oxidizing medium in the heating furnace. Furthermore, it allows for coating or spraying without requiring the steel billet to cool down, preventing issues such as coating cracking. This effectively reduces oxidation loss and surface decarburization. Moreover, the raw materials for this coating are inexpensive, making it a promising technology with excellent application prospects.

[0005] However, existing high-temperature anti-oxidation coatings generally suffer from insufficient versatility when applied to high-alloy steel billets with a total alloy content exceeding 10%. The core issue lies in the inability to simultaneously achieve both high-temperature protection and easy pre-rolling removal. To achieve reliable high-temperature protection, the coating must be dense and firmly adhered; however, this results in the coating becoming a difficult-to-remove foreign object after the furnace is removed. For subsequent removal of this coating, if the design relies on the thermal expansion mismatch between the coating and the substrate during cooling to achieve self-peeling, the peeling effect is extremely unstable under complex actual working conditions, often leaving residues. These residual coatings, when rolled into the steel, form inclusion defects that are even more harmful than oxide scale. If forced removal methods such as high-pressure water or mechanical grinding are used before rolling, the coating itself is designed to be firmly bonded to the substrate and is difficult to break, easily damaging the surface of the high-alloy steel billet and inducing stress cracks, failing to meet the needs of large-scale production. Summary of the Invention

[0006] The present invention aims to provide a water-based anti-oxidation coating for high-temperature cast billets of high alloy steel, its preparation method and application, in order to solve the problems existing in the prior art and achieve the effect of high-temperature anti-oxidation of high alloy steel cast billets and easy removal before rolling in the heating furnace.

[0007] To achieve the above objectives, the technical solution of the present invention is as follows: This invention provides a water-based anti-oxidation coating for high-temperature cast billets of high-alloy steel, the coating being composed of glass powder, mullite powder, zirconium oxide powder, liquid colloid, and deionized water; wherein: The mass ratio of the glass powder, mullite powder, and zirconium oxide powder is (3~5):(3~4):(1~2); The liquid colloid is composed of an aqueous solution of sodium hexaphosphate metaate and nano-alumina sol in a mass ratio of (2~4):1. The liquid colloid accounts for 10% to 20% of the total mass of glass powder, mullite powder, and zirconium oxide powder; The deionized water accounts for 10% to 15% of the total mass of glass powder, mullite powder, and zirconium oxide powder.

[0008] In the above technical solution, the glass powder has a purity of ≥99% and a particle size of 100~600µm; the mullite powder has a purity of ≥99% and a particle size of 100~600µm; and the zirconium oxide powder has a purity of ≥99% and a particle size of 100~600µm.

[0009] In the above technical solution, the mass concentration of the sodium hexaphosphate aqueous solution is further 25%~30%.

[0010] In the above technical solution, the solid content of the nano-alumina sol is further 20%~25%.

[0011] A second aspect of the present invention provides a method for preparing the above-mentioned water-based high-alloy steel high-temperature cast billet anti-oxidation coating, the method comprising the following steps: (1) Mix glass powder, mullite powder and zirconium oxide powder evenly and stir to obtain powdered material; (2) Mix the sodium hexaphosphate aqueous solution with the nano alumina sol to form a liquid colloid; (3) Add the powdered material obtained in step (1) to the mixer, turn on the mixer and stir at a stirring speed of 30~50r / min, add the liquid colloid obtained in step (2), add deionized water, and after the addition is completed, increase the stirring speed to 100~150r / min, stir for 6~8h, let stand for 6~8h, and obtain the coating.

[0012] In the above technical solution, further, in step (1), the stirring speed is 30~50 r / min and the stirring time is 30~50 min.

[0013] A third aspect of the present invention provides an application of the above-mentioned water-based high-alloy steel high-temperature cast billet anti-oxidation coating, comprising the following steps: a. Add water to the antioxidant coating and stir to obtain a liquid coating; b. After filtering the liquid coating, load it into the spraying machine and spray it on the surface of the steel billet between room temperature and 700°C.

[0014] In the above technical solution, further, in step a, the solid content of the liquid coating is 75%~80%.

[0015] In the above technical solution, further, in step b, a 60-80 mesh sieve is used for filtration.

[0016] In the above technical solution, further, in step b, the spraying pressure is 0.4~0.6 bar, and the paint flow rate is 100~150 mL / min.

[0017] The beneficial effects of this invention are as follows: 1. In the coating of this invention, glass powder, mullite powder, and alumina sol form a liquid glass phase under high temperature, which can adhere to the surface of the cast billet and isolate the cast billet from gas. In addition, zirconium oxide particles are dispersed in the glass phase, which act as microcrack sources when the glass phase is forcibly cooled, which is beneficial to the removal of the coating.

[0018] 2. The raw materials used in this invention are common and inexpensive, and the equipment for preparing the coating requires little investment, is portable, flexible and convenient. The water-based coating of this invention does not produce any toxic or harmful gases during the preparation and application process, making it highly environmentally friendly. Attached Figure Description

[0019] Figure 1 The results of sintering tests on the coatings of Examples 1 and 2 are shown. Figure 2 The coating peeling tests are for Example 1 and Comparative Example 1, where a is Example 1 and b is Comparative Example 1. Detailed Implementation

[0020] The following examples are intended to enable those skilled in the art to more fully understand the present invention, but do not limit the invention in any way.

[0021] Example 1 This embodiment provides a water-based anti-oxidation coating for high-temperature cast billets of high-alloy steel, which is composed of the following raw materials: 4 kg of glass powder (purity ≥99%, particle size 100~600µm), 4 kg of mullite powder (purity ≥99%, particle size 100~600µm), 2 kg of zirconium oxide powder (purity ≥99%, particle size 100~600µm), 2 kg of liquid colloid (of which the mass ratio of 25% sodium hexaphosphate metaate aqueous solution and 21% solid content nano alumina sol is 3:1), and 1 kg of deionized water; The above-mentioned method for preparing the coating includes the following steps: (1) Mix 4 kg of glass powder, 4 kg of mullite powder and 2 kg of zirconium oxide powder, put them into a drum, and stir at a stirring speed of 30 r / min and a stirring time of 50 min to obtain powdered material; (2) Prepare a sodium hexaphosphate solution with a mass concentration of 25%, and mix the sodium hexaphosphate solution with nano alumina sol at a mass ratio of 3:1 to obtain a liquid colloid. (3) Add the powdered material obtained in step (1) to the mixer, turn on the mixer and stir at a stirring speed of 30 r / min, add 2 kg of liquid colloid obtained in step (2), add 1 kg of deionized water, and after the addition is completed, increase the stirring speed to 100 r / min, stir for 8 hours, and let stand for 7 hours to obtain the coating.

[0022] The above-mentioned coating is used to spray the wear-resistant steel (ZGMn13) billet. The spraying process is as follows: a. Add water to the above coating and stir to obtain a liquid coating (solid content 75%~80%). b. After being filtered through a 70-mesh sieve, the coating is loaded into a spraying machine and sprayed onto the surface of the steel billet at room temperature. The spraying pressure is 0.4 bar and the coating flow rate is 100 mL / min.

[0023] Example 2 This embodiment provides a water-based anti-oxidation coating for high-temperature cast billets of high-alloy steel, which is composed of the following raw materials: 5 kg of glass powder (purity ≥99%, particle size 100~600µm), 3 kg of mullite powder (purity ≥99%, particle size 100~600µm), 2 kg of zirconium oxide powder (purity ≥99%, particle size 100~600µm), 2 kg of liquid colloid (of which the mass ratio of 30% sodium hexaphosphate metaate aqueous solution and 23% solid content nano alumina sol is 3:1), and 1 kg of water; The above-mentioned method for preparing the coating includes the following steps: (1) Mix 5kg of glass powder, 3kg of mullite powder and 2kg of zirconium oxide powder, put them into a drum, and stir at a stirring speed of 30r / min and a stirring time of 50min to obtain powdered material; (2) Prepare a 30% sodium hexaphosphate solution and mix the sodium hexaphosphate solution with nano alumina sol at a mass ratio of 3:1 to form a liquid colloid. (3) Add the powdered material obtained in step (1) to the mixer, turn on the mixer and stir at a stirring speed of 30 r / min, add 2 kg of liquid colloid obtained in step (2) and 1 kg of deionized water in sequence. After the addition is completed, increase the stirring speed to 100 r / min, stir for 8 hours, and let stand for 8 hours to obtain the coating.

[0024] The above-mentioned coating is used to spray the wear-resistant steel (ZGMn13) billet. The spraying process is as follows: a. Add water to the coating and stir to obtain a liquid coating (solid content 75%~80%). b. After being filtered through a 70-mesh sieve, the coating is loaded into a spraying machine and sprayed onto the surface of the steel billet at room temperature. The spraying pressure is 0.4 bar and the coating flow rate is 100 mL / min.

[0025] Comparative Example 1 Traditional anti-oxidation coating component ratio: Dry powder: 4 kg of industrial α-alumina powder, 1.5 kg of fused magnesium powder, 2.5 kg of silica powder, 1.2 kg of kaolin, and 0.8 kg of SiC powder; The binder liquid phase consists of purchased silica sol (30% silica by mass), accounting for 28%~36% of the dry powder. Additives: PVA accounts for 0.2%~0.4% of the dry powder, lithium-based bentonite accounts for 0.4% of the dry powder, and dispersant accounts for 0.2% of the dry powder.

[0026] Test Example 1 The wear-resistant steel (ZGMn13) billet samples coated with paint in Examples 1 and 2 were heated in a muffle furnace at 1300°C for 1 hour, and then cooled to 200°C in the furnace before the furnace door was opened.

[0027] like Figure 1 As shown in the figure, 1 is the wear-resistant steel coated with the coating of Example 1, 2 is the wear-resistant steel billet coated with the coating of Example 2, 3 is the wear-resistant steel billet without coating protection, and 4 is the material used for sintering test. It can be seen that the wear-resistant steel coating layers of Example 1 and Example 2 are completely adhered to the steel plate, while the wear-resistant steel without coating protection is oxidized into slag.

[0028] Test Example 2 Wear-resistant steel (ZGMn13) billets were coated with the coatings used in Example 1 and Comparative Example 1. After heat treatment at 1300℃, the billet samples were directly immersed in water. The coating peeling performance was then examined after removal from the water, as follows: Figure 2 As shown.

[0029] like Figure 2 As shown in Figure a, after the steel billet sample of the coating in Example 1 was immersed in water after being removed from the heating furnace, most of the coating had already peeled off, with no patches that were difficult to peel off; while Figure 2 After the steel billet sample coated with traditional paint was immersed in water, some patches that were not easy to remove remained.

[0030] The above embodiments are merely preferred embodiments of the present invention and are not intended to limit the implementation. The scope of protection of the present invention should be determined by the scope defined in the claims. Other variations or modifications can be made based on the above description. Obvious variations or modifications derived therefrom are still within the scope of protection of the present invention.

Claims

1. A water-based anti-oxidation coating for high-temperature cast billets of high-alloy steel, characterized in that, The coating is composed of glass powder, mullite powder, zirconium oxide powder, liquid colloid, and deionized water; wherein: The mass ratio of the glass powder, mullite powder, and zirconium oxide powder is (3~5):(3~4):(1~2); The liquid colloid is composed of an aqueous solution of sodium hexaphosphate metaate and nano-alumina sol in a mass ratio of (2~4):

1. The liquid colloid accounts for 10% to 20% of the total mass of glass powder, mullite powder, and zirconium oxide powder; The deionized water accounts for 10% to 15% of the total mass of glass powder, mullite powder, and zirconium oxide powder.

2. The water-based high-alloy steel high-temperature cast billet anti-oxidation coating according to claim 1, characterized in that, The glass powder has a purity of ≥99% and a particle size of 100~600µm; The purity of the mullite powder is ≥99%, and the particle size is 100~600µm; The zirconium oxide powder has a purity of ≥99% and a particle size of 100~600µm.

3. The water-based high-alloy steel high-temperature cast billet anti-oxidation coating according to claim 1, characterized in that, The mass concentration of the sodium hexaphosphate aqueous solution is 25%~30%.

4. The water-based high-alloy steel high-temperature cast billet anti-oxidation coating according to claim 1, characterized in that, The solid content of the nano-alumina sol is 20%~25%.

5. A method for preparing a water-based high-alloy steel high-temperature casting anti-oxidation coating as described in any one of claims 1-4, characterized in that, The method includes the following steps: (1) Mix glass powder, mullite powder and zirconium oxide powder evenly and stir to obtain powdered material; (2) Mix the sodium hexaphosphate aqueous solution with the nano alumina sol to form a liquid colloid; (3) Add the powdered material obtained in step (1) to the mixer, turn on the mixer and stir at a stirring speed of 30~50r / min, add the liquid colloid obtained in step (2), add deionized water, and after the addition is completed, increase the stirring speed to 100~150r / min, stir for 6~8h, let stand for 6~8h, and obtain the coating.

6. The preparation method according to claim 5, characterized in that, In step (1), the stirring speed is 30~50 r / min and the stirring time is 30~50 min.

7. The application of a water-based anti-oxidation coating for high-temperature cast billets of high-alloy steel according to any one of claims 1-4, or a water-based anti-oxidation coating for high-temperature cast billets of high-alloy steel prepared by the preparation method according to any one of claims 5-6, characterized in that, Includes the following steps: a. Add water to the antioxidant coating and stir to obtain a liquid coating; b. After filtering the liquid coating, load it into the spraying machine and spray it on the surface of the steel billet between room temperature and 700°C.

8. The application according to claim 7, characterized in that, In step a, the solid content of the liquid coating is 75%~80%.

9. The application according to claim 7, characterized in that, In step b, a 60-80 mesh sieve is used for filtration.

10. The application according to claim 7, characterized in that, In step b, the spraying pressure is 0.4~0.6 bar, and the paint flow rate is 100~150 mL / min.

Citation Information

Patent Citations

  • High-temperature-resistant anti-oxidation coating as well as preparation method and application thereof

    CN111117308A