Transparent self-cleaning coating and preparation method of transparent self-cleaning coating for solar photovoltaic panel

Through the composite technology of fluorine-free modifier-free nanoparticles and resin, a transparent self-cleaning coating with high light transmission and high mechanical properties was prepared, which solved the short service life of photovoltaic panel coatings in harsh environments and high environmental protection costs. The problem has achieved environmentally friendly and low-cost self-cleaning effect.

CN118994980AActive Publication Date: 2024-11-22LANZHOU UNIVERSITY OF TECHNOLOGY

Patent Information

Application Number
CN202410900453.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-11-22
Estimated Expiration
2044-07-05

AI Technical Summary

Technical Problem

The self-cleaning coatings of existing photovoltaic panels have short service life, low light transmittance, poor mechanical properties in harsh environments, and contain a large amount of fluorine, which affects environmental protection and cost.

Method used

Use fluorine-free modifier-free nanoparticles to mix with fluorine-free resin to prepare transparent self-cleaning coatings, and use silicon source, hydrophobic modifier and resin composite resin sol, and combine anti-reflective layer and transparent self-cleaning coating with double layers. The structure forms a self-cleaning coating with high light transmission and high mechanical properties.

Benefits of technology

It achieves high light transmittance, excellent mechanical properties and hydrophobic angle, achieving self-cleaning effect without ash, and is environmentally friendly and low-cost, and is suitable for existing photovoltaic glass.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994980A_ABST
    Figure CN118994980A_ABST
Patent Text Reader

Abstract

The invention provides a transparent self-cleaning coating and a preparation method of a transparent self-cleaning coating for a solar photovoltaic panel, belongs to the technical field of self-cleaning materials, and aims to solve the technical problems of low light transmittance and poor mechanical properties of a self-cleaning film. The preparation method of the transparent self-cleaning coating comprises the following steps: (1) uniformly mixing a silicon source, a hydrophobic modifier, a solvent I and water, and then aging to prepare hydrophobic modified silica sol; (2) dissolving hydroxy acrylic resin, a cross-linking agent and hydrophobic resin into a solvent II to obtain composite resin sol; and (3) diluting the hydrophobic modified silica sol, and then uniformly mixing the diluent with the composite resin sol to prepare the transparent self-cleaning coating. The prepared self-cleaning film is high in light transmittance and excellent in mechanical performance, has a high hydrophobic angle and achieves the dust-free self-cleaning effect. And the fluorine-free modifier is adopted to modify the nanoparticles and is mixed with the fluorine-free resin, so that high weather resistance and wear resistance are achieved, the environment is hardly influenced, and the self-cleaning coating is green, environment-friendly and pollution-free.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of self-cleaning materials, and in particular relates to a method for preparing a transparent self-cleaning coating and a transparent self-cleaning coating for a solar photovoltaic panel. Background Art

[0002] With the rapid development of the photovoltaic industry, many problems have been left behind, especially the cleaning problem of photovoltaic panels is difficult to be properly solved. Every year, dust causes economic losses of more than tens of billions of yuan to the photovoltaic industry, and the cleaning technology of photovoltaic panels is costly and difficult to operate. For this reason, a new type of nano self-cleaning protective coating has gradually appeared on the market for use on solar photovoltaic glass to solve this problem. However, photovoltaic modules are exposed to the outside all year round, and are eroded by rain, wind and sand, which degrades the coating protection and reduces the self-cleaning efficiency. Therefore, what is needed now is a coating that can reduce or even prevent dust accumulation, and can exert its self-cleaning benefits in harsh working environments for a long time without human intervention, and at the same time cannot affect the light transmittance of photovoltaic glass and thus affect the power generation efficiency of photovoltaic modules.

[0003] Patent CN 108358469A discloses a wear-resistant self-cleaning anti-reflection film for solar cells. The wear-resistant self-cleaning anti-reflection film is based on photovoltaic encapsulation glass, and from the side close to the glass to the outside, it is a magnesium fluoride film layer, an inorganic anti-reflection film layer and a high-transmittance self-cleaning coating. The anti-reflection film can improve the transmittance of the encapsulation material, the material has high adhesion, good wear resistance and corrosion resistance, and has certain self-cleaning performance, but the magnesium fluoride coating is evaporated on the glass substrate, which contains a large amount of fluorine elements, is difficult to operate, has high costs, and is not environmentally friendly. The evaporation method can only be used on photovoltaic glass that is about to leave the factory, and cannot be used on existing photovoltaic glass, and its use value is greatly reduced.

[0004] Patent CN 104530852A discloses the preparation of a highly hydrophobic fluorocarbon coating for the backplane of a photovoltaic module, and provides a simple preparation process. Nano-silicon dioxide is uniformly dispersed in the main resin after being hydrophobically modified by a coupling agent, and a micro-nano rough texture structure is formed after being coated on the substrate. Combined with the low surface energy of the fluorocarbon resin itself, the surface has a high hydrophobicity of the "lotus effect", while avoiding the adhesion of dew, rain and water vapor on the surface of the backplane, improving the hydrolysis resistance of the backplane, and having a good anti-fouling effect. However, the patent uses hydrophobic particles to mix with fluorocarbon resin, which is difficult to mix, and the uniformity of the coating is difficult to ensure, which has an adverse effect on the light transmission performance and mechanical properties. In addition, the use of fluorocarbon resin as the main resin contains a large amount of fluorine elements, and uses a variety of organics, which is not conducive to environmental protection and has high costs. Summary of the invention

[0005] In view of the technical problems of low light transmittance and poor mechanical properties of self-cleaning films, the present invention proposes a method for preparing a transparent self-cleaning coating and a transparent self-cleaning coating for solar photovoltaic panels. The self-cleaning film prepared by the method has high light transmittance, excellent mechanical properties, a high hydrophobic angle, and a coating that achieves a dust-free self-cleaning effect. In addition, the nanoparticles are modified with a fluorine-free modifier and mixed with a fluorine-free resin to achieve high weather resistance and wear resistance while having almost no impact on the environment. It is a green, environmentally friendly and pollution-free self-cleaning coating.

[0006] In order to achieve the above object, the technical solution of the present invention is achieved as follows:

[0007] A method for preparing a transparent self-cleaning coating comprises the following steps:

[0008] (1) uniformly mixing a silicon source, a hydrophobic modifier, a solvent I and water, and then aging the mixture to prepare a hydrophobically modified silica sol;

[0009] (2) dissolving the hydroxy acrylic resin, the crosslinking agent and the hydrophobic resin in the solvent II to obtain a composite resin sol;

[0010] (3) The hydrophobically modified silica sol is diluted, and then the diluent, the composite resin sol and the silane coupling agent I are evenly mixed to obtain a transparent self-cleaning coating.

[0011] The silicon source is one or more of methyl orthosilicate, ethyl orthosilicate, methyl triethoxysilane, phenyl trimethoxysilane, n-octyl triethoxysilane, octadecyl triethyl, oxysilane, methoxysilane, ethoxysilane, propoxysilane and butoxysilane; the hydrophobic modifier is hexamethyldisilazane; and the solvent I is one or more of ethanol, methanol, ethyl acetate, toluene, xylene and n-hexane.

[0012] The volume ratio of the silicon source, the hydrophobic modifier, the solvent I and water is 1:(0.5-2):(10-15):(1-2).

[0013] The aging temperature is 35-45° C. and the aging time is 3-14 days.

[0014] The cross-linking agent is an amino resin; the hydrophobic resin is one or more of an organic silicone resin, an MQ methyl silicone resin, a methylphenyl silicone resin and a methylvinyl silicone resin; the solvent II is one or more of ethanol, methanol, ethyl acetate, toluene, xylene and n-hexane; and the silane coupling agent I is γ-aminopropyltriethoxysilane (KH-550).

[0015] The mass ratio of the hydroxy acrylic resin, the crosslinking agent and the hydrophobic resin is 1:(0.5-1):(0.5-3), and the ratio of the hydroxy acrylic resin to the solvent II is 10-50 g / mL.

[0016] The diluent used to dilute the hydrophobically modified silica sol in step (3) is solvent I, and the volume ratio of the diluent to the hydrophobically modified silica sol is (3-5):1; the mass ratio of the diluent, the composite resin sol and the silane coupling agent I is 1:(0.8-1.2):(0.005-0.01).

[0017] A method for preparing a transparent self-cleaning coating for a solar photovoltaic panel comprises the following steps:

[0018] (1) mixing silane coupling agent II, octadecylamine, polyethylene glycol, ethanol and water to prepare an anti-reflection sol;

[0019] (2) coating the anti-reflection sol onto a substrate, followed by annealing to obtain an anti-reflection layer on the substrate;

[0020] (3) coating the transparent self-cleaning coating on the anti-reflection layer of step (2), and calcining to obtain a transparent self-cleaning coating.

[0021] The mass ratio of the silane coupling agent II, octadecylamine, polyethylene glycol, ethanol and water is 1:0.1:2:20:0.3.

[0022] The silane coupling agent II is γ-glycidyloxypropyltrimethoxysilane (KH-560).

[0023] The substrate is a glass substrate, which is treated with piranha solution before use and dried with nitrogen for later use.

[0024] The piranha solution is prepared by mixing a strong acid and 30% hydrogen peroxide in a ratio of 7:3, wherein the strong acid is one or more of concentrated sulfuric acid and concentrated hydrochloric acid. The treatment steps are to place the cleaned glass substrate in the piranha solution and shake it for 5 minutes, let it stand at a temperature of 60-80°C for 1-2 hours, and then rinse it with a large amount of distilled water after taking it out.

[0025] The annealing temperature in step (2) is 450°C-550°C; the calcination temperature in step (3) is 200°C-250°C.

[0026] Beneficial effects of the present invention:

[0027] (1) The fluorine-free modifier of the present invention modifies the silanol produced by hydrolysis of TEOS, and uses hydrophobically modified silica sol to replace traditional silica powder, thereby avoiding agglomeration in the coating, so that the light transmittance of the transparent self-cleaning coating can reach 85%;

[0028] (2) The double-layer composite structure is adopted. The anti-reflection layer of the bottom layer has a positive effect on the transmittance of the transparent self-cleaning coating. The bottom layer and the substrate are bonded by covalent bonds, and the connection is tight, which also increases the adhesion of the transparent self-cleaning coating to the substrate.

[0029] (3) The three resins are compounded in a way that the -COOH in the hydroxylated acrylic resin and the -NH in the amino resin 3 Cross-linking polymerization will occur, and then hydrophobic MQ methyl silicone resin will be introduced to form a composite resin base. The resins will undergo a cross-linking reaction to form a three-dimensional network structure. The hydrophobic groups in the MQ methyl silicone resin will improve the wetting properties of the coating. In addition, the hydroxy acrylic resin and the hydrophobically modified silica sol can further react, and the composite resin will wrap the hydrophobic nanoparticles, greatly increasing the weather resistance and durability of the coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0031] Figure 1 This is the XPS comparison curve of the anti-reflection layer before and after calcination.

[0032] Figure 2 This is a scanning electron microscope photo of the anti-reflection layer.

[0033] Figure 3 Water contact angle for a transparent self-cleaning coating.

[0034] Figure 4 This is the transmittance spectrum of the transparent self-cleaning coating.

[0035] Figure 5 White light interference image of the transparent self-cleaning coating.

[0036] Figure 6 FT-IR spectrum of the transparent self-cleaning coating.

[0037] Figure 7 This is a scanning electron microscope photo of the transparent self-cleaning coating.

[0038] Figure 8 (a) PV curve of the transparent self-cleaning coating, (b) IV curve of the transparent self-cleaning coating.

[0039] Fig. 9(a) PV curve of the film-coated photovoltaic module after dust coating and the blank photovoltaic module, (b) IV curve of the film-coated photovoltaic module after dust coating and the blank photovoltaic module. DETAILED DESCRIPTION

[0040] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] Example 1

[0042] A transparent self-cleaning coating, the preparation method comprising the following steps:

[0043] (1) 8.4 mL of tetraethyl orthosilicate was dissolved in 120 mL of anhydrous ethanol and ultrasonically dispersed for 0.5 h. Then, a mixture of 8 mL of hexamethyldisilazane and 12 mL of high-purity water was added and stirred for 2 h. After aging for one week, a hydrophobically modified SiO 2 sol, all reactions were carried out at 40 °C;

[0044] (2) dispersing 0.88 g of hydroxy acrylic resin, 0.56 g of amino resin and 0.4 g of MQ methyl silicone resin in 30 ml of anhydrous ethanol by high-speed stirring to obtain a composite resin sol;

[0045] (3) The hydrophobic modified sol is diluted with ethanol at a ratio of 1:4, 10 g of the dilution is mixed evenly with 10 g of the composite resin sol, and then 0.1 g of γ-aminopropyltriethoxysilane is added. After sufficient reaction, a transparent self-cleaning coating is prepared for use.

[0046] Example 2

[0047] A transparent self-cleaning coating, the preparation method comprising the following steps:

[0048] (1) 8.4 mL of tetraethyl orthosilicate was dissolved in 120 mL of anhydrous ethanol and ultrasonically dispersed for 0.5 h. Then, a mixture of 8 mL of hexamethyldisilazane and 12 mL of high-purity water was added and stirred for 2 h. After aging for one week, a hydrophobically modified SiO 2 sol, all reactions were carried out at 40 °C;

[0049] (2) dispersing 0.88 g of hydroxy acrylic resin, 0.56 g of amino resin and 0.8 g of MQ methyl silicone resin in 30 ml of anhydrous ethanol by high-speed stirring to obtain a composite resin sol;

[0050] (3) The hydrophobic modified sol is diluted with ethanol at a ratio of 1:4, 10 g of the dilution is mixed evenly with 10 g of the composite resin sol, and then 0.1 g of γ-aminopropyltriethoxysilane is added. After sufficient reaction, a transparent self-cleaning coating is prepared for use.

[0051] Example 3

[0052] A transparent self-cleaning coating, the preparation method comprising the following steps:

[0053] (1) 8.4 mL of tetraethyl orthosilicate was dissolved in 120 mL of anhydrous ethanol and ultrasonically dispersed for 0.5 h. Then, a mixture of 8 mL of hexamethyldisilazane and 12 mL of high-purity water was added and stirred for 2 h. After aging for one week, a hydrophobically modified SiO 2 sol, all reactions were carried out at 40 °C;

[0054] (2) dispersing 0.88 g of hydroxy acrylic resin, 0.56 g of amino resin and 1.2 g of MQ methyl silicone resin in 30 ml of anhydrous ethanol by high-speed stirring to obtain a composite resin sol;

[0055] (3) The hydrophobic modified sol is diluted with ethanol at a ratio of 1:4, 10 g of the dilution is mixed evenly with 10 g of the composite resin sol, and then 0.1 g of γ-aminopropyltriethoxysilane is added. After sufficient reaction, a transparent self-cleaning coating is prepared for use.

[0056] Example 4

[0057] A transparent self-cleaning coating, the preparation method comprising the following steps:

[0058] (1) 8.4 mL of tetraethyl orthosilicate was dissolved in 120 mL of anhydrous ethanol and ultrasonically dispersed for 0.5 h. Then, a mixture of 8 mL of hexamethyldisilazane and 12 mL of high-purity water was added and stirred for 2 h. After aging for one week, a hydrophobically modified SiO 2 sol, all reactions were carried out at 40 °C;

[0059] (2) dispersing 0.88 g of hydroxy acrylic resin, 0.56 g of amino resin and 1.6 g of MQ methyl silicone resin in 30 ml of anhydrous ethanol by high-speed stirring to obtain a composite resin sol;

[0060] (3) The hydrophobic modified sol is diluted with ethanol at a ratio of 1:4, 10 g of the dilution is mixed evenly with 10 g of the composite resin sol, and then 0.1 g of γ-aminopropyltriethoxysilane is added. After sufficient reaction, a transparent self-cleaning coating is prepared for use.

[0061] Comparative Example 1

[0062] A transparent self-cleaning coating, the preparation method comprising the following steps:

[0063] (1) 8.4 mL of tetraethyl orthosilicate was dissolved in 120 mL of anhydrous ethanol and ultrasonically dispersed for 0.5 h. Then, a mixture of 8 mL of hexamethyldisilazane and 12 mL of high-purity water was added and stirred for 2 h. After aging for one week, a hydrophobically modified SiO 2 sol, all reactions were carried out at 40 °C;

[0064] (2) dispersing 0.88 g of hydroxy acrylic resin and 0.56 g of amino resin in 30 ml of anhydrous ethanol by high-speed stirring to obtain a composite resin sol;

[0065] (3) The hydrophobic modified sol is diluted with ethanol at a ratio of 1:4, 10 g of the dilution is mixed evenly with 10 g of the composite resin sol, and then 0.1 g of γ-aminopropyltriethoxysilane is added. After sufficient reaction, a transparent self-cleaning coating is prepared for use.

[0066] Comparative Example 2

[0067] A transparent self-cleaning coating, the preparation method comprising the following steps:

[0068] (1) 8.4 mL of tetraethyl orthosilicate was dissolved in 120 mL of anhydrous ethanol and ultrasonically dispersed for 0.5 h. Then, a mixture of 8 mL of hexamethyldisilazane and 12 mL of high-purity water was added and stirred for 2 h. After aging for one week, a hydrophobically modified SiO 2 Sol, all reactions were carried out at 40°C; the hydrophobically modified sol was centrifuged, washed with ethanol, and centrifuged three times, and the obtained colloid was placed in a drying oven at 80°C, and finally ground and sieved to obtain hydrophobically modified SiO 2 Particles.

[0069] (2) dispersing 0.88 g of hydroxy acrylic resin, 0.56 g of amino resin and 0.8 g of MQ methyl silicone resin in 30 ml of anhydrous ethanol by high-speed stirring to obtain a composite resin sol;

[0070] (3) 0.35 g of hydrophobically modified nano-SiO 2 Disperse 10 g of nano-SiO in 30 mL of ethanol. 2 The dispersion was mixed evenly with 10 g of composite resin sol, and 0.1 g of KH-550 was added to react fully to obtain a transparent self-cleaning coating for use.

[0071] Example 5

[0072] A transparent self-cleaning coating for a solar photovoltaic panel, the preparation method comprising the following steps:

[0073] (1) 5.75 mL of silane coupling agent KH-560 was added dropwise to 92 mL of anhydrous ethanol and stirred at 35° C. for 1 h. Subsequently, 2.3 mL of high-purity water and 0.69 g of octadecylamine were added and stirred for 0.5 h. Finally, 10 g of polyethylene glycol 1500 was added and stirred for two hours to obtain an anti-reflection sol.

[0074] (2) Place the glass slide in a piranha solution (98% concentrated sulfuric acid: 30% hydrogen peroxide = 3:1), heat it to keep the temperature at 70°C, react for 1 hour, take it out and rinse it with a large amount of distilled water, finally blow away the residual moisture on the surface with nitrogen gas, and place it in a 40°C oven for later use;

[0075] (3) The anti-reflection sol is coated on the treated glass substrate and annealed at high temperature to obtain a substrate with an anti-reflection layer. The transparent self-cleaning coating prepared in Example 1 is evenly coated on the bottom layer and calcined at high temperature to form a transparent self-cleaning coating. The prepared sample is recorded as a.

[0076] Technical mechanism:

[0077] The present invention first uses piranha solution to hydroxylate the glass surface, so that the surface is rich in -OH functional groups; the anti-reflection layer is then calcined at high temperature to cause PEG to crack and volatilize to form a porous structure, thereby increasing the light transmittance of the coating; at the same time, KH-560 and ODA react after ring opening to form a three-dimensional network structure, thereby increasing the stability of the coating; the -OH after ring opening reacts with the -OH group on the glass surface to undergo dehydration condensation, thereby increasing the adhesion between the coating and the glass; the -COOH in the hydroxylated acrylic resin in the top layer reacts with the -NH 3 At the same time, the terminal hydroxyl groups in the hydroxylated acrylic resin react with the -OH in the silanol produced by the hydrolysis of TEOS to form a covalent bond, making the nano-SiO 2 The particles are better coated and have excellent stability. The hydrophobic MQ methyl silicone resin is introduced to form a suitable resin base, which neutralizes the hydrophilic properties of the excess hydroxyl and amino groups produced after the resin is compounded, thereby increasing the hydrophobic properties of the coating. The three resins work together to play a positive role in the stability, mechanical properties and self-cleaning properties of the coating. Under the action of KH-550, the organic and inorganic are better combined by combining with the hydrolyzed silanol to form a self-cleaning coating material for solar photovoltaic panels.

[0078] Example 6

[0079] The difference from Example 5 is that the transparent self-cleaning coating is prepared using the transparent self-cleaning coating prepared in Example 2, and other conditions are the same. The prepared sample is recorded as b.

[0080] Example 7

[0081] The difference from Example 5 is that the transparent self-cleaning coating is prepared by using Example 3, and other conditions are the same. The prepared sample is recorded as c.

[0082] Example 8

[0083] The difference from Example 5 is that the transparent self-cleaning coating is prepared using Example 4, and other conditions are the same. The prepared sample is recorded as d.

[0084] Comparative Example 3

[0085] The difference from Example 5 is that the transparent self-cleaning coating is prepared by using Comparative Example 1, and other conditions are the same. The prepared sample is recorded as e.

[0086] Comparative Example 4

[0087] The difference from Example 5 is that the transparent self-cleaning coating is prepared by using the self-cleaning coating prepared in Comparative Example 2, and other conditions are the same. The prepared sample is recorded as f.

[0088] Samples af prepared in the above Examples 5-8 and Comparative Examples 3 and 4 were characterized and compared with bare glass.

[0089] 1. XPS analysis of anti-reflection layer

[0090] XPS test was performed on the anti-reflection layer in Example 5 before and after calcination. PEG-1500 was used as a pore-forming agent in the bottom anti-reflection solution. The coated sample was calcined at 500°C to crack the carbon chain structure of PEG and volatilize into gas. Figure 1 It can be seen that the content of C element before calcination is greater than that of Si and O. After calcination, the C content is greatly reduced and the O content is increased compared with that before calcination, which indicates that C is oxidized and volatilized into gas during calcination, and the remaining elements continue to react with KH-560 and ODA, thus forming a dense three-dimensional network structure with a large number of pore structures.

[0091] 2. Scanning electron microscopy analysis of anti-reflection layer

[0092] After the anti-reflection layer in Example 5 is annealed, Figure 2 From the SEM image of the anti-reflection layer, it can be seen that there are a large number of pore structures in the coating. Because of the existence of the pore structure, it can increase the refractive index of light, thereby reducing the reflectivity of light and then increasing the transmittance of light. This is also an important reason why the transmittance of the anti-reflection layer is higher than that of bare glass. Therefore, the effect of using the anti-reflection layer to improve the transmittance of the hydrophobic coating is obvious.

[0093] 3. Surface wetting properties of self-cleaning coatings

[0094] In order to explore the hydrophobic properties of the self-cleaning coating, this experiment used a contact angle meter to measure the contact angle of water droplets on coatings with different ratios. Specifically, a drop of deionized water was dropped on three locations on the sample surface using a needle, and the average contact angle was taken. By observing and analyzing the contact angle between the water droplet and the coating surface, the performance of the hydrophobic coating on the sample surface was characterized. Figure 3 As shown in the figure, different contents of MQ methyl silicone resin show different contact angles. As the content of MQ methyl silicone resin increases, the contact angle of the coating reaches a maximum of 133.1° when the content is 0.8g. Then, as the content of the resin continues to increase, the contact angle gradually decreases. This is because when the resin content increases to a certain level, when its content continues to increase, the spreading speed of water droplets on the coating surface is accelerated. At the same time, as the content increases, the surface roughness of the coating decreases, which in turn causes the contact angle to decrease. When using traditional nano-SiO2 particles, the contact angle of the coating decreases, such as Figure 3 As shown in sample f, the nanoparticles are unstable during further dispersion and agglomerate, and are unable to exhibit their hydrophobic properties when wrapped with resin.

[0095] 4. Analysis of light transmission performance of self-cleaning coating

[0096] This test used a UV-Vis-NIR spectrophotometer to measure the transmittance of a series of hydrophobic coatings with different ratios at room temperature. The wavelength range used was 300-1100nm, and the instrument was calibrated with air as the reference and the transmittance was 100%. Figure 4 The following is the transmittance spectrum of hydrophobic coatings with different contents of MQ methyl silicone resin. This experiment mainly prepares hydrophobic coatings on photovoltaic glass substrates and then studies their light transmittance. During the test, special attention was paid to the effect of different contents of MQ methyl silicone resin on the light transmittance of the coating in the visible light range, and samples with good light transmittance were screened out.

[0097] Effects of different contents of MQ methyl silicone resin on the transmittance of coatings Figure 3-5 As shown, from Figure 4It can be seen that the transmittance of 0.8g, 1.2g, and 1.6g MQ methyl silicone resin is only about 80%, which is 10% lower than the transmittance of bare glass. When the MQ methyl silicone resin content is 0.4g, the transmittance is moderate, about 85%, and when there is no MQ methyl silicone resin, the transmittance reaches the best, which is 90%, which is close to the transmittance of bare glass. Since the adhesion of the coating is improved after the addition of MQ methyl silicone resin, it will affect the transmittance, which will lead to a certain degree of decrease in the transmittance of the coating. The transmittance of the best hydrophobic materials containing 0.4g and 0.8g MQ methyl silicone resin reached 85% and 80%, achieving the effect of taking into account both hydrophobicity and transmittance.

[0098] 5. Surface roughness analysis

[0099] like Figure 5 The plane and 3D images of the coating roughness are shown. The coatings with MQ methyl silicone resin addition amounts of 0g, 0.4g, 0.8g, 1.2g, and 1.6g were tested respectively. This method utilizes the Michelson interference principle, uses white light as the light source, and uses a white light interferometer to test the roughness of the coating. As shown in the figure, there are micro-nano-level bulges in the ab figure. From the 3D graphics of the sample, it can be seen that due to the presence of tight bulges on the surface of the sample, the coating has a certain rough structure, which makes the coating have water repellency to droplets. It can be seen from the figure that the roughness (Ra) value of a is 29nm, while the Ra value of c is 64nm. From the discussion of the contact angle above, it is known that the water contact angle of c is greater than that of a, which further verifies that the roughness has a positive effect on the contact angle of the sample. However, when the content of MQ-Me continues to increase, the contact angle of the coating decreases instead. It can also be concluded from the WLI image that the Ra values ​​of samples d and e are 56nm and 27nm, respectively, and their roughness values ​​decrease, affecting the wettability of the sample to water. In summary, c has the highest Ra value and the best contact angle, which shows that the roughness is proportional to the hydrophobicity of the coating to a certain extent.

[0100] 6. Infrared spectrum analysis of self-cleaning coating

[0101] The transparent self-cleaning coating prepared in Example 6 was measured for infrared, such as Figure 6 As shown in the figure, the chemical composition of the surface of each sample was analyzed by FT-IR spectroscopy. From the curve, it can be seen that at 2966cm -1 and 1400cm -1 The peaks appearing near are due to Si-CH 3 -CH in the bond 3 The bending vibration of the group causes 804cm -1 The peaks appearing nearby are due to Si-CH 3 -CH in the bond3 Rocking and asymmetric deformation vibration of the group. 1022cm -1 and 700cm -1 The peaks appearing nearby are the result of the stretching motion of the Si-O-Si bond and Si-C of the silicone resin. These results indicate that the SiO 2 Most of them are modified by the fluorine-free modifier HMDS, and at the same time, the introduced resin is firmly wrapped in it, making the coating stronger.

[0102] 7. SEM analysis of self-cleaning coatings

[0103] In order to further prove the mechanical properties of the coating, we took scanning electron microscope pictures of sample b, such as Figure 7 As shown in the figure, the nanoparticles are evenly distributed in the flat composite resin, indicating that the nano-silica and the resin have cross-linked, bonded and coated. The resin protects the fragile inorganic nano-silica particles. When subjected to external forces, the coating can have excellent mechanical properties, thereby improving the durability and weather resistance of the coating.

[0104] 8. Pencil hardness of self-cleaning coating

[0105] According to the standard test method of coating performance, the hardness of hydrophobic coating is assessed by whether the coating can be scratched by pencil marks, and the highest hardness (divided into 6B-6H from soft to hard) of the pencil lead that the test coating can bear. The coating hardness prepared by different MQ methyl silicone resin contents is as shown in Table 1, when the content of MQ methyl silicone resin is 0g, the pencil hardness of coating is now 2B along with the increase of binder MQ methyl silicone resin content, the pencil hardness of coating presents a rising trend, when the content of MQ methyl silicone resin reaches 0.8g, the pencil hardness on the hydrophobic coating surface reaches 2H, and now the pencil hardness of coating reaches the highest, which illustrates that in the layer when the content of MQ methyl silicone resin reaches 0.8g, the adhesion of coating reaches the best. And the pencil hardness of comparative example f is HB, illustrating that nanoparticles dissolve again and that large agglomeration occurs, making resin coating uneven, and then mechanical property declines.

[0106] Table 1 Pencil hardness values ​​of transparent self-cleaning coatings

[0107] Sample No. a b c d e f Pencil hardness value HB 2H 3B 4B 2B HB

[0108] 9. Performance test of self-cleaning coating on photovoltaic modules

[0109] Figure 8The PV (a) and IV curves (b) of MQ-Me coatings with different contents. It can be seen from the figure that the open circuit voltages of bare glass and sample e are 5.85V and 5.9V respectively, indicating that the open circuit voltage will increase by 0.8% after the hydrophobic coating is applied. The short circuit currents of bare glass and sample e are 0.186A and 0.1863A respectively, while the maximum output power is 0.825W and 0.83W. It can be seen that after the hydrophobic coating is applied, the short circuit current, open circuit voltage and maximum output power are improved to a certain extent. The main reason is that the anti-reflective coating applied increases the transmittance due to its anti-reflective properties, which enables the component to receive more light sources and generate more photogenerated carriers to increase the current. Since the coating has a weak effect on the output voltage, the output current is increased while the output power of the module is also increased.

[0110] from Figure 8 It can also be seen that with the increase of the content of MQ methyl silicone resin, the short-circuit current, open-circuit voltage and maximum output power of the coating have a small decrease, especially for S5, the open-circuit voltage is 4.2% lower than that of S1. Therefore, it can be seen that MQ methyl silicone resin has a certain influence on the light transmittance of the coating, resulting in a decrease in the light source received by the solar cell. Therefore, fewer photogenerated carriers lead to a corresponding decrease in current and power.

[0111] In addition, the coating with sample number b was used to coat the photovoltaic glass panels and blank photovoltaic glass panels with dust to study the effect of dust on photovoltaic modules. Fig. 9 As mentioned above, by comparison, it can be found that after the photovoltaic module is covered with dust, the maximum output power of the film-coated photovoltaic module is 0.95247W, while the maximum output power of the blank photovoltaic module is 0.94369W, and at this time, the short-circuit current of the film-coated photovoltaic module is also higher than that of the blank glass module. This shows that after the hydrophobic coating is applied, the photovoltaic glass obviously has dust-repelling properties. This is because the coating surface has a rough micro-nano structure, which reduces the adhesion between the dust and the coating, and the dust is more easily removed by gravity or wind. At the same time, the coating surface has low surface energy, and it is more difficult for dust to stay on the surface of the photovoltaic module, so that the coating can still maintain a good light transmittance, so that more sunlight is absorbed, and more photogenerated carriers can be generated, so that the output power is higher than that of the blank photovoltaic module.

[0112] Example 9

[0113] A transparent self-cleaning coating, the preparation method comprising the following steps:

[0114] (1) 10 mL of methyltriethoxysilane was dissolved in 120 mL of anhydrous ethanol and ultrasonically dispersed for 0.5 h. Then, a mixture of 5 mL of hexamethyldisilazane and 10 mL of high-purity water was added and stirred for 2 h. After aging for two weeks, a hydrophobically modified SiO 2 Sol, all reactions were carried out at 35 °C;

[0115] (2) dispersing 1 g of hydroxy acrylic resin, 0.5 g of amino resin and 0.5 g of methylphenyl silicone resin in 10 ml of anhydrous ethanol by high-speed stirring to obtain a composite resin sol;

[0116] (3) The hydrophobic modified sol is diluted with ethanol at a ratio of 1:5, 10 g of the dilution is mixed evenly with 10 g of the composite resin sol, and then 0.1 g of γ-aminopropyltriethoxysilane is added. After sufficient reaction, a transparent self-cleaning coating is prepared for use.

[0117] Example 10

[0118] A transparent self-cleaning coating, the preparation method comprising the following steps:

[0119] (1) 10 mL of methoxysilane was dissolved in 100 mL of anhydrous ethanol and ultrasonically dispersed for 0.5 h. Then, a mixture of 20 mL of hexamethyldisilazane and 20 mL of high-purity water was added and stirred for 2 h. After aging for 3 days, a hydrophobically modified SiO 2 sol, all reactions were carried out at 45 °C;

[0120] (2) dispersing 1 g of hydroxy acrylic resin, 1 g of amino resin and 0.8 g of methylphenyl silicone resin in 50 ml of anhydrous ethanol by high-speed stirring to obtain a composite resin sol;

[0121] (3) The hydrophobic modified sol is diluted with ethanol at a ratio of 1:3, 20 g of the dilution is mixed evenly with 24 g of the composite resin sol, and then 0.1 g of γ-aminopropyltriethoxysilane is added. After sufficient reaction, a transparent self-cleaning coating is prepared for use.

[0122] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a transparent self-cleaning coating, characterized in that: The following steps are involved: (1) uniformly mixing a silicon source, a hydrophobic modifier, a solvent I and water, and then aging the mixture to prepare a hydrophobically modified silica sol; (2) dissolving the hydroxy acrylic resin, the crosslinking agent and the hydrophobic resin in the solvent II to obtain a composite resin sol; (3) The hydrophobically modified silica sol is diluted, and then the diluent, the composite resin sol and the silane coupling agent I are evenly mixed to obtain a transparent self-cleaning coating.

2. The method for preparing the transparent self-cleaning coating according to claim 1, characterized in that: The silicon source is one or more of methyl orthosilicate, ethyl orthosilicate, methyl triethoxysilane, phenyl trimethoxysilane, n-octyl triethoxysilane, octadecyl triethyl, oxysilane, methoxysilane, ethoxysilane, propoxysilane and butoxysilane; the hydrophobic modifier is hexamethyldisilazane; and the solvent I is one or more of ethanol, methanol, ethyl acetate, toluene, xylene and n-hexane.

3. The method for preparing the transparent self-cleaning coating according to claim 2, characterized in that: The volume ratio of the silicon source, the hydrophobic modifier, the solvent I and water is 1:(0.5-2):(10-15):(1-2).

4. The method for preparing the transparent self-cleaning coating according to claim 3, characterized in that: The aging temperature is 35-45° C. and the aging time is 3-14 days.

5. The method for preparing the transparent self-cleaning coating according to claim 4, characterized in that: The cross-linking agent is an amino resin; the hydrophobic resin is one or more of an organic silicone resin, an MQ methyl silicone resin, a methylphenyl silicone resin and a methylvinyl silicone resin; the solvent II is one or more of ethanol, methanol, ethyl acetate, toluene, xylene and n-hexane; and the silane coupling agent I is γ-aminopropyltriethoxysilane.

6. The method for preparing the transparent self-cleaning coating according to claim 5, characterized in that: The mass ratio of the hydroxy acrylic resin, the crosslinking agent and the hydrophobic resin is 1:(0.5-1):(0.5-3), and the ratio of the hydroxy acrylic resin to the solvent II is 10-50 g / mL.

7. The method for preparing the transparent self-cleaning coating according to claim 6, characterized in that: The diluent used to dilute the hydrophobically modified silica sol in step (3) is solvent I, and the volume ratio of the diluent to the hydrophobically modified silica sol is (3-5):1; the mass ratio of the diluent, the composite resin sol and the silane coupling agent I is 1:(0.8-1.2):(0.005-0.01).

8. A method for preparing a transparent self-cleaning coating for a solar photovoltaic panel, characterized in that: The following steps are involved: (1) mixing silane coupling agent II, octadecylamine, polyethylene glycol, ethanol and water to prepare an anti-reflection sol; (2) coating the anti-reflection sol onto a substrate, followed by annealing to obtain an anti-reflection layer on the substrate; (3) coating the transparent self-cleaning coating on the anti-reflection layer of step (2), and calcining to obtain a transparent self-cleaning coating.

9. The method for preparing the transparent self-cleaning coating for solar photovoltaic panels according to claim 8, characterized in that: The mass ratio of the silane coupling agent II, octadecylamine, polyethylene glycol, ethanol and water is 1:0.1:2:20:0.

3.

10. The method for preparing a transparent self-cleaning coating for a solar photovoltaic panel according to claim 9, characterized in that: The annealing temperature in step (2) is 450°C-550°C; the calcination temperature in step (3) is 200°C-250°C.

Citation Information

Patent Citations

  • Anti-reflection and high-transparency super-hydrophobic self-cleaning film and preparation method thereof

    CN108219169A

  • Transparent super-hydrophobic coating and preparation method thereof

    CN112300648A

  • Anticorrosive and clean-keeping nano coating material and preparation method thereof

    CN115505316A

  • Transparent composite compound

    US20100178478A1

  • Coating compositions for hydrophobic films and articles having hydrophobic surfaces

    WO2020226865A1

Cited By

  • Anti-reflection self-cleaning coating for photovoltaic module and preparation method of anti-reflection self-cleaning coating

    CN119752265A

  • Antireflective self-cleaning coating for photovoltaic modules and preparation method thereof

    CN119752265B

  • Photovoltaic glass surface hydrophobic treatment process

    CN120887655A