A corrosion-resistant coating for the surface of the anode steel claws in an aluminum electrolytic cell and its preparation method.

By combining organosilicon resin with hydrophobically modified polyacrylamide and using modified core-shell and sheet fillers, a dense coating is formed, which solves the corrosion problem of anode steel claws in aluminum electrolytic cells in high-temperature electrolyte environments, improves the adhesion and corrosion resistance of the coating, and extends its service life.

CN123107537APending Publication Date: 2026-11-17XINJIANG BINGNENG SCIENCE & TECHNOLOGY RESEARCH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202610959746.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-06-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The existing anti-corrosion coatings for the anode steel claws of aluminum electrolytic cells are prone to corrosion in high-temperature electrolyte environments, resulting in a shortened service life. Existing coating materials are insufficient in terms of corrosion resistance, adhesion, and thermal stability.

Method used

A cross-linked network structure is formed by compounding organosilicon resin with hydrophobic modified polyacrylamide, and modified core-shell filler and modified sheet filler are added to form a dense coating. Combined with corrosion inhibitors and inorganic binders, an organic-inorganic interpenetrating hybrid network is formed, which improves the adhesion and corrosion resistance of the coating.

Benefits of technology

It significantly improves the adhesion and corrosion resistance of the coating, extends the service life of the anode steel claws of the aluminum electrolytic cell, reduces the electrolyte permeability, and enhances the thermal stability and impact resistance of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention discloses an anti-corrosion coating for the surface of the anode steel claws in aluminum electrolytic cells and its preparation method, belonging to the field of coating preparation technology. This invention crosslinks organosilicon resin and hydrophobically modified polyacrylamide into a network structure, then adds a modified core-shell structure filler, and combines chromium oxide and titanium carbide. After carbon encapsulation, an inert filler system is formed, which can effectively block oxygen diffusion and reduce the high-temperature oxidation rate. The formed core-shell structure enhances the thermal stability of the coating. When microcracks appear, the titanium carbide in the core layer is exposed and can chemically bond with the system components, achieving a certain self-healing effect. Mica sheets and graphene are combined, oriented, and interspersed between the modified core-shell structure fillers, extending the penetration path of corrosive media and forming a synergistic effect with corrosion inhibitors, achieving a more significant corrosion resistance effect. Furthermore, mica sheets and graphene with different thickness-to-diameter ratios can form a better interleaving and stacking effect, further enhancing corrosion resistance and impact resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of coating technology, and more specifically, to an anti-corrosion coating for the surface of the anode steel claws of an aluminum electrolytic cell and its preparation method. Background Technology

[0002] Electrolytic claws used in aluminum electrolysis, also known as anode steel claws, are key components in the aluminum electrolysis production process. As they connect the anode carbon block and the guide rod, they are exposed to corrosive electrolytes and oxidizing atmospheres for a long time, making them susceptible to corrosion and leading to a decline in their mechanical properties.

[0003] To address the issue of easy corrosion of anode steel claws, various methods are commonly used, including carbon protective rings, alumina protective rings, and aluminum tube protection. Both carbon and alumina protective rings aim to extend the anode's service life, reduce the number of electrode replacements, decrease the amount of residual anode material, and improve anode utilization. While carbon protective rings offer good protection for anode steel claws, their overall corrosion resistance still needs improvement. For example, Chinese patent application CN104005056A discloses a method for preparing a carbon anode protective coating for electrolytic aluminum, using calcium aluminate cement as a binder, waste electrolyte from aluminum electrolysis production as aggregate, and sodium pyrophosphate, sodium tripolyphosphate, sodium hexametaphosphate, sodium lignosulfonate, and calcium lignosulfonate as additives. However, these additives contain carbon-containing organic matter, which is prone to volatilization at high temperatures, leading to coating cracking. For example, Chinese patent application CN113563056B proposes a coating material for high-temperature oxidation prevention of carbon anodes, composed of the following components: 35-55 wt% inorganic binder, 30-60 wt% composite ceramic filler, 1-10 wt% catalyst, 0-1 wt% sintering agent, and 1-10 wt% toughening agent. This coating material exhibits strong thermal shock resistance, but it is prone to partial oxidation of the anode substrate and has poor corrosion resistance.

[0004] To improve the corrosion resistance of materials, existing technologies have explored corrosion-resistant coatings, such as metal coatings, ceramic coatings, and paint coatings. While metal coatings offer some high-temperature resistance, their adhesion to the substrate is poor, and they are prone to electrochemical corrosion in electrolytic environments, resulting in insufficient corrosion resistance for application requirements. Ceramic coatings are brittle, have poor thermal shock resistance, and are prone to thermal stress cracking, which also affects their application performance. Paint coatings generally have limited resistance to electrolyte corrosion and are prone to powdering after long-term use. Therefore, there is an urgent need to develop an anti-corrosion coating whose corrosion resistance meets application requirements. Summary of the Invention

[0005] Therefore, in order to solve one of the aforementioned technical problems, this invention provides an anti-corrosion coating for the surface of the anode steel claws in an aluminum electrolysis cell and its preparation method. The specific technical solution is as follows: An anti-corrosion coating for the surface of the anode steel claws of an aluminum electrolytic cell, the anti-corrosion coating comprising the following raw materials in parts by weight; The composition includes 35-40 parts of silicone resin, 8-10 parts of hydrophobically modified polyacrylamide, 15-18 parts of potassium silicate, 10-15 parts of sodium silicate, 3-5 parts of polyethylene glycol, 12-20 parts of modified core-shell filler, 8-12 parts of modified flake filler, 1-3 parts of corrosion inhibitor, 1-3 parts of adhesive, 1-2 parts of film-forming agent, 0.1-0.5 parts of defoamer, 3-5 parts of toughening agent, 0.1-0.5 parts of surfactant, 0.5-2 parts of dispersant, and 20-30 parts of solvent.

[0006] Preferably, the preparation method of the modified core-shell structured filler includes the following steps: Chromium oxide and titanium carbide were added to the dispersion, and 3-aminophenol and ammonia were added under stirring. The mixture was ultrasonically dispersed and then formaldehyde was added. The mixture was stirred for 30 to 60 minutes. After drying and calcination, the mixture was cooled to room temperature and modified to obtain the modified core-shell structure filler.

[0007] Preferably, the ratio of chromium oxide, titanium carbide, dispersion, 3-aminophenol, ammonia, and formaldehyde by weight is (1~10):(1~5):100:(50~80):(3~5):(5~10).

[0008] Preferably, the calcination treatment conditions are: heating to 500℃~700℃ at a heating rate of 3℃ / min~8℃ / min, and holding at that temperature for 1h~2h.

[0009] Preferably, the modification process is as follows: the calcined carbon-encapsulated core-shell material is added to a silane coupling agent, stirred at a speed of 50 r / min to 100 r / min for 30 min to 60 min, centrifuged, washed, and dried to obtain the modified core-shell structure filler.

[0010] Preferably, the modified sheet packing is prepared by adding the sheet packing to a silane coupling agent, stirring at a speed of 50 r / min to 100 r / min for 30 min to 60 min, centrifuging, washing, and drying to obtain the modified sheet packing.

[0011] Preferably, the sheet-like filler is a mixture of mica sheets and graphene; The mass ratio of the mica sheet to the graphene is (1~8):(1~10). The mica sheet has a thickness of 0.1μm to 0.5μm and a diameter of 20μm to 100μm. The graphene has a thickness of 1 nm to 30 nm and a particle size of 1 μm to 40 μm.

[0012] Preferably, the corrosion inhibitor is at least one selected from sodium hydroxide, potassium hydroxide, calcium hydroxide, and aluminum hydroxide.

[0013] Preferably, the binder is at least one of silica sol, sodium silicate, and potassium silicate.

[0014] In addition, the present invention also provides a method for preparing an anti-corrosion coating for the surface of the anode steel claws of an aluminum electrolytic cell, the preparation method comprising the following steps: Add the silicone resin to the solvent and stir at 300r / min~500r / min for 10min~15min. Then add the hydrophobically modified polyacrylamide, polyethylene glycol, defoamer and dispersant, and continue stirring for 15min~30min to obtain mixture A. Potassium silicate, sodium silicate and surfactant are mixed and stirred and dispersed at 50℃~65℃ for 10min~30min to obtain mixture B; Add the mixture B to the mixture A, and continue to add the modified core-shell structure filler, modified flake filler, corrosion inhibitor and toughening agent under the stirring condition of 200 r / min to 500 r / min. Stir for 1 h to 3 h, add film-forming agent and binder, and continue stirring for 30 min to 60 min to obtain the anti-corrosion coating for the surface of the anode steel claw of the aluminum electrolytic cell.

[0015] Compared with the prior art, this application has the following beneficial effects: 1. This invention combines organosilicon resin and hydrophobically modified polyacrylamide to form a cross-linked network structure. The amide groups in the hydrophobically modified polyacrylamide form Si-OC bonds with the silanol groups of the organosilicon resin. At the same time, the hydrophobic long chains of the hydrophobically modified polyacrylamide interpenetrate and entangle with the organic side chains of the silicone resin, enhancing toughness and exhibiting superior adhesion. Furthermore, the use of hydrophobic groups can significantly reduce the system permeability and electrolyte adhesion, thereby helping to improve the service life of the coating.

[0016] 2. This invention adds a modified core-shell structure filler, which combines chromium oxide and titanium carbide. After carbon encapsulation, it forms an inert filler system that effectively blocks oxygen diffusion. The resulting core-shell structure enhances the thermal stability of the coating. When microcracks appear, the titanium carbide in the core layer is exposed and can chemically bond with the system components, reducing the occurrence of microcracks in the coating. Mica sheets and graphene are combined, oriented, and interspersed between the modified core-shell structure filler, extending the penetration path of corrosive media and forming a synergistic effect with corrosion inhibitors to achieve a more significant corrosion resistance. Furthermore, mica sheets with different thickness-to-diameter ratios and graphene can form a better interspersed stacking effect, further enhancing corrosion resistance and impact resistance.

[0017] 3. The modified core-shell structure filler and modified sheet filler of this invention are uniformly dispersed in the coating and form chemical bonds with the organosilicon resin in the system. They have the advantages of chemical stability and resistance to sintering, which helps to block the contact between high-temperature gases and the protected substrate, thereby reducing the risk of corrosion.

[0018] 4. This invention uses methylphenyl silicone resin with excellent heat resistance as the organic matrix, and adds potassium silicate and sodium silicate to the system to further fill the coating, forming an organic-inorganic interpenetrating hybrid network, which improves the density, promotes the formation of the glass phase, and enhances the thermal stability and corrosion resistance. Detailed Implementation

[0019] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to its embodiments. It should be understood that the specific embodiments described herein are merely illustrative of the invention and do not limit the scope of protection of the invention.

[0020] Unless otherwise specified, all the raw materials used in this application are commercially available and will not be described further here.

[0021] An anti-corrosion coating for the surface of the anode steel claw of an aluminum electrolytic cell according to one embodiment of the present invention, the anti-corrosion coating comprising the following raw materials in parts by weight; The composition includes 35-40 parts of silicone resin, 8-10 parts of hydrophobically modified polyacrylamide, 15-18 parts of potassium silicate, 10-15 parts of sodium silicate, 3-5 parts of polyethylene glycol, 12-20 parts of modified core-shell filler, 8-12 parts of modified flake filler, 1-3 parts of corrosion inhibitor, 1-3 parts of adhesive, 1-2 parts of film-forming agent, 0.1-0.5 parts of defoamer, 3-5 parts of toughening agent, 0.1-0.5 parts of surfactant, 0.5-2 parts of dispersant, and 20-30 parts of solvent.

[0022] In one embodiment, the silicone resin is a methylphenyl silicone resin.

[0023] In one embodiment, the hydrophobic modified polyacrylamide is prepared as follows: acrylamide, 2-acrylamido-2-methylpropanesulfonic acid, and octylphenol polyoxyethylene ether in a weight ratio of 15:9:5 are added to a stirred tank, nitrogen gas is introduced, and the mixture is stirred and reacted at 40°C for 1 hour to obtain a premix; then, N-hydroxymethylbenzamide (12% by weight of the premix) and hydrochloric acid (1% by weight of the premix) are added, and stirring is continued for 1 hour to obtain the hydrophobic modified polyacrylamide. The introduction of the hydrophobic modified polyacrylamide of this invention endows the coating surface with excellent hydrophobic properties, effectively blocking the wetting and adsorption of liquid electrolytes and water vapor, and helping to reduce the adverse effects of corrosive media on the steel claw surface.

[0024] In one embodiment, the method for preparing the modified core-shell structured filler includes the following steps: Chromium oxide and titanium carbide were added to the dispersion, and 3-aminophenol and ammonia were added under stirring. The mixture was ultrasonically dispersed and then formaldehyde was added. The mixture was stirred for 30 to 60 minutes. After drying and calcination, the mixture was cooled to room temperature and modified to obtain the modified core-shell structure filler.

[0025] In one embodiment, the ratio of chromium oxide, titanium carbide, dispersion, 3-aminophenol, ammonia and formaldehyde by weight is (1~10):(1~5):100:(50~80):(3~5):(5~10).

[0026] In one embodiment, the dispersion is obtained by mixing deionized water and anhydrous ethanol in a volume ratio of (1~3):1.

[0027] In one embodiment, the ultrasonic dispersion time is 20 min to 30 min.

[0028] In one embodiment, the drying process is carried out at a temperature of 60°C to 65°C.

[0029] In one embodiment, the calcination treatment conditions are as follows: heating to 500°C to 700°C at a heating rate of 3°C / min to 8°C / min, and holding at that temperature for 1 hour to 2 hours.

[0030] In one embodiment, the modification process involves adding the calcined carbon-coated core-shell material to a silane coupling agent, stirring at 50-100 rpm for 30-60 minutes, centrifuging, washing, and drying to obtain the modified core-shell structured filler. The modified core-shell structured filler of this invention uses high-hardness, highly chemically inert chromium oxide and titanium carbide as the core, with an external carbon layer and grafted silane coupling agent, effectively hindering the penetration and corrosion of electrolyte molten salts at high temperatures. Furthermore, the silane coupling agent modifies the surface of both fillers, greatly improving the interfacial bonding force between the filler and the resin matrix, preventing peeling due to interfacial defects.

[0031] In one embodiment, the silane coupling agent is at least one selected from 3-aminopropyltriethoxysilane, γ-(2,3-epoxypropoxy)propyltrimethoxysilane, 3-(isobutenoyloxy)propyltrimethoxysilane, and N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane.

[0032] In one embodiment, the amount of the silane coupling agent added accounts for 5% to 8% of the mass of the carbon-coated core-shell material.

[0033] In one embodiment, the average particle size of the modified core-shell structured filler is 20 μm to 100 μm.

[0034] In one embodiment, the modified sheet packing is prepared by adding the sheet packing to a silane coupling agent, stirring at a speed of 50 r / min to 100 r / min for 30 min to 60 min, centrifuging, washing, and drying to obtain the modified sheet packing.

[0035] In one embodiment, when preparing the modified sheet filler, the silane coupling agent is at least one selected from 3-aminopropyltriethoxysilane, γ-(2,3-epoxypropoxy)propyltrimethoxysilane, 3-(isobutenoyloxy)propyltrimethoxysilane, and N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane.

[0036] In one embodiment, the sheet-like filler is a mixture of mica sheets and graphene; The mass ratio of the mica sheet to the graphene is (1~8):(1~10). The mica sheet has a thickness of 0.1μm to 0.5μm and a diameter of 20μm to 100μm. The graphene has a thickness of 1 nm to 30 nm and a particle size of 1 μm to 40 μm.

[0037] In one embodiment, the amount of silane coupling agent added during the preparation of the modified sheet filler is 1% to 5% of the mass of the sheet filler. The modified sheet filler (mica / graphene) of the present invention is stacked layer by layer in the coating to form a dense "maze" barrier, which greatly prolongs the diffusion path of corrosive media.

[0038] In one embodiment, the corrosion inhibitor is at least one selected from sodium hydroxide, potassium hydroxide, calcium hydroxide, and aluminum hydroxide.

[0039] In one embodiment, the binder is at least one of silica sol, sodium silicate, and potassium silicate.

[0040] In one embodiment, the film-forming agent is polyethersulfone.

[0041] In one embodiment, the defoamer is a polysiloxane.

[0042] In one embodiment, the toughening agent is at least one of carboxymethyl cellulose and polyvinyl alcohol. The present invention adds carboxymethyl cellulose and polyvinyl alcohol as toughening agents, and combines them with triethylene glycol to effectively alleviate internal stress caused by resin curing and thermal cycling, thereby improving the flexibility and crack resistance of the coating.

[0043] In one embodiment, the surfactant is a polyoxyethylene fatty alcohol ether.

[0044] In one embodiment, the dispersant is at least one of sodium hexametaphosphate, sodium silicate, sodium tripolyphosphate, and polyvinyl alcohol.

[0045] In one embodiment, the solvent is at least one of n-butanol, toluene, and xylene.

[0046] In addition, the present invention also provides a method for preparing an anti-corrosion coating for the surface of the anode steel claws of an aluminum electrolytic cell, the preparation method comprising the following steps: Add the silicone resin to the solvent and stir at 300r / min~500r / min for 10min~15min. Then add the hydrophobically modified polyacrylamide, polyethylene glycol, defoamer and dispersant, and continue stirring for 15min~30min to obtain mixture A. Potassium silicate, sodium silicate and surfactant are mixed and stirred and dispersed at 50℃~65℃ for 10min~30min to obtain mixture B; Add the mixture B to the mixture A, and continue to add the modified core-shell structure filler, modified flake filler, corrosion inhibitor and toughening agent under the stirring condition of 200 r / min to 500 r / min. Stir for 1 h to 3 h, add film-forming agent and binder, and continue stirring for 30 min to 60 min to obtain the anti-corrosion coating for the surface of the anode steel claw of the aluminum electrolytic cell.

[0047] The anti-corrosion coating prepared by the above method has excellent corrosion resistance and good application performance. When applied to the surface of the anode steel claws of aluminum electrolytic cells, it can reduce the risk of corrosion of the anode steel claws of aluminum electrolytic cells and thus extend their service life.

[0048] The implementation schemes of the present invention will now be described in detail with reference to specific embodiments. Example 1

[0049] A method for preparing an anti-corrosion coating for the surface of the anode steel claws in an aluminum electrolytic cell includes the following steps: Acrylamide, 2-acrylamido-2-methylpropanesulfonic acid, and octylphenol polyoxyethylene ether in a weight ratio of 15:9:5 were added to a stirred tank, nitrogen gas was introduced, and the mixture was stirred and reacted at 40°C for 1 hour to obtain a premix. Then, N-hydroxymethylbenzamide (12% of the premix mass) and hydrochloric acid (1% of the premix mass) were added, and the mixture was stirred for another 1 hour to obtain hydrophobically modified polyacrylamide. By weight, 5 parts of chromium oxide and 5 parts of titanium carbide were added to 100 parts of dispersion (a mixture of deionized water and anhydrous ethanol in a volume ratio of 3:1). Under stirring, 62 parts of 3-aminophenol and 4 parts of ammonia were added, and the mixture was ultrasonically dispersed for 25 min. Then, 8 parts of formaldehyde were added, and the mixture was stirred for 50 min. After drying at 60°C, the temperature was increased to 680°C at a rate of 5°C / min and held for 1 h. After cooling to room temperature, carbon-coated core-shell material was obtained. Then, 7% of the mass of the carbon-coated core-shell material was added to 3-aminopropyltriethoxysilane, and the mixture was stirred at 50 r / min for 60 min. After centrifugation, washing, and drying, the modified core-shell structure filler was obtained. By weight, 5 parts mica sheets and 5 parts graphene were mixed to obtain a mixture. Then, 3% of the mass of the mixture was added to 3-aminopropyltriethoxysilane. The mixture was stirred at 50 r / min for 60 min, centrifuged, washed, and dried to obtain the modified sheet filler. By weight, 37 parts of methylphenyl silicone resin were added to 26 parts of n-butanol and stirred at 300 r / min for 15 min. Then, 10 parts of hydrophobic modified polyacrylamide, 5 parts of polyethylene glycol, 0.5 parts of polysiloxane and 1 part of sodium tripolyphosphate were added and stirred for another 30 min to obtain mixture A. Mix 18 parts potassium silicate, 10 parts sodium silicate and 0.5 parts polyoxyethylene fatty alcohol ether, and stir and disperse at 65°C for 30 min to obtain mixture B; Mixture B is added to mixture A. Under stirring conditions of 300 r / min, 15 parts of modified core-shell structure filler, 10 parts of modified sheet filler, 3 parts of aluminum hydroxide and 5 parts of carboxymethyl cellulose are added. The mixture is stirred for 2 hours. Then, 1 part of polyethersulfone and 3 parts of silica sol are added. The mixture is stirred for another 60 minutes to obtain the anti-corrosion coating for the surface of the anode steel claw of the aluminum electrolytic cell. Example 2

[0050] A method for preparing an anti-corrosion coating for the surface of the anode steel claws in an aluminum electrolytic cell includes the following steps: Acrylamide, 2-acrylamido-2-methylpropanesulfonic acid, and octylphenol polyoxyethylene ether in a weight ratio of 15:9:5 were added to a stirred tank, nitrogen gas was introduced, and the mixture was stirred and reacted at 40°C for 1 hour to obtain a premix. Then, N-hydroxymethylbenzamide (12% of the premix mass) and hydrochloric acid (1% of the premix mass) were added, and the mixture was stirred for another 1 hour to obtain hydrophobically modified polyacrylamide. By weight, 6 parts of chromium oxide and 4 parts of titanium carbide were added to 100 parts of dispersion (a mixture of deionized water and anhydrous ethanol in a volume ratio of 3:1). Under stirring, 58 parts of 3-aminophenol and 3 parts of ammonia were added, and the mixture was ultrasonically dispersed for 20 min. Then, 8 parts of formaldehyde were added, and the mixture was stirred for 40 min. After drying at 60°C, the temperature was increased to 680°C at a heating rate of 4°C / min and held for 1 h. After cooling to room temperature, carbon-coated core-shell material was obtained. Then, 3-aminopropyltriethoxysilane, accounting for 8% of the mass of the carbon-coated core-shell material, was added, and the mixture was stirred at 50 r / min for 60 min. After centrifugation, washing, and drying, the modified core-shell structure filler was obtained. By weight, 5 parts mica sheets and 5 parts graphene were mixed to obtain a mixture. Then, 4% of the mass of the mixture was added to 3-aminopropyltriethoxysilane. The mixture was stirred at 50 r / min for 60 min, centrifuged, washed, and dried to obtain the modified sheet filler. By weight, 36 parts of methylphenyl silicone resin were added to 25 parts of n-butanol and stirred at 300 r / min for 15 min. Then, 10 parts of hydrophobic modified polyacrylamide, 5 parts of polyethylene glycol, 0.5 parts of polysiloxane and 0.8 parts of sodium tripolyphosphate were added and stirred for another 20 min to obtain mixture A. Mix 18 parts potassium silicate, 10 parts sodium silicate and 0.3 parts polyoxyethylene fatty alcohol ether, and stir and disperse at 65°C for 20 min to obtain mixture B; Mixture B is added to mixture A. Under stirring conditions of 300 r / min, 15 parts of modified core-shell structure filler, 11 parts of modified sheet filler, 2 parts of aluminum hydroxide and 5 parts of carboxymethyl cellulose are added. The mixture is stirred for 2 hours. Then, 1 part of polyethersulfone and 2 parts of silica sol are added. The mixture is stirred for another 50 minutes to obtain the anti-corrosion coating for the surface of the anode steel claw of the aluminum electrolytic cell. Example 3

[0051] A method for preparing an anti-corrosion coating for the surface of the anode steel claws in an aluminum electrolytic cell includes the following steps: Acrylamide, 2-acrylamido-2-methylpropanesulfonic acid, and octylphenol polyoxyethylene ether in a weight ratio of 15:9:5 were added to a stirred tank, nitrogen gas was introduced, and the mixture was stirred and reacted at 40°C for 1 hour to obtain a premix. Then, N-hydroxymethylbenzamide (12% of the premix mass) and hydrochloric acid (1% of the premix mass) were added, and the mixture was stirred for another 1 hour to obtain hydrophobically modified polyacrylamide. By weight, 7 parts of chromium oxide and 3 parts of titanium carbide were added to 100 parts of dispersion (a mixture of deionized water and anhydrous ethanol in a volume ratio of 3:1). Under stirring, 60 parts of 3-aminophenol and 4 parts of ammonia were added, and the mixture was ultrasonically dispersed for 25 min. Then, 7 parts of formaldehyde were added, and the mixture was stirred for 45 min. After drying at 60°C, the temperature was increased to 700°C at a rate of 5°C / min and held for 1 h. After cooling to room temperature, a carbon-coated core-shell material was obtained. Then, 6% of the mass of the carbon-coated core-shell material, 3-aminopropyltriethoxysilane was added, and the mixture was stirred at 50 r / min for 60 min. After centrifugation, washing, and drying, a modified core-shell structure filler was obtained. By weight, 6 parts of mica sheets and 4 parts of graphene were mixed to obtain a mixture. Then, 3% of the mass of the mixture was added to 3-aminopropyltriethoxysilane. The mixture was stirred at 50 r / min for 60 min, centrifuged, washed, and dried to obtain the modified sheet filler. By weight, 38 parts of methylphenyl silicone resin were added to 25 parts of n-butanol and stirred at 300 r / min for 15 min. Then, 9 parts of hydrophobic modified polyacrylamide, 4 parts of polyethylene glycol, 0.5 parts of polysiloxane and 1 part of sodium tripolyphosphate were added and stirred for another 20 min to obtain mixture A. Mix 16 parts potassium silicate, 10 parts sodium silicate and 0.4 parts polyoxyethylene fatty alcohol ether, and stir and disperse at 60°C for 25 min to obtain mixture B; Mixture B is added to mixture A. Under stirring conditions of 300 r / min, 15 parts of modified core-shell structure filler, 10 parts of modified sheet filler, 3 parts of aluminum hydroxide and 4 parts of carboxymethyl cellulose are added. The mixture is stirred for 2 hours. Then, 1 part of polyethersulfone and 2 parts of silica sol are added. The mixture is stirred for another 50 minutes to obtain the anti-corrosion coating for the surface of the anode steel claw of the aluminum electrolytic cell.

[0052] Comparative Example 1: Compared with Example 3, Comparative Example 1 did not contain hydrophobically modified polyacrylamide, but was otherwise the same as Example 3.

[0053] Comparative Example 2: Compared with Example 3, the preparation method of the anti-corrosion coating of Comparative Example 2 includes the following steps: By weight, 6 parts of mica sheets and 4 parts of graphene were mixed to obtain a mixture. Then, 3% of the mass of the mixture was added to 3-aminopropyltriethoxysilane. The mixture was stirred at 50 r / min for 60 min, centrifuged, washed, and dried to obtain the modified sheet filler. By weight, 38 parts of methylphenyl silicone resin were added to 25 parts of n-butanol and stirred at 300 r / min for 15 min. Then, 9 parts of hydrophobic modified polyacrylamide, 4 parts of polyethylene glycol, 0.5 parts of polysiloxane and 1 part of sodium tripolyphosphate were added and stirred for another 20 min to obtain mixture A. Mix 16 parts potassium silicate, 10 parts sodium silicate and 0.4 parts polyoxyethylene fatty alcohol ether, and stir and disperse at 60°C for 25 min to obtain mixture B; Add the mixture B to the mixture A, and under stirring conditions of 300 r / min, continue to add 7 parts of chromium oxide, 3 parts of titanium carbide, 10 parts of modified flake filler, 3 parts of aluminum hydroxide and 4 parts of carboxymethyl cellulose. Stir for 2 hours, then add 1 part of polyethersulfone and 2 parts of silica sol, and continue stirring for 50 minutes to obtain the anti-corrosion coating for the surface of the anode steel claw of the aluminum electrolytic cell.

[0054] Comparative Example 3: The difference between Comparative Example 3 and Example 3 is that Comparative Example 3 uses only chromium oxide and does not add titanium carbide, while the rest is the same as Example 3.

[0055] Comparative Example 4: Compared with Example 3, Comparative Example 4 uses barium sulfate instead of chromium oxide and titanium carbide, while the rest is the same as Example 3.

[0056] Comparative Example 5: The difference between Comparative Example 5 and Example 3 is that no modified core-shell structure filler was added in Comparative Example 5, but otherwise it is the same as Example 3.

[0057] Comparative Example 6: The difference between Comparative Example 6 and Example 3 is that no graphene was added in Comparative Example 6, but otherwise it is the same as Example 3.

[0058] Comparative Example 7: The difference between Comparative Example 7 and Example 3 is that no modified sheet filler was added in Comparative Example 7, but otherwise it is the same as Example 3.

[0059] Comparative Example 8: The difference between Comparative Example 8 and Example 3 is that no corrosion inhibitor was added in Comparative Example 8, but otherwise it is the same as Example 3.

[0060] Comparative Example 9: The difference between Comparative Example 9 and Example 3 is that no potassium silicate or sodium silicate was added in Comparative Example 9, but otherwise it is the same as Example 3.

[0061] The coating samples prepared in Examples 1-3 and the comparative coating samples prepared in Comparative Examples 1-9 were subjected to performance tests. Adhesion was tested according to GB / T 5210; temperature resistance according to GB / T 1740 (1500℃); thermal weight loss was tested using differential scanning calorimetry (1000℃); salt spray resistance according to GB / T 1771; and impact resistance according to GB / T 1732. The results are shown in Table 1 below.

[0062] Specific method: The surface of the anode steel claw is pre-treated by sandblasting to make its surface meet the rust removal grade Sa2.5. Sa2.5 rust removal grade standard: Thorough abrasive blasting completely removes rust and oxide scale, and after dust removal, the steel surface has a near-white metallic luster; then, the anti-corrosion coating samples prepared in Examples 1-3 and the comparative anti-corrosion coating samples prepared in Comparative Examples 1-9 are sprayed onto the surface of the anode steel claw, with a coating thickness of 150μm, and the coating is formed after drying.

[0063] Table 1: Performance Test Results

[0064] Analysis of the data in Table 1 shows that by optimizing the composition and component ratio, this application achieves a coating system with superior adhesion, temperature resistance, corrosion resistance, and impact resistance. Compared to Example 3, Comparative Example 1 did not add hydrophobically modified polyacrylamide, but the coating performance decreased, indicating that adding a certain amount of hydrophobically modified polyacrylamide can ensure the application performance of the coating of this application. In Comparative Example 2, chromium oxide and titanium carbide were added directly to the system without resin carbonization encapsulation treatment, resulting in some uneven dispersion. The adhesion, temperature resistance, and corrosion resistance were all worse than in Example 3. Comparative Example 3 used only chromium oxide, Comparative Example 4 used barium sulfate to replace chromium oxide and titanium carbide, and Comparative Example 5 did not add modified core-shell structure filler, but the performance of the coatings was worse than in Example 3, indicating that the core-shell structure filler... The composition significantly affects the performance of the coating. Comparative Example 6 did not contain graphene, and Comparative Example 7 did not contain modified flake filler, yet their performance was worse than Example 3, indicating that the optimized composition of the modified flake filler in this application also significantly promotes the coating's performance. Comparative Example 8 did not contain corrosion inhibitors, resulting in overall performance worse than Example 3, demonstrating that adding appropriate corrosion inhibitors can have a synergistic effect, increasing the coating's corrosion resistance. Comparative Example 9 did not contain potassium silicate or sodium silicate, which not only affected the coating's bonding strength, leading to poor adhesion, but also reduced the coating's performance and service life due to the lack of potassium silicate and sodium silicate. Overall, the anti-corrosion coating of this application, through optimization of its composition and component ratios, exhibits superior application performance and a longer coating service life due to the interaction of its components.

[0065] The above description is merely a specific embodiment of this application, enabling those skilled in the art to understand or implement this application. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of this application. Therefore, this application is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features claimed herein.

Claims

1. An anti-corrosion coating for the surface of the anode steel claws in an aluminum electrolytic cell, characterized in that, The anti-corrosion coating comprises the following raw materials in parts by weight; The composition includes 35-40 parts of silicone resin, 8-10 parts of hydrophobically modified polyacrylamide, 15-18 parts of potassium silicate, 10-15 parts of sodium silicate, 3-5 parts of polyethylene glycol, 12-20 parts of modified core-shell filler, 8-12 parts of modified flake filler, 1-3 parts of corrosion inhibitor, 1-3 parts of adhesive, 1-2 parts of film-forming agent, 0.1-0.5 parts of defoamer, 3-5 parts of toughening agent, 0.1-0.5 parts of surfactant, 0.5-2 parts of dispersant, and 20-30 parts of solvent.

2. The anti-corrosion coating for the surface of the anode steel claws in an aluminum electrolytic cell according to claim 1, characterized in that, The preparation method of the modified core-shell structured filler includes the following steps: Chromium oxide and titanium carbide were added to the dispersion, and 3-aminophenol and ammonia were added under stirring. The mixture was ultrasonically dispersed and then formaldehyde was added. The mixture was stirred for 30 to 60 minutes. After drying and calcination, the mixture was cooled to room temperature and modified to obtain the modified core-shell structure filler.

3. The anti-corrosion coating for the surface of the anode steel claws in an aluminum electrolytic cell according to claim 2, characterized in that, The ratio of chromium oxide, titanium carbide, dispersion, 3-aminophenol, ammonia and formaldehyde by weight is (1~10): (1~5): 100: (50~80): (3~5): (5~10).

4. The anti-corrosion coating for the surface of the anode steel claws in an aluminum electrolytic cell according to claim 2, characterized in that, The calcination treatment conditions are as follows: the temperature is increased to 500℃~700℃ at a heating rate of 3℃ / min~8℃ / min, and held at that temperature for 1h~2h.

5. The anti-corrosion coating for the surface of the anode steel claws in an aluminum electrolytic cell according to claim 2, characterized in that, The modification process involves adding the calcined carbon-coated core-shell material to a silane coupling agent, stirring at a speed of 50 r / min to 100 r / min for 30 min to 60 min, centrifuging, washing, and drying to obtain the modified core-shell structure filler.

6. The anti-corrosion coating for the surface of the anode steel claws in an aluminum electrolytic cell according to claim 1, characterized in that, The modified sheet packing is prepared by adding the sheet packing to a silane coupling agent, stirring at a speed of 50 r / min to 100 r / min for 30 min to 60 min, centrifuging, washing, and drying to obtain the modified sheet packing.

7. The anti-corrosion coating for the surface of the anode steel claws in an aluminum electrolytic cell according to claim 6, characterized in that, The sheet-like filler is a mixture of mica sheets and graphene; The mass ratio of the mica sheet to the graphene is (1~8):(1~10). The mica sheet has a thickness of 0.1μm to 0.5μm and a diameter of 20μm to 100μm. The graphene has a thickness of 1 nm to 30 nm and a particle size of 1 μm to 40 μm.

8. The anti-corrosion coating for the surface of the anode steel claws in an aluminum electrolytic cell according to claim 1, characterized in that, The corrosion inhibitor is at least one of sodium hydroxide, potassium hydroxide, calcium hydroxide, aluminum hydroxide, and silicon carbide fiber.

9. The anti-corrosion coating for the surface of the anode steel claws in an aluminum electrolytic cell according to claim 1, characterized in that, The binder is at least one of silica sol, sodium silicate, and potassium silicate.

10. A method for preparing an anti-corrosion coating for the surface of the anode steel claws in an aluminum electrolytic cell, characterized in that, The preparation method is used to prepare an anti-corrosion coating for the surface of the anode steel claw of the aluminum electrolytic cell as described in any one of claims 1 to 9, and the preparation method includes the following steps: Add the silicone resin to the solvent and stir at 300r / min~500r / min for 10min~15min. Then add the hydrophobically modified polyacrylamide, polyethylene glycol, defoamer and dispersant, and continue stirring for 15min~30min to obtain mixture A. Potassium silicate, sodium silicate and surfactant are mixed and stirred and dispersed at 50℃~65℃ for 10min~30min to obtain mixture B; Add the mixture B to the mixture A, and continue to add the modified core-shell structure filler, modified flake filler, corrosion inhibitor and toughening agent under the stirring condition of 200 r / min to 500 r / min. Stir for 1 h to 3 h, add film-forming agent and binder, and continue stirring for 30 min to 60 min to obtain the anti-corrosion coating for the surface of the anode steel claw of the aluminum electrolytic cell.

Citation Information

Patent Citations

  • Method for preparing electrolytic aluminium carbon anode protective coating

    CN104005056A

  • A coating material for high-temperature oxidation protection of carbon anodes

    CN113563056B