A self-cleaning nano-coating material for photovoltaic modules and its preparation method
By preparing a self-cleaning nano-coating for photovoltaic modules composed of silicon-based mesoporous materials and nano-titanium dioxide, the problems of insufficient high-temperature curing process and anti-fouling properties of existing coatings are solved, achieving a high-efficiency and low-cost self-cleaning effect for photovoltaic modules, and improving the photoelectric conversion efficiency and service life of photovoltaic modules.
Patent Information
- Application Number
- CN202611257171.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-19
- Publication Date
- 2026-11-17
AI Technical Summary
Existing photovoltaic module coatings are difficult to meet the requirements of large-area, low-cost, and high-efficiency applications under the high-temperature curing process. Furthermore, existing self-cleaning films do not have significant anti-reflection and anti-fouling properties, resulting in reduced photovoltaic module efficiency and shortened lifespan.
A self-cleaning nano-coating material for photovoltaic modules, composed of silicon-based mesoporous materials, coated nano-titanium dioxide, hollow silica microspheres, and fluorine-modified acrylic resin, is formed by low-temperature ultraviolet light curing to create a dense organic-inorganic hybrid cross-linked network. Combining hydrophobic and antifouling properties with photocatalytic degradation and antistatic dust reduction functions, it solves the problems of coating adhesion, antifouling, and cleaning.
It achieves high adhesion between the coating and photovoltaic glass, and has hydrophobic and antifouling, photocatalytic degradation and antistatic dust reduction functions, which improves the photoelectric conversion efficiency and service life of photovoltaic modules, and reduces cleaning frequency and operation and maintenance costs.
Abstract
Description
Technical Field
[0001] This invention relates to the field of solar photovoltaic technology, and in particular to a self-cleaning nano-coating material for photovoltaic modules and its preparation method. Background Technology
[0002] As one of the clean and efficient green energy technologies of the future, solar energy technology has been increasingly widely used in recent years. The solar photovoltaic glass industry, which combines solar energy utilization with the traditional glass industry, is becoming one of the fastest-growing high-tech industries in the world, hailed as a rising sunrise industry. In recent years, the photovoltaic power generation industry has developed rapidly, with installed capacity experiencing explosive growth. Due to national policies encouraging the development of distributed photovoltaic power generation, it has also developed rapidly. In particular, the use of residential and factory rooftops for distributed grid-connected photovoltaic power generation is encouraged and promoted.
[0003] Photovoltaic modules operate in harsh outdoor environments for extended periods. Issues such as Fresnel reflection, surface dust accumulation, and contaminant adhesion lead to reduced efficiency, shortened lifespan, and high cleaning and maintenance costs, becoming major pain points for existing photovoltaic power plants. Self-cleaning anti-reflective coatings combine optical anti-reflective properties with self-cleaning capabilities, effectively suppressing dust accumulation, reducing solar energy loss due to interface reflection, improving photovoltaic module photoelectric conversion efficiency, and significantly reducing cleaning frequency. However, the curing process for photovoltaic glass coatings requires high-temperature calcination to ensure coating adhesion, which presents challenges in meeting the demands of large-area, low-cost, and high-efficiency photovoltaic module applications.
[0004] Chinese patent ZL201910155427.1 discloses a method for preparing a superhydrophilic self-cleaning photocatalytic thin film of titanium dioxide using a modified PTA method. The prepared film has excellent superhydrophilic self-cleaning properties and high light transmittance. Moreover, it does not require high-temperature treatment and can be immobilized on the surface of existing photovoltaic modules or substrates that cannot be tempered at high temperatures to achieve long-term self-cleaning function at room temperature, thus having broad application prospects.
[0005] However, this self-cleaning film layer does not have significant anti-reflection and dust-repellent properties, making it difficult to meet the application requirements of photovoltaic modules for anti-reflection and long-term anti-fouling. Furthermore, the photocatalytic nanosol prepared by this method uses water as the main solvent and has limited extensibility, which easily leads to uneven coating, localized over-coating, and difficulties in drying due to freezing in low-temperature environments during autumn and winter when loaded onto the surface of existing photovoltaic modules. Summary of the Invention
[0006] To address the problems mentioned in the background section, this invention provides a self-cleaning nano-coating material for photovoltaic modules and its preparation method.
[0007] To achieve the above objectives, the present invention adopts the following technical solution:
[0008] A self-cleaning nano-coating material for photovoltaic modules is prepared from the following raw materials in parts by weight:
[0009] 0.5-1.5 parts of silicon-based mesoporous material;
[0010] 0.8-2.0 parts of coated nano-titanium dioxide;
[0011] Hollow silica microspheres, 1.5-2.0 parts;
[0012] 10-12 parts of fluorinated modified acrylic resin;
[0013] 3-4 parts of reactive dilution monomer;
[0014] 0.5-1 part of modified PMMA diffusion particles;
[0015] 0.5-0.7 parts of silane coupling agent γ-methacryloyloxypropyltrimethoxysilane;
[0016] Phosphate ester adhesion promoter 0.2-0.5 parts;
[0017] Hydrophobically modified nano-ATO 0.5-1.2 parts;
[0018] Photoinitiator 0.3-0.4 parts;
[0019] Hindered amine light stabilizer HALS 0.1-0.5 parts;
[0020] Solvent 75-80 parts: Anhydrous ethanol and acetone are mixed at a mass ratio of 1-1.5:1.
[0021] Preferably, the silicon-based mesoporous material is SBA-15 with a particle size of 80-150 nm and a pore size of 8-10 nm, and the silicon-based mesoporous material is pre-modified with fluorosilane to achieve full-surface hydrophobicity.
[0022] The full-surface hydrophobic modification specifically includes:
[0023] (a) Vacuum dry and activate the SBA-15 mesoporous material at 150°C for 2-4 hours;
[0024] (b) Under an inert atmosphere, disperse the activated SBA-15 in an anhydrous organic solvent, add 10-30% of its mass of fluorosilane coupling agent, and react at 60-80°C for 6-12 hours.
[0025] (c) After the reaction is complete, centrifuge and wash, then vacuum dry to obtain the fully hydrophobic modified SBA-15.
[0026] Preferably, the coated nano-titanium dioxide is silica coated anatase crystal with a core particle size of 2-3 nm and a coating layer thickness of 3-5 nm. Long-chain hydrophobic silanes are grafted onto the coating layer to construct a double barrier layer, reducing the oxidative damage of free radicals to the resin. The pure titanium dioxide content is ≥80 wt%.
[0027] The long-chain hydrophobic silane is selected from at least one of octyltriethoxysilane and dodecyltriethoxysilane.
[0028] Preferably, the hollow silica microspheres have an average particle size of 55-60 nm, a wall thickness of 8-10 nm, and a visible light transmittance of ≥99%.
[0029] Preferably, the fluorinated acrylic resin is a dodecafluoroheptyl methacrylate copolymer, provided in the form of an ethanol dispersion system with a solid content of 50 wt%, and has an intrinsic water contact angle ≥105°.
[0030] Preferably, the reactive diluent monomer is a compound of dodecyl methacrylate and trimethylolpropane triacrylate in a mass ratio of (2.5-3):(0.5-1).
[0031] Preferably, the phosphate adhesion promoter is HEMA-phosphate.
[0032] Preferably, the hydrophobically modified nano-ATO is a silane-modified tin-antimony oxide with a particle size of 20-30 nm, and the hydrophobic modification specifically includes:
[0033] (a) Vacuum drying and activation of nano-ATO powder at 120°C for 1-2 hours;
[0034] (b) Under an inert atmosphere, the activated nano-ATO was ultrasonically dispersed in an anhydrous organic solvent, and 5-15% of silane coupling agent by mass was added. The pH was adjusted to 4-5, and the reaction was carried out at 50-60°C for 4-6 hours.
[0035] (c) After the reaction is complete, the nano-ATO is obtained by centrifugation, washing, vacuum drying, and grinding.
[0036] Preferably, the photoinitiator is a compound of acylphosphine oxide (TPO) and amine co-initiator (EDAB) in a mass ratio of 2-4:1.
[0037] Preferably, the hindered amine light stabilizer is bis(1-octoxy-2,2,6,6-tetramethyl-4-piperidinyl) sebacate.
[0038] The method for preparing the modified PMMA diffusion particles includes the following steps:
[0039] S1. Preparation of nanoscale hydroxy-crosslinked PMMA seed particles
[0040] Add 60-65 parts by weight of anhydrous ethanol and 20-25 parts by weight of deionized water to the reactor, add 2-2.5 parts by weight of polyvinylpyrrolidone K30, stir to dissolve and heat to 70-73℃, continuously purging with nitrogen for 25-30 min; add 10-12 parts by weight of methyl methacrylate, 1.5-2 parts by weight of hydroxyethyl methacrylate, 0.5-1 parts by weight of ethylene glycol dimethacrylate and 0.1-0.5 parts by weight of azobisisobutyronitrile to the reaction system at one time, and polymerize at a constant temperature of 450-500 rpm under nitrogen protection for 6-8 h; after the reaction is completed, cool to room temperature, centrifuge at high speed, wash with anhydrous ethanol and deionized water alternately 3-5 times, and vacuum dry at 45-50℃ for 20-24 h to obtain cross-linked PMMA seed particles with an average particle size of 90-110 nm and a surface rich in hydroxyl groups.
[0041] S2, Preparation of surface-bonded isocyanate active intermediates
[0042] Take 10-15 parts of the cross-linked PMMA seed particles prepared by S1 and disperse them in 170-200 parts of anhydrous ethyl acetate, and disperse them thoroughly by ultrasonication; add 4.5-5 parts of isophorone diisocyanate and 0.05-0.1 parts of dibutyltin dilaurate, and keep the system anhydrous and oxygen-free; pre-react at 30-40℃ for 0.5-1h, and then raise the temperature to 60-65℃ and continue the reaction for 4-6h; after the reaction is completed, centrifuge and wash several times to remove free unreacted diisocyanate molecules, and obtain functionalized PMMA diffusion particle intermediates with partially bonded isocyanate groups on the surface;
[0043] S3. Stepwise bifunctional grafting preparation of organic-inorganic bireactive modified PMMA diffusion particles:
[0044] The functionalized PMMA intermediates obtained from S2 were all re-dispersed ultrasonically in 150-170 parts of anhydrous ethyl acetate, and 0.6-0.8 parts of 3-aminopropyltriethoxysilane were slowly added dropwise. The reaction was carried out at 25-40℃ for 0.5-1 h. Subsequently, 5-6 parts of pentaerythritol triacrylate, 0.03-0.05 parts of phenothiazine polymerization inhibitor, and 0.05-0.1 parts of dibutyltin dilaurate catalyst were added, and the temperature was raised to 60-70℃ for 3-6 h. After the reaction was completed, the particles were centrifuged, washed multiple times with anhydrous ethyl acetate, and vacuum dried to obtain bireactive modified PMMA diffusion particles with siloxane groups and polyfunctional acrylate double bonds simultaneously bonded on the surface.
[0045] A method for preparing a self-cleaning nano-coating material for photovoltaic modules includes the following steps:
[0046] (1) Disperse the silicon-based mesoporous material, hollow silica microspheres, hydrophobically modified nano-ATO, and silane coupling agent in the first part of the solvent according to the weight parts mentioned above. Add 0.5-1.0% of deionized water according to the mass of the first part of the solvent, adjust the pH of the system to 4-5, and stir at room temperature for 15-20 min to complete the silane pre-hydrolysis. Then, disperse by ultrasonication and high-speed shearing to form an inorganic nanoparticle pre-dispersion liquid.
[0047] (2) Fluorine-modified acrylic resin, reactive diluent monomer, phosphate ester adhesion promoter, photoinitiator and hindered amine light stabilizer are mixed to form a photocurable resin matrix;
[0048] (3) The coated nano-titanium dioxide and modified PMMA diffusion particles are dispersed in the second solvent and ultrasonically formed into a functional particle slurry under light-protected conditions;
[0049] (4) Under light-protected conditions, the pre-dispersed liquid from step (1) is mixed with the resin matrix from step (2), and the functional particle slurry from step (3) is added. The remaining solvent is added, and the mixture is stirred and mixed evenly and degassed to obtain the coating liquid.
[0050] (5) The coating liquid is applied to the surface of photovoltaic glass, and after pre-baking, ultraviolet curing and post-baking treatment, a self-cleaning nano-coating is formed.
[0051] Preferably, the coating method is dip coating, spray coating, scraping coating, or spin coating;
[0052] The pre-baking process employs a gradient heating process, first evaporating most of the solvent at a low temperature of 40-50℃, and then raising the temperature to 70-80℃ to remove residual solvent, thereby reducing coating defects.
[0053] The ultraviolet curing uses a high-energy LED ultraviolet curing device;
[0054] The post-drying temperature is 100-150℃, and the time is 20-40 minutes.
[0055] Preferably, the first portion of solvent is 40-55% of the total solvent mass, and the second portion of solvent is 5-10%.
[0056] Compared with the prior art, the beneficial effects of the present invention are:
[0057] 1. The coating prepared by this invention is dense and has a much stronger adhesion to photovoltaic glass than physically stacked sol-gel films. It is easy to apply and has extremely low energy consumption. This invention uses a composite initiation system of acylphosphine oxide (TPO) and amine co-initiator EDAB. Under LED ultraviolet light irradiation, TPO undergoes α-cleavage to generate highly active phosphonyl and benzoyl free radicals. EDAB, as an amine co-initiator, reacts with the low-activity peroxy radicals generated by oxygen inhibition, converting them into highly active aminoalkyl free radicals, effectively counteracting the inhibitory effect of dissolved oxygen on the polymerization reaction. These free radicals rapidly initiate chain polymerization reactions in the unsaturated double bonds of the fluorinated acrylic resin side chains, the carbon-carbon double bonds of the reactive diluent monomers, and the polymerizable double bonds carried by the modified PMMA particles and the silane coupling agent KH-570, rapidly forming a highly cross-linked three-dimensional organic network. Meanwhile, the silanol groups generated after hydrolysis of the silane coupling agent KH-570 undergo dehydration condensation with the silanol groups on the glass surface and the surface of inorganic nanoparticles, forming strong Si-O-Si covalent bonds. The specially added HEMA-phosphate adhesion promoter has phosphate groups that can form strong hydrogen bonds with the silanol groups on the glass surface and coordinate bonds with metal ions on the glass surface. During the post-baking process, further dehydration strengthens the interfacial bonding, while the terminal methacrylate double bonds participate in free radical polymerization. The resulting organic-inorganic hybrid cross-linked network structure is dense and connected to the substrate through multi-point chemical bonds, exhibiting extremely strong adhesion and preventing it from being easily washed away by rainwater like physically deposited sol films. Furthermore, the ethanol-acetone mixed solvent system has low surface tension and good film wettability, avoiding the uneven coating and sagging defects common in water-based systems, and has no risk of freezing at low temperatures, making it suitable for outdoor construction in autumn and winter.
[0058] 2. The coating prepared by this invention possesses four self-cleaning functions: hydrophobic antifouling, photocatalytic degradation, antistatic dust reduction, and mesoporous enrichment enhancement. This solves the fundamental problems of single superhydrophilic self-cleaning membranes failing in the absence of light and having limited ability to remove inorganic dust. Specifically, the fluorinated side chains of the dodecafluoroheptyl methacrylate copolymer spontaneously migrate and accumulate at the coating-air interface during film formation, forming a low surface energy antifouling shielding layer. Furthermore, the SiO2 coating layer of the coated nano-TiO2 is further grafted with long-chain hydrophobic silanes on the outer layer. Under ultraviolet light excitation, the electron-hole pairs generated by the TiO2 core react with O2 and H2O diffused into the porous SiO2 shell to generate reactive oxygen free radicals, thereby degrading trace organic pollutants adhering to the coating surface. This dual-barrier layer design effectively prevents the reverse diffusion of reactive free radicals into the organic resin matrix, greatly slowing down the photo-oxidative degradation of the matrix.
[0059] Hydrophobically modified nano-ATO is uniformly dispersed in the coating, constructing carrier transport channels and effectively reducing the surface resistivity of the coating. Static charges generated on the coating surface due to friction or airflow can be rapidly discharged through these channels, thereby significantly reducing dry inorganic dust adhering to the surface due to electrostatic adsorption and reducing the dust accumulation rate at the source.
[0060] The SBA-15 mesoporous material, modified with fluorosilane for hydrophobicity across its entire surface, exhibits hydrophobicity in both the inner and outer walls of its ordered pores. It can preferentially adsorb and enrich low-concentration gaseous organic pollutants from the air using its high specific surface area, allowing them to diffuse through the concentration gradient to nearby TiO2 catalytic sites, thereby increasing the substrate concentration and reaction efficiency in the photocatalytic reaction. Simultaneously, the hydrophobic pores avoid the risk of water and scale buildup due to capillary condensation, ensuring long-term effectiveness. Detailed Implementation
[0061] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0062] Unless otherwise specified, the raw materials used in this invention are all from commercially available conventional products.
[0063] Dodecyl methacrylate was purchased from Aladdin, CAS No.: 142-90-5;
[0064] Trimethylolpropane triacrylate was purchased from Aladdin, CAS No.: 15625-89-5;
[0065] HEMA-phosphate ester was purchased from Aladdin, CAS No.: 52628-03-2;
[0066] Acylphosphine oxide (TPO) was purchased from Aladdin, CAS No.: 75980-60-8;
[0067] The amine co-initiator EDAB was purchased from Aladdin, CAS No.: 10287-53-3;
[0068] The bis(1-octyloxy-2,2,6,6-tetramethyl-4-piperidinyl) sebacate was purchased from Aladdin, CAS No.: 129757-67-1;
[0069] Polyvinylpyrrolidone K30 was purchased from Aladdin, CAS No.: 9003-39-8.
[0070] The solvents in steps (2), (3) and (4) described below are anhydrous ethanol and acetone mixed in a mass ratio of 1:1.
[0071] The silicon-based mesoporous material is SBA-15, with a particle size of 80 nm and a pore size of 8 nm. It has undergone pre-treatment with fluorosilanes to perform full-surface hydrophobic modification, specifically including:
[0072] (a) The SBA-15 mesoporous material was vacuum dried and activated at 150°C for 3 hours;
[0073] (b) Under an inert atmosphere, the activated SBA-15 was dispersed in anhydrous ethanol, and perfluorooctyltriethoxysilane at a mass of 20% of SBA-15 was added. The mixture was reacted at 70°C for 8 hours.
[0074] (c) After the reaction is complete, centrifuge and wash, then vacuum dry to obtain the fully hydrophobic modified SBA-15.
[0075] The hollow silica microspheres have an average particle size of 58 nm, a wall thickness of 8.5 nm, and a visible light transmittance of ≥99%.
[0076] The hydrophobically modified nano-ATO is a silane-modified tin-antimony oxide with a particle size of 25 nm. The hydrophobic modification specifically includes:
[0077] (a) The tin antimony oxide powder was vacuum dried and activated at 120°C for 1 hour;
[0078] (b) Under an inert atmosphere, the activated tin antimony oxide was ultrasonically dispersed in anhydrous ethanol, and 10% of its mass of isobutyltriethoxysilane was added to adjust the pH to 4.5. The reaction was carried out at 55°C for 5 hours.
[0079] (c) After the reaction is complete, the product is centrifuged, washed, vacuum dried, and ground to obtain hydrophobic modified tin-antimony oxide.
[0080] The coated nano-titanium dioxide is anatase crystal coated with silicon dioxide, with a core particle size of 2nm and a coating layer thickness of 3nm. Octyltriethoxysilane is grafted onto the coating layer, and the pure titanium dioxide content is 85wt%.
[0081] Preparation Example 1
[0082] S1. Preparation of nanoscale hydroxy-crosslinked PMMA seed particles
[0083] Add 620g of anhydrous ethanol and 230g of deionized water to the reactor, then add 22g of polyvinylpyrrolidone K30. After stirring until completely dissolved, raise the temperature to 72℃ and continuously purge with nitrogen for 30min to remove oxygen from the system. Mix 110g of methyl methacrylate, 18g of hydroxyethyl methacrylate, 7g of ethylene glycol dimethacrylate, and 3g of azobisisobutyronitrile (AIBN) and add them to the reaction system all at once. Under nitrogen protection and constant stirring speed of 480rpm, the polymerization reaction is carried out at a constant temperature for 7h.
[0084] After the reaction was completed, the mixture was naturally cooled to room temperature and centrifuged at 10,500 rpm. The solid was washed four times with anhydrous ethanol and deionized water to remove residual monomers and dispersants. The washed solid was then dried in a vacuum oven at 48°C for 22 hours to obtain cross-linked polymethyl methacrylate seed particles with an average particle size of 100 nm and a surface rich in hydroxyl groups. The particles were then dried for later use.
[0085] S2, Preparation of surface-bonded isocyanate active intermediates
[0086] Accurately weigh 130g of cross-linked PMMA seed particles prepared by S1, add them to 1850g of anhydrous ethyl acetate, and ultrasonically disperse for 20min until the system is uniform, transparent and free of agglomerated particles; add 48g of isophorone diisocyanate and 0.8g of dibutyltin dilaurate, and maintain an anhydrous and oxygen-free environment throughout the process;
[0087] First, the temperature was raised to 35℃ for a pre-reaction of 0.8h to eliminate surface activity defects of the particles; then the temperature was raised to 62℃ and the reaction was continued at a constant temperature for 5h; after the reaction was completed, the particles were washed multiple times by high-speed centrifugation to completely remove free unreacted isophorone diisocyanate molecules, and functionalized PMMA diffusion particle intermediates with some isocyanate groups uniformly bonded to the surface were obtained.
[0088] S3. Stepwise bifunctional grafting preparation of organic-inorganic bireactive modified PMMA diffusion particles
[0089] All the functionalized PMMA intermediates prepared by S2 were redispersed in 1600g of anhydrous ethyl acetate and thoroughly reconstituted by sonication; 7g of 3-aminopropyltriethoxysilane was slowly added dropwise and reacted at 30℃ for 0.8h to complete the grafting of siloxane functional segments.
[0090] Subsequently, 55g of pentaerythritol triacrylate, 0.4g of phenothiazine polymerization inhibitor, and 0.7g of dibutyltin dilaurate catalyst were added to the system. The temperature was raised to 65℃ and the reaction was carried out at a constant temperature for 4.5h to completely graft the remaining isocyanate groups onto the polyfunctional acrylate active segment. After the reaction was completed, the particles were separated by centrifugation, washed repeatedly with anhydrous ethyl acetate four times, and dried under vacuum to obtain bireactive modified PMMA diffusion particles with siloxane groups and polyfunctional acrylate double bonds simultaneously bonded to the surface.
[0091] Preparation Example 2
[0092] S1. Preparation of nanoscale hydroxy-crosslinked PMMA seed particles
[0093] Add 600g of anhydrous ethanol and 200g of deionized water to the reactor, then add 20g of polyvinylpyrrolidone K30. After stirring and dissolving, heat to 70℃ and continuously purge with nitrogen for 25min. Mix 100g of methyl methacrylate, 15g of hydroxyethyl methacrylate, 5g of ethylene glycol dimethacrylate, and 1g of azobisisobutyronitrile (AIBN) evenly and add the mixture all at once. Polymerize under nitrogen protection at a constant temperature of 450rpm for 6h.
[0094] After cooling, the particles were centrifuged at 10,000 rpm, washed three times alternately with anhydrous ethanol and deionized water, and dried under vacuum at 45°C for 20 h to obtain hydroxyl cross-linked PMMA seed particles with an average particle size of 90 nm.
[0095] S2, Preparation of surface-bonded isocyanate active intermediates
[0096] 100g of dried S1 PMMA seed particles were weighed and dispersed in 1700g of anhydrous ethyl acetate and ultrasonically dispersed evenly. 45g of isophorone diisocyanate and 0.5g of dibutyltin dilaurate were added. Under anhydrous and oxygen-free conditions, the mixture was pre-reacted at 30℃ for 0.5h and then reacted at 60℃ for 4h. Free small molecules were removed by centrifugation and washing with anhydrous ethyl acetate to obtain NCO-functionalized PMMA intermediate.
[0097] S3. Stepwise bifunctional grafting preparation of modified PMMA diffusion particles
[0098] The S2 intermediate was dispersed in 1500g of anhydrous ethyl acetate, and 6g of 3-aminopropyltriethoxysilane was added dropwise. The reaction was carried out at 25℃ for 0.5h. Then, 50g of pentaerythritol triacrylate, 0.3g of phenothiazine, and 0.5g of dibutyltin dilaurate were added, and the reaction was carried out at 60℃ for 3h. The product was washed by centrifugation with anhydrous ethyl acetate and dried to obtain bireactive modified PMMA diffusion particles.
[0099] Preparation Example 3
[0100] S1. Preparation of nanoscale hydroxy-crosslinked PMMA seed particles
[0101] Add 650g of anhydrous ethanol and 250g of deionized water to the reactor, then add 25g of polyvinylpyrrolidone K30. After stirring and dissolving, heat to 73℃ and continuously purge with nitrogen for 30min. Mix 120g of methyl methacrylate, 20g of hydroxyethyl methacrylate, 10g of ethylene glycol dimethacrylate, and 5g of azobisisobutyronitrile (AIBN) evenly and add the mixture all at once. Polymerize under nitrogen protection at a constant temperature of 500rpm for 8h.
[0102] After cooling, the particles were centrifuged at 11,000 rpm, washed five times with anhydrous ethanol and deionized water, and dried under vacuum at 50°C for 24 h to obtain hydroxyl cross-linked PMMA seed particles with an average particle size of 110 nm.
[0103] S2, Preparation of surface-bonded isocyanate active intermediates
[0104] 150g of dried S1 seed particles were weighed and dispersed in 2000g of anhydrous ethyl acetate and ultrasonically dispersed evenly. 50g of isophorone diisocyanate and 1.0g of dibutyltin dilaurate were added. Under anhydrous and oxygen-free conditions, the mixture was pre-reacted at 40℃ for 1h and then reacted at 65℃ for 6h. Free small molecules were removed by centrifugation and washing with anhydrous ethyl acetate to obtain NCO-functionalized PMMA intermediate.
[0105] S3. Stepwise bifunctional grafting preparation of modified PMMA diffusion particles
[0106] The S2 intermediate was dispersed in 1700g of anhydrous ethyl acetate, and 8g of 3-aminopropyltriethoxysilane was added dropwise. The reaction was carried out at 40℃ for 1h. Then, 60g of pentaerythritol triacrylate, 0.5g of phenothiazine, and 1.0g of dibutyltin dilaurate were added, and the reaction was carried out at 70℃ for 6h. After centrifugation, washing, and drying, bireactive modified PMMA diffusion particles were obtained.
[0107] Example 1
[0108] (1) 0.5g of silica-based mesoporous material SBA-15, 1.5g of hollow silica microspheres, 0.5g of hydrophobically modified nano-ATO, and 0.5g of γ-methacryloyloxypropyltrimethoxysilane were dispersed in 40g of solvent, 0.4g of deionized water was added, the pH of the system was adjusted to 4, and the mixture was stirred at room temperature for 20min to complete the silane pre-hydrolysis; then, the mixture was ultrasonically dispersed and subjected to high-speed shearing to form an inorganic nanoparticle pre-dispersion liquid;
[0109] (2) Mix 20g of 50wt% dodecafluoroheptyl methacrylate copolymer ethanol dispersion, 3g of reactive diluent monomer, 0.2g of HEMA-phosphate ester, 0.3g of photoinitiator and 0.1g of bis(1-octoxy-2,2,6,6-tetramethyl-4-piperidinyl) sebacate to form a photocurable resin matrix;
[0110] The reactive diluent monomer is a compound of dodecyl methacrylate and trimethylolpropane triacrylate in a mass ratio of 2.5:1.
[0111] The photoinitiator is a compound of acylphosphine oxide (TPO) and amine co-initiator (EDAB) in a mass ratio of 2:1.
[0112] (3) 0.8g of coated nano-titanium dioxide and 0.8g of modified PMMA diffusion particles prepared in Preparation Example 1 were dispersed in 8g of solvent and ultrasonically formed into functional particle slurry under light-protected conditions;
[0113] (4) Under light-protected conditions, the pre-dispersed liquid from step (1) is mixed with the resin matrix from step (2), and the functional particle slurry from step (3) is added. The remaining 32g of solvent is added, and the mixture is stirred and degassed to obtain the coating liquid.
[0114] (5) The coating liquid is spin-coated onto the surface of photovoltaic glass. Most of the solvent is evaporated at a low temperature of 40°C, and then the temperature is raised to 70°C to remove the residual solvent. The coating is then cured by ultraviolet light and post-baking to form a self-cleaning nano-coating. The post-baking temperature is 100°C and the time is 30 minutes.
[0115] Example 2
[0116] (1) 1.2g of silica-based mesoporous material SBA-15, 1.8g of hollow silica microspheres, 1g of hydrophobically modified nano-ATO, and 0.6g of γ-methacryloyloxypropyltrimethoxysilane were dispersed in 40g of solvent, 0.4g of deionized water was added, the pH of the system was adjusted to 4, and the mixture was stirred at room temperature for 20min to complete the silane pre-hydrolysis; then, the mixture was ultrasonically dispersed and subjected to high-speed shearing to form an inorganic nanoparticle pre-dispersion.
[0117] (2) Mix 20g of 50wt% methacrylate dodecyl fluoroheptyl ester copolymer ethanol dispersion, 3.5g of reactive diluent monomer, 0.3g of HEMA-phosphate ester, 0.3g of photoinitiator and 0.2g of bis(1-octoxy-2,2,6,6-tetramethyl-4-piperidinyl) sebacate to form a photocurable resin matrix;
[0118] The reactive diluent monomer is a compound of dodecyl methacrylate and trimethylolpropane triacrylate in a mass ratio of 2.5:1.
[0119] The photoinitiator is a compound of acylphosphine oxide (TPO) and amine co-initiator (EDAB) in a mass ratio of 2:1.
[0120] (3) 1.5g of coated nano-titanium dioxide and 0.5g of modified PMMA diffusion particles prepared in Preparation Example 1 were dispersed in 8g of solvent and ultrasonically formed into functional particle slurry under light-protected conditions;
[0121] (4) Under light-protected conditions, the pre-dispersed liquid from step (1) is mixed with the resin matrix from step (2), and the functional particle slurry from step (3) is added. The remaining 32g of solvent is added, and the mixture is stirred and degassed to obtain the coating liquid.
[0122] (5) The coating liquid is spin-coated onto the surface of photovoltaic glass. Most of the solvent is evaporated at a low temperature of 40°C, and then the temperature is raised to 70°C to remove the residual solvent. The coating is then cured by ultraviolet light and post-baking to form a self-cleaning nano-coating. The post-baking temperature is 100°C and the time is 30 minutes.
[0123] Example 3
[0124] (1) 1.5g of silica-based mesoporous material SBA-15, 2g of hollow silica microspheres, 1.2g of hydrophobically modified nano-ATO, and 0.7g of γ-methacryloyloxypropyltrimethoxysilane were dispersed in 40g of solvent, 0.4g of deionized water was added, the pH of the system was adjusted to 4, and the mixture was stirred at room temperature for 20min to complete the silane pre-hydrolysis; then, the mixture was ultrasonically dispersed and subjected to high-speed shearing to form an inorganic nanoparticle pre-dispersion.
[0125] (2) Mix 24g of 50wt% methacrylate dodecyl fluoroheptyl ester copolymer ethanol dispersion, 4g of reactive diluent monomer, 0.5g of HEMA-phosphate ester, 0.4g of photoinitiator and 0.5g of bis(1-octoxy-2,2,6,6-tetramethyl-4-piperidinyl) sebacate to form a photocurable resin matrix;
[0126] The reactive diluent monomer is a compound of dodecyl methacrylate and trimethylolpropane triacrylate in a mass ratio of 2.5:1.
[0127] The photoinitiator is a compound of acylphosphine oxide (TPO) and amine co-initiator (EDAB) in a mass ratio of 2:1.
[0128] (3) 2g of coated nano-titanium dioxide and 0.9g of modified PMMA diffusion particles prepared in Preparation Example 1 were dispersed in 8g of solvent and ultrasonically formed into functional particle slurry under light-protected conditions;
[0129] (4) Under light-protected conditions, the pre-dispersed liquid from step (1) is mixed with the resin matrix from step (2), and the functional particle slurry from step (3) is added. The remaining 32g of solvent is added, and the mixture is stirred and degassed to obtain the coating liquid.
[0130] (5) The coating liquid is spin-coated onto the surface of photovoltaic glass. Most of the solvent is evaporated at a low temperature of 40°C, and then the temperature is raised to 70°C to remove the residual solvent. The coating is then cured by ultraviolet light and post-baking to form a self-cleaning nano-coating. The post-baking temperature is 100°C and the time is 30 minutes.
[0131] Example 4
[0132] The difference between this embodiment and Example 1 is that the modified PMMA diffusion particles are replaced with the modified PMMA diffusion particles prepared in Example 2.
[0133] The reactive diluent monomer is a compound of dodecyl methacrylate and trimethylolpropane triacrylate in a mass ratio of 3:1.
[0134] Example 5
[0135] The difference between this embodiment and Example 1 is that the modified PMMA diffusion particles are replaced with the modified PMMA diffusion particles prepared in Example 3.
[0136] The reactive diluent monomer is a compound of dodecyl methacrylate and trimethylolpropane triacrylate in a mass ratio of 2.8:0.5.
[0137] Example 6
[0138] The difference between this embodiment and Example 2 is that the modified PMMA diffusion particles are replaced with the modified PMMA diffusion particles prepared in Example 3.
[0139] The photoinitiator is a compound of acylphosphine oxide (TPO) and amine co-initiator (EDAB) in a mass ratio of 2:1.
[0140] Comparative Example 1
[0141] The difference between this comparative example and Example 1 is that no modified PMMA diffusion particles are added.
[0142] Comparative Example 2
[0143] The difference between this comparative example and Example 1 is that the modified PMMA diffusion particles are replaced with an equal amount of PMMA particles that have not undergone surface double bond grafting (i.e., cross-linked PMMA seed particles that have only completed step S1 and whose surface contains only hydroxyl groups).
[0144] The remaining components, proportions, and process conditions are exactly the same as in Example 1.
[0145] Comparative Example 3
[0146] The difference between this comparative example and Example 1 is that the modified PMMA diffusion particles are replaced with an equal amount of the same modified PMMA diffusion particles with an average particle size of 350 nm.
[0147] The remaining steps and all components, proportions and process conditions in Example 1 are exactly the same.
[0148] Comparative Example 4
[0149] The difference between this comparative example and Example 1 is that the coated nano titanium dioxide in Example 1 is replaced with commercially available nano titanium dioxide, which was purchased from Suzhou Jixin Trading Co., Ltd., CAS No.: 1317-80-2.
[0150] Comparative Example 5
[0151] The difference between this comparative example and Example 1 is that the silicon-based mesoporous material SBA-15 was not modified with fluorosilane for full-surface hydrophobicity.
[0152] Comparative Example 6
[0153] The difference between this comparative example and Example 1 is that the hydrophobically modified nano-ATO is replaced with commercially available tin-antimony oxide, purchased from Shanghai Pantian Powder Materials Co., Ltd., with the product number PT-ATO-20nm.
[0154] Performance testing: The coatings obtained in Examples 1-6 and Comparative Examples 1-6 were subjected to various performance tests. The results are shown in Table 1. The test methods are as follows:
[0155] 1. Initial water contact angle: Using a contact angle meter, 2 μL of deionized water was dropped onto the coating surface at room temperature, and the contact angle was measured after standing for 10 seconds. Five different locations were measured for each sample, and the average value was calculated.
[0156] 2. Water contact angle after UV aging: The coating sample was placed in a UV aging test chamber under a UVA-340 lamp with an irradiance of 0.68 W / m². 2 After aging for 500h and 1000h at 60℃ and 50% relative humidity, the samples were taken out and the water contact angle after UV aging was tested according to the initial water contact angle test method.
[0157] 3. Transmittance: Using a UV-Vis spectrophotometer, with uncoated photovoltaic glass as a reference, the absolute transmittance of the coated sample was tested, and the average transmittance in the wavelength range of 380~500nm was taken.
[0158] 4. Haze: According to GB / T 2410-2008 "Determination of light transmittance and haze of transparent plastics", the haze of the coating samples was tested using a haze meter. Five different locations were measured for each sample, and the average value was calculated.
[0159] 5. Outdoor natural dust accumulation rate: The transmittance attenuation method was adopted: the sample was naturally exposed outdoors at a 45° angle for 30 days, and the visible light transmittance before and after dust accumulation was tested. The degree of dust accumulation was characterized by the percentage decrease in transmittance.
[0160] 6. Solvent immersion adhesion: First, according to GB / T9286-1998, the sample is divided into sections, then immersed in anhydrous ethanol at 25℃ for 24 hours, taken out and dried, and then evaluated according to GB / T9286-1998 again. Grade 0 is the best and grade 5 is the worst.
[0161] Table 1
[0162] Test Items Initial water contact angle / ° Water contact angle after 500 hours of UV aging / ° Water contact angle / ° after 1000h of UV aging Average transmittance (%) of 380~500nm Haze / % Outdoor natural dust accumulation rate / % Solvent immersion adhesion Example 1 128 115 105 94.5 0.5 1.5 Level 0 Example 2 125 112 103 94.2 0.6 1.6 Level 0 Example 3 123 114 105 94.3 0.6 1.7 Level 0 Example 4 122 113 103 94.1 0.5 1.8 Level 0 Example 5 126 118 108 94.2 0.7 1.6 Level 0 Example 6 124 114 105 94.4 0.6 1.5 Level 0 Comparative Example 1 123 110 94 93.5 0.3 1.8 Level 0 Comparative Example 2 118 98 87 93.2 0.8 3.3 Level 1 Comparative Example 3 115 103 90 89.7 4.1 3.7 Level 1 Comparative Example 4 102 85 74 85.1 1.2 4.2 Level 2 Comparative Example 5 118 96 84 92.5 0.9 3.5 Level 1 Comparative Example 6 106 92 81 91.3 1.3 3.9 Level 1
[0163] In summary, a comparison between Comparative Example 2 and Example 1 shows that this invention overcomes the technical bias of ordinary organic diffusion particles migrating and precipitating after being added to the coating, thus degrading long-term weather resistance, by using surface covalently grafted modified PMMA diffusion particles. Comparative Example 1 demonstrates that, while maintaining basic properties such as hydrophobicity, weather resistance, adhesion, and dust prevention, the introduction of covalently bonded modified PMMA diffusion particles achieves optical gain and significantly improves the coating's long-term UV aging resistance. Through precise particle size control and surface double-bond covalent grafting structural design, this invention resolves a long-standing technical challenge in the field.
[0164] Modified PMMA diffused particles are covalently bonded into the coating's cross-linked network via surface double bonds, forming stress-buffered microdomains with a certain degree of toughness. This effectively inhibits particle migration and coating structure degradation during UV aging, significantly improving the coating's long-term UV resistance. When the coating is subjected to long-term outdoor exposure to alternating temperature changes, UV radiation, and wind and sand, these elastic microdomains absorb and dissipate stress through deformation, preventing the initiation and propagation of microcracks. Coatings without particles or with only physically filled particles will gradually fail under long-term stress due to the accumulation of microcracks.
[0165] In Comparative Example 2, after 1000 hours of UV aging, the water contact angle decreased to 87°, a significantly greater decrease than in Example 1. During the curing stage, microscopic interface defects had already formed due to differences in interfacial compatibility between the two phases. During UV aging, accompanied by resin micro-degradation and molecular chain thermal motion, these defects gradually expanded, and particles easily migrated and precipitated onto the coating surface, disrupting the uniform distribution of fluorine and leading to a rapid decline in hydrophobic properties. Simultaneously, the interfacial voids between particles and the matrix increased light scattering loss and reduced transmittance; these interface defects also became channels for water molecules and oxygen to permeate, accelerating the oxidative degradation of the resin matrix and further weakening the coating's weather resistance and antifouling capabilities.
[0166] In Comparative Example 3, the average particle size of PMMA particles increased from 100nm to 350nm. Particles with a diameter of 350nm cannot be completely embedded within the coating and will partially protrude from the film surface, resulting in a significant decrease in light transmittance and increased outdoor dust accumulation. Simultaneously, the large-diameter particles induce strong Mie scattering. For photovoltaic systems reliant on direct sunlight, a large amount of direct light is converted into diffuse light, increasing the coating haze from 0.5% to over 4%, thus increasing scattering loss and reducing the light utilization efficiency of the photovoltaic module.
[0167] Comparative Example 4 replaced the coated nano-titanium dioxide in Example 1 with commercially available nano-titanium dioxide, which lacked a silica coating layer and an outer hydrophobic silane graft, and was directly exposed to the organic resin matrix. This resulted in a sharp decrease in the water contact angle after UV aging. The absence of a SiO2 barrier layer caused rapid aging and yellowing of the matrix, and a significant degradation in hydrophobic properties. Furthermore, the resin degraded, losing some of its binding force to the functional particles, leading to a significant decrease in coating adhesion.
[0168] Comparative Example 5 shows that because the silicon-based mesoporous material SBA-15 did not use fluorosilane for full-surface hydrophobic modification, the overall hydrophobic performance of the coating was reduced, and the initial water contact angle decreased significantly. Furthermore, the hydrophilic channels accumulated water due to capillary condensation outdoors, and the salts and pollutants dissolved in the water remained in the channels, which led to a decrease in light transmittance over a long period of time.
[0169] Comparative Example 6 replaced the hydrophobically modified nano-ATO with commercially available tin-antimony oxide. The ATO surface was not modified with silane hydrophobicity, retaining a large number of hydrophilic hydroxyl groups. The initial water contact angle decreased significantly. The introduction of hydrophilic ATO formed hydrophilic sites on the coating surface, disrupting the continuity of the low surface energy fluoropolymer enrichment layer. Furthermore, the hydrophilic ATO became a water vapor adsorption center, accelerating the interfacial degradation of the surrounding resin under the synergistic effect of UV aging, thus leading to a further decrease in the water contact angle after UV aging.
[0170] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.
Claims
1. A self-cleaning nano-coating material for photovoltaic modules, characterized in that, The nano-coating material is made from the following raw materials in parts by weight: The composition includes: 0.5-1.5 parts of silicon-based mesoporous material, 0.8-2.0 parts of coated nano-titanium dioxide, 1.5-2.0 parts of hollow silica microspheres, 10-12 parts of fluorinated acrylic resin, 3-4 parts of reactive diluent monomer, 0.5-1 part of modified PMMA diffusion particles, 0.5-0.7 parts of silane coupling agent, 0.2-0.5 parts of phosphate ester adhesion promoter, 0.5-1.2 parts of hydrophobically modified nano-ATO, 0.3-0.4 parts of photoinitiator, 0.1-0.5 parts of hindered amine light stabilizer, and 75-80 parts of solvent.
2. The self-cleaning nano-coating material for photovoltaic modules according to claim 1, characterized in that, The silicon-based mesoporous material is SBA-15, with a particle size of 80-150 nm and a pore size of 8-10 nm. The silicon-based mesoporous material is pre-modified with fluorosilane to achieve full-surface hydrophobicity.
3. The self-cleaning nano-coating material for photovoltaic modules according to claim 1, characterized in that, The coated nano-titanium dioxide is silicon dioxide coated with anatase crystals, with a core particle size of 2-3 nm and a coating layer thickness of 3-5 nm. Long-chain hydrophobic silanes are grafted onto the coating layer, and the pure titanium dioxide content is ≥80 wt%.
4. The self-cleaning nano-coating material for photovoltaic modules according to claim 1, characterized in that, The hollow silica microspheres have an average particle size of 55-60 nm, a wall thickness of 8-10 nm, and a visible light transmittance of ≥99%. The fluorinated acrylic resin is a copolymer of dodecafluoroheptyl methacrylate, provided in the form of an ethanol dispersion system with a solid content of 50wt%, and has an intrinsic water contact angle ≥105°.
5. The self-cleaning nano-coating material for photovoltaic modules according to claim 1, characterized in that, The reactive diluent monomer is a compound of dodecyl methacrylate and trimethylolpropane triacrylate in a mass ratio of (2.5-3):(0.5-1).
6. The self-cleaning nano-coating material for photovoltaic modules according to claim 1, characterized in that, The phosphate adhesion promoter is HEMA-phosphate; The hydrophobically modified nano-ATO is a tin-antimony oxide modified with silane hydrophobicity, with a particle size of 20-30 nm; The hindered amine light stabilizer is selected as bis(1-octoxy-2,2,6,6-tetramethyl-4-piperidinyl) sebacate.
7. The self-cleaning nano-coating material for photovoltaic modules according to claim 1, characterized in that, The photoinitiator is a compound of acylphosphine oxide (TPO) and amine co-initiator (EDAB) in a mass ratio of 2-4:
1.
8. The self-cleaning nano-coating material for photovoltaic modules according to claim 1, characterized in that, The method for preparing the modified PMMA diffusion particles includes the following steps: S1. Preparation of nanoscale hydroxy-crosslinked PMMA seed particles Anhydrous ethanol and deionized water were added to the reactor, followed by polyvinylpyrrolidone K30. The mixture was stirred to dissolve and heated while nitrogen was continuously introduced. Methyl methacrylate, hydroxyethyl methacrylate, ethylene glycol dimethacrylate, and azobisisobutyronitrile were then mixed evenly and added to the reaction system in one go. The polymerization reaction was carried out at a constant temperature under nitrogen protection and stirring. After the reaction was completed, the mixture was cooled to room temperature, centrifuged at high speed, washed alternately with anhydrous ethanol and deionized water, and dried under vacuum to obtain cross-linked PMMA seed particles with an average particle size of 90-110 nm and a surface rich in hydroxyl groups. S2, Preparation of surface-bonded isocyanate active intermediates The cross-linked PMMA seed particles prepared by S1 were dispersed in anhydrous ethyl acetate and thoroughly ultrasonically dispersed. Isophorone diisocyanate and dibutyltin dilaurate were added, and the system was kept anhydrous and oxygen-free. The reaction was pre-reacted first, and then the temperature was increased to continue the reaction. After the reaction was completed, the free unreacted diisocyanate molecules were removed by centrifugation and washing several times to obtain functionalized PMMA diffusion particle intermediates with partially bonded isocyanate groups on the surface. S3. Stepwise bifunctional grafting preparation of organic-inorganic bireactive modified PMMA diffusion particles All the functionalized PMMA intermediates obtained from S2 were re-dispersed ultrasonically in anhydrous ethyl acetate, and 3-aminopropyltriethoxysilane was slowly added dropwise for reaction. Subsequently, pentaerythritol triacrylate, phenothiazine as a polymerization inhibitor, and dibutyltin dilaurate as a catalyst were added, and the reaction was heated. After the reaction was completed, the particles were centrifuged, washed multiple times with anhydrous ethyl acetate, and dried under vacuum to obtain bireactive modified PMMA diffusion particles with siloxane groups and polyfunctional acrylate double bonds simultaneously bonded to the surface.
9. A method for preparing a self-cleaning nano-coating material for photovoltaic modules as described in any one of claims 1-8, characterized in that, Includes the following steps: (1) The silicon-based mesoporous material, hollow silica microspheres, hydrophobically modified nano-ATO, and silane coupling agent are dispersed in the first part of the solvent according to the weight parts mentioned above. Deionized water is added to adjust the pH of the system, and the silane pre-hydrolysis is completed by stirring at room temperature. Then, an inorganic nanoparticle pre-dispersion liquid is formed by ultrasonic dispersion and high-speed shearing. (2) Fluorine-modified acrylic resin, reactive diluent monomer, phosphate ester adhesion promoter, photoinitiator and hindered amine light stabilizer are mixed to form a photocurable resin matrix; (3) The coated nano-titanium dioxide and modified PMMA diffusion particles are dispersed in the second solvent and ultrasonically formed into a functional particle slurry under light-protected conditions; (4) Under light-protected conditions, the pre-dispersed liquid from step (1) is mixed with the resin matrix from step (2), and the functional particle slurry from step (3) is added. The remaining solvent is added, and the mixture is stirred and mixed evenly and degassed to obtain the coating liquid. (5) The coating liquid is applied to the surface of photovoltaic glass, and after pre-baking, ultraviolet curing and post-baking treatment, a self-cleaning nano-coating is formed.
10. The method for preparing a self-cleaning nano-coating material for photovoltaic modules according to claim 9, characterized in that, The first part of the solvent input is 40-55% of the total solvent mass, and the second part of the solvent input is 5-10%.
Citation Information
Patent Citations
Preparation of superhydrophilic self-cleaning titanium dioxide photocatalytic thin films by modified PTA method
CN109734327B