A self-detachable adhesive tape for lithium batteries, its preparation method, and its electrode manufacturing method.
By designing a self-detachable tape for lithium batteries, the problem of disturbance to the electrode slurry during the drying process of the thermally triggered tape is solved by utilizing the elastic recovery of the substrate layer and the interface separation of the pressure-sensitive adhesive layer. This achieves stable tape detachment and centralized collection, improving the manufacturing efficiency and battery performance of lithium batteries.
Patent Information
- Application Number
- CN202611595213.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-15
- Publication Date
- 2026-11-17
AI Technical Summary
Existing heat-triggered tapes can easily disturb the incompletely dried electrode slurry during the drying process of lithium battery electrodes, resulting in thickening or uneven morphology at the edges of the empty foil area. Furthermore, it is difficult to achieve automatic overall detachment and centralized collection, which affects the service life and production efficiency of lithium batteries.
A self-removing tape for lithium batteries is adopted, comprising a substrate layer and a pressure-sensitive adhesive layer. The substrate layer remains stable during the drying stage and automatically detaches during cold pressing through elastic recovery. Combined with a hot melt adhesive layer and an anti-stick layer, the stability and peelability of the tape are ensured, avoiding disturbance to the electrode slurry.
In the manufacturing process of lithium battery electrodes, the tape remains stable during the drying stage, does not affect the drying of the electrode slurry, and automatically falls off after cold pressing, reducing the risk of residual adhesive. It is suitable for continuous production and improves battery performance and production efficiency.
Smart Images

Figure CN123107569A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium-ion battery manufacturing technology, and in particular to a self-detachable adhesive tape for lithium batteries, its preparation method, and its electrode manufacturing method. Background Technology
[0002] Electrodes in lithium-ion batteries are typically produced using a continuous coating process. The coating substrate (i.e., current collector) is usually a metal foil. The specific process involves coating a polymer electrode slurry onto the metal foil, and then using laser cleaning to create empty foil areas on certain parts of the surface to facilitate welding with the tabs.
[0003] During laser cleaning, the metal foil undergoes high-temperature oxidation, which leads to performance degradation and reduces the lifespan and unit capacity of lithium-ion batteries.
[0004] Currently, thermal foaming tape and heat shrinkable tape technologies have emerged to replace traditional laser cleaning methods. Before the lithium battery electrode is coated, the aforementioned tape is attached to the pre-reserved position of the tab on the current collector, with the adhesive side corresponding to the empty foil area. After the coating operation is completed, in the subsequent drying process, the foaming tape is heated and foamed and curled, and the heat shrinkable tape is heated and curled, thus peeling off from the current collector, thereby leaving an empty foil area in the active material layer to facilitate welding with the tab.
[0005] However, in battery cells made from electrodes using foamed tape, lithium plating has consistently occurred at the edges of the tape and the contact points between the positive and negative electrode materials. This is because during the coating slurry baking process, the foamed tape begins to expand in volume as the slurry dries. At this point, the slurry at the tape edges is not yet fully dry. This expansion also causes the slurry at the edges to deform, resulting in a thicker slurry layer than where no foamed tape is applied. During the battery cell winding or chip mounting process, this increased thickness creates a stepped difference, preventing a tight bond between the positive and negative electrodes and the separator, leading to lithium plating over time.
[0006] For example, patent application CN115232570A discloses a lithium battery foamed tape, its preparation process, and its preparation apparatus. The lithium battery foamed tape includes a composite layer, an adhesive layer, a foamed layer, and a PET release film. The foamed layer contains thermally expandable microspheres and a foaming agent. This solution designs the tape layer structure, raw material formulation, and hot-pressing composite process to improve the overall peel strength of the tape and mitigate the problem of easy bubbling. It also incorporates corresponding separating and cutting modules to achieve tape slitting. However, the peeling mechanism of this solution relies on the thermal expansion of the foamed layer during electrode slurry drying. Furthermore, it does not limit the relationship between the foaming trigger point and the degree of electrode slurry drying, nor does it control the thickness change of the electrode active material layer at the edge of the empty foil area during foaming. Therefore, it is still possible for the slurry at the tape edge to bulge and deform before the slurry is completely dry.
[0007] In contrast, heat shrinkable tape technology involves heat shrinkage deformation during the baking process. However, since the heat shrinkage of the tape often occurs in the plane along the XY axis, the shrinkage effect along the Z axis is not significant. This makes it difficult for the tape to significantly reduce the adhesion to the substrate, and it is difficult to collect the detached tape in subsequent processes. Therefore, the process cannot be automated.
[0008] For example, patent application CN120888248A discloses a heat-shrinkable tape for welding the tabs of lithium-ion batteries. This tape is formed by sequentially compounding a heat-shrinkable unidirectional shrinkable base layer, a first adhesive layer, a high-temperature resistant base layer, and a second adhesive layer. The tape covers the tab welding position before the electrode current collector is coated. During the drying process, the heat-shrinkable unidirectional shrinkable base layer generates horizontal shrinkage stress, which drives the high-temperature resistant base layer to curl through the first adhesive layer, causing the tape to automatically peel off from the electrode current collector. However, this patent describes that the heat-shrinkable tape begins to shrink directionally before the electrode slurry in the front section of the drying tunnel is completely dry, and the electrode slurry on the tape surface will follow the tape's shrinkage and flow. Therefore, the tape's detachment process may still disturb the electrode slurry at the edge of the empty foil area that is not completely dry, and this solution is difficult to balance the stability of the edge morphology of the empty foil area with the centralized recycling requirements of continuous production.
[0009] It is evident that while existing thermal foaming tapes and heat shrinkable tapes can replace laser cleaning processes to some extent, their deformation and detachment processes typically occur during the electrode slurry drying stage. This can easily disturb the edge slurry that is not yet fully dried, leading to thickening or uneven morphology of the electrode active material layer at the edge of the empty foil area. Furthermore, some tapes also have the problem of not being able to automatically detach as a whole or being inconvenient to collect.
[0010] Therefore, how to provide a lithium battery tape that solves the technical problems of existing heat-triggered tapes, such as premature deformation during the drying stage, easy disturbance of undried slurry, and insufficient stability in overall shedding and centralized collection, and achieves uniform thickness at the edge of the empty foil area, minimal residue when the tape falls off, and suitability for continuous production, is a problem that urgently needs to be solved by those skilled in the art. Summary of the Invention
[0011] To address the shortcomings of the existing technology, this invention provides a self-detachable adhesive tape for lithium batteries, its preparation method, and an electrode manufacturing method. This method ensures that the tape remains stably attached during the coating and drying stage without thermal deformation. In the subsequent cold pressing process, the elastic recovery of the substrate layer generates a peeling force to achieve automatic tape detachment. This avoids disturbance to the incompletely dried edge paste and inhibits the thickening of the empty foil area at the edge, while simultaneously achieving stable tape detachment and centralized collection.
[0012] In a first aspect, the present invention provides a self-removing adhesive tape for lithium batteries, comprising a substrate layer and a pressure-sensitive adhesive layer disposed on one side of the substrate layer; The thickness of the pressure-sensitive adhesive layer is 1-20 μm, including acrylic pressure-sensitive adhesives, which, by weight, are formed by crosslinking and curing the following raw materials: 80-100 parts of acrylic masterbatch; Curing component: 0.5-15 parts; The curing component includes at least one of isocyanate curing agent and epoxy curing agent; The adhesive force F1 of the pressure-sensitive adhesive layer to the bonded object is 1-20 gf / inch, and the interfacial bonding force F2 between the pressure-sensitive adhesive layer and the substrate layer is ≥50×F1; The thickness of the substrate layer is 5-50μm, and the elastic modulus at 120℃ is not less than 400MPa; The substrate layer undergoes elastic deformation under roller pressure of over 20 tons, causing the pressure-sensitive adhesive layer to separate from the bonded object, thus allowing the tape to fall off automatically.
[0013] It should be noted that the curing component of the present invention preferably involves pre-mixing the curing agent (solute) and solvent, and diluting the curing agent to a certain solid content (e.g., 2%-80%) before use. The solvent includes at least one of ethyl acetate, butyl acetate, and toluene. The acrylate masterbatch contains functional groups capable of cross-linking with the curing agent in the curing component, and the corresponding curing agent is selected according to the type and content of the functional groups contained in the acrylate masterbatch. Specifically, the isocyanate groups in the isocyanate curing agent can react with the hydroxyl groups or other active hydrogen groups in the acrylate masterbatch; the epoxy groups in the epoxy curing agent can react with the carboxyl groups and anhydrides in the acrylate masterbatch, thereby forming a cross-linked network and curing the acrylate masterbatch. By adjusting the type and amount of the curing component and its curing agent, the degree of cross-linking of the pressure-sensitive adhesive layer can be adjusted, enabling it to possess both the temporary adhesive properties required in the slurry coating and drying stages and the peelable properties required in the cold pressing stage.
[0014] It is understood that the bonding object in this invention refers to the electrode current collector (e.g., aluminum foil, copper foil, etc.) or the stainless steel plate used to test the bonding strength.
[0015] Preferably, the thickness of the substrate layer is 5-35 μm, including at least one of PET film layer, PI film layer, PEEK film layer, PPS film layer, LCP film layer, PEN film layer, PBT film layer, and aramid film layer.
[0016] The substrate layer of this invention maintains high dimensional stability during the electrode coating and drying stages, enabling the pressure-sensitive adhesive layer to maintain a temporary bond with the electrode current collector to prevent lifting or displacement. Simultaneously, the relationship between F2 and F1 ensures that the preferential separation interface is located between the pressure-sensitive adhesive layer and the electrode current collector. During cold pressing, the substrate layer undergoes bending or compressive elastic deformation under the roller gap pressure. After leaving the roller gap, it elastically recovers and generates a peeling torque at the edge of the tape, thereby causing the pressure-sensitive adhesive layer to gradually separate, curl, and effectively detach from the electrode current collector.
[0017] Preferably, the acrylate masterbatch comprises an acrylate copolymer formed by copolymerization of flexible segment monomers, rigid segment monomers and functional monomers; The functional monomer contains at least one of carboxyl, hydroxyl, amide, and acid anhydride groups.
[0018] Flexible monomers are used to improve the flexibility of the acrylate copolymer molecular chains and its wetting ability on the electrode current collector surface, enabling the pressure-sensitive adhesive layer to form a temporary bond under relatively low bonding pressure. Rigid monomers are used to improve the cohesive strength and heat resistance of the acrylate copolymer, limiting excessive flow of the pressure-sensitive adhesive layer during drying and cold pressing. Functional monomers are used to provide crosslinking reaction sites and / or polar interaction sites, enabling the acrylate copolymer to form a crosslinking network with the curing agent and improving the interfacial bonding stability between the pressure-sensitive adhesive layer and the substrate layer. Through the synergistic combination of these three types of monomers, the surface wettability, temporary adhesion, cohesive strength, and peelability of the pressure-sensitive adhesive layer can be balanced, reducing the risk of premature warping during the coating and drying stage and residual adhesive during the cold pressing stage.
[0019] More preferably, the flexible segment monomer includes at least one selected from ethyl acrylate, butyl acrylate, isobutyl acrylate, 2-ethylhexyl acrylate, lauryl acrylate, and octadecyl acrylate. The rigid segment monomers include at least one of methyl acrylate, methyl methacrylate, ethyl methacrylate, isobutyl methacrylate, cyclohexyl methacrylate, isobornyl methacrylate, styrene, acrylonitrile, and vinyl acetate. The functional monomers include at least one of acrylic acid, methacrylic acid, itaconic acid, maleic acid, maleic anhydride, hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, acrylamide, methacrylamide, N-hydroxymethylacrylamide, and diacetone acrylamide.
[0020] The aforementioned monomers can be used to adjust the glass transition temperature, molecular chain mobility, polarity, and crosslinking density of acrylate copolymers by utilizing differences in alkyl side chain length, cyclic or aromatic structure, polar groups, and reactive functional groups. By adjusting the types and proportions of flexible segment monomers, rigid segment monomers, and functional monomers, it is beneficial to control the adhesion force of the pressure-sensitive adhesive layer to the electrode current collector within a range that allows for stable adhesion and can be overcome by the elastic recovery force of the substrate layer, while simultaneously improving the cohesive strength and heat resistance stability of the pressure-sensitive adhesive layer.
[0021] Preferably, the self-removing adhesive tape for lithium batteries further includes at least one of the following layers: 1) A hot melt adhesive layer is disposed on the side of the substrate layer away from the pressure-sensitive adhesive layer, with a thickness of 0.5 to 20 μm, an elongation at break of not less than 150%, and a room temperature elastic modulus of not less than 1 MPa. The hot melt adhesive layer includes at least one of rubber adhesives, polyolefin adhesives, polyester adhesives, epoxy adhesives, and silicone adhesives. 2) Release layer, disposed on the side of the pressure-sensitive adhesive layer away from the substrate layer, with a thickness of 12 to 100 μm, including single-sided release film or double-sided release film.
[0022] Preferably, the hot melt adhesive layer comprises, by weight: 20-60 parts of polyolefin resin; 20-80 parts of tackifying resin; 0-20 parts of elastic component; Viscosity modifier 0-20 parts; 0-10 parts of color paste; The polyolefin resin includes at least one of EVA resin, α-olefin polymer resin and modified polyolefin resin, and the elastic component includes at least one of SBS, SIS and SEBS. Preferably, an anti-sticking layer is provided on the side of the hot melt adhesive layer opposite to the substrate layer, and the thickness of the anti-sticking layer is not greater than 10 μm; The anti-stick layer includes at least one of the following: ceramic coating, epoxy coating, acrylic coating, polyolefin coating or emulsion microsphere coating, PET film layer, PI film layer, BOPP film layer, and PE film layer.
[0023] Preferably, the self-removing adhesive tape for lithium batteries includes a plurality of adhesive units spaced apart on the side of the release layer, each adhesive unit including the pressure-sensitive adhesive layer, the substrate layer and the hot melt adhesive layer stacked sequentially from the release layer outward.
[0024] Secondly, the present invention also provides a method for preparing the self-removing adhesive tape for lithium batteries, comprising the following steps: Step 1: Prepare pressure-sensitive adhesive coating solution: After diluting the acrylic masterbatch and optional solvent by stirring, add the curing component, stir, and let stand to remove bubbles; Step 2: Based on the solid content of the pressure-sensitive adhesive coating liquid and the target thickness of the pressure-sensitive adhesive layer, select an appropriate micro-grooved roller, apply the pressure-sensitive adhesive coating liquid onto the release layer, and dry it to form a pressure-sensitive adhesive layer. Step 3: Unwind the substrate layer and bond it to the pressure-sensitive adhesive layer to obtain a self-removing tape for lithium batteries comprising a substrate layer and a pressure-sensitive adhesive layer.
[0025] Preferably, after bonding the substrate layer and the pressure-sensitive adhesive layer, the following step is further included: Prepare a hot melt adhesive coating liquid, apply the hot melt adhesive coating liquid directly to the side of the substrate layer away from the pressure-sensitive adhesive layer, dry to form a hot melt adhesive layer, and roll up to obtain a self-detachable tape for lithium batteries. Optionally, after drying to form the hot melt adhesive layer, an anti-stick layer may be applied or bonded to the side of the hot melt adhesive layer away from the substrate layer; Optionally, each layer on the side of the release layer can be die-cut to form multiple bonding units at intervals.
[0026] Thirdly, the present invention also provides a method for manufacturing an electrode using the self-detachable adhesive tape for lithium batteries, comprising the following steps: S1. The pressure-sensitive adhesive layer of the self-removing tape is bonded to the electrode current collector to cover the reserved electrode tab area; S2. Apply electrode slurry to the surface of the electrode current collector and the self-detachable adhesive tape, and dry the electrode slurry to form an electrode active material layer; S3. Apply a roller pressure of more than 20 tons to the electrode active material layer for cold pressing. The substrate layer undergoes elastic deformation under force, which causes the pressure-sensitive adhesive layer to separate from the electrode current collector, so that the tape curls on the electrode current collector and automatically falls off, exposing the reserved tab area on the electrode current collector. S4. Forming a tab in the reserved tab area to obtain the electrode sheet.
[0027] Preferably, the 180° peel force of the pressure-sensitive adhesive layer on the electrode current collector is 1-20 gf / inch, more preferably 2-10 gf / inch, and the total pressure of the cold pressing is 20-150 tons, more preferably 50-130 tons; The self-detaching tape can quickly bounce off the electrode current collector after cold pressing, and the time for bounce-off is less than 60s, preferably less than 30s, more preferably less than 15s. The increase in the thickness of the electrode active material layer at the edge of the reserved tab area relative to the thickness of the electrode active material layer at other locations of the electrode current collector is less than 8μm, preferably less than 5μm, more preferably less than 2μm.
[0028] The self-detachable adhesive tape for lithium batteries, its preparation method, and its electrode manufacturing method provided by this invention have at least the following beneficial effects: (1) The present invention uses a substrate layer with a high elastic modulus at the drying temperature, which makes the tape stable during the electrode slurry coating and drying stages, and does not rely on heat-induced foaming or heat-induced shrinkage to achieve detachment, thereby reducing the disturbance caused by the thermal deformation of the tape to the edge slurry that is not completely dried. At the same time, the elastic recovery of the substrate layer after cold pressing triggers the tape curling and detachment, and by using the difference between the adhesion force of the pressure-sensitive adhesive layer to the electrode current collector and the interfacial bonding force between the pressure-sensitive adhesive layer and the substrate layer, the tape is controlled to separate preferentially at the electrode current collector interface, so that the pressure-sensitive adhesive layer is removed as a whole with the substrate layer, reducing the risk of residual adhesive and adhesive layer transfer.
[0029] (2) By setting a hot melt adhesive layer, an anti-sticking layer and an intermittently set bonding unit, the present invention can further improve the integrity of the detached tape, prevent the tape from being adhered to the process roller, and facilitate continuous feeding, automatic bonding and centralized collection according to the position of the reserved tab area.
[0030] (3) The preparation method of the present invention can control the thickness and interface bonding state of the pressure-sensitive adhesive layer and the hot melt adhesive layer respectively. The process steps are continuous and suitable for roll-to-roll production. The electrode manufacturing method uses the existing cold pressing process to trigger the tape to fall off, without the need to add laser cleaning or special heat-triggered peeling process, which helps to simplify the electrode manufacturing process. Attached Figure Description
[0031] Figure 1 This is a schematic diagram of the laminated structure of the self-removing adhesive tape in Examples 1-1 to 1-3; Figure 2 This is a schematic diagram of the laminated structure of the self-removing adhesive tape with a hot melt adhesive layer in Examples 2-1 to 2-5; Figure 3 This is a schematic diagram of the laminated structure of the self-removing adhesive tape with a hot melt adhesive layer and an anti-stick layer in Examples 3-1 to 3-2; Figure 4 This is a schematic diagram of the laminated structure of the self-detachable adhesive tape roll with spaced adhesive units in Example 4; Figure 5 This is a schematic diagram of the planar arrangement of multiple adhesive units on a continuous release layer in Example 4; Figure 6 This is a flowchart illustrating the operation of the self-removing adhesive tape for lithium batteries according to the present invention, from application to automatic detachment, wherein: (a) is a schematic diagram of the structure before the self-removing adhesive tape is applied; (b) is a schematic diagram of the structure after the self-detachable adhesive tape is attached to the reserved tab area of the electrode current collector; (c) is a schematic diagram of the electrode structure after the electrode paste has been coated and dried; (d) is a schematic diagram of the cold pressing of the electrode sheet; (e) is a schematic diagram of the structure after the self-detaching tape curls off and exposes the reserved electrode area.
[0032] Reference numerals: 1-Substrate layer; 2-Pressure-sensitive adhesive layer; 3-Release layer; 4-Hot melt adhesive layer; 5-Anti-stick layer; 10-Adhesive unit; 100 - Electrode current collector; 200 - Reserved tab area; 300 - Electrode active material layer; X - length direction; Y - width direction. Detailed Implementation
[0033] To better understand the above technical solutions, a detailed description of the solutions will be provided below in conjunction with the accompanying drawings and specific embodiments. Obviously, the described embodiments are merely some, not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0034] The terminology used in the embodiments of this invention is for the purpose of describing particular embodiments only and is not intended to limit the invention. The singular forms “a,” “the,” and “the” as used in the embodiments of this invention and the appended claims are also intended to include the plural forms, and “multiple” generally includes at least two unless the context clearly indicates otherwise.
[0035] It should also be noted that the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that an article or device that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such an article or device. Without further limitation, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the article or device that includes said element.
[0036] This invention provides a self-removing adhesive tape for lithium batteries, specifically comprising: (1) Substrate layer 1, with a thickness of 5 to 50 μm, has an elastic modulus of not less than 400 MPa at 120°C, preferably not less than 600 MPa, and is capable of elastic deformation under a roller pressure of more than 20 tons.
[0037] In one preferred embodiment, the thickness of the substrate layer 1 is 5–35 μm. The substrate layer 1 may include at least one of a PET film layer, a PI film layer, a PEEK film layer, a PPS film layer, an LCP film layer, a PEN film layer, a PBT film layer, and an aramid film layer, or may be a composite film formed from the above materials. Regardless of whether a single-layer film or a composite film is used, the resulting substrate layer should meet the performance requirements of thickness, elastic modulus at 120°C, and elastic recovery after cold pressing.
[0038] In a more preferred embodiment, the substrate layer 1 undergoes recoverable elastic deformation when a nominal total pressure of 20 to 150 tons is applied by a cold pressing device (such as a cold pressing roller), and the elongation at break along the length direction of the substrate layer 1 is not less than 100%, the elongation at break along the width direction is not less than 100%, and the tensile strength is not less than 150 MPa.
[0039] In one preferred embodiment, the substrate layer 1 or the adhesive layer disposed on the substrate layer 1 is green, blue, yellow or brown, so as to use a CCD vision system to identify the adhesion position, curling state and detachment state of the tape.
[0040] (2) Pressure-sensitive adhesive layer 2, with a thickness of 1 to 20 μm, including acrylic pressure-sensitive adhesive; by weight, the acrylic pressure-sensitive adhesive is formed by cross-linking and curing 80 to 100 parts of acrylate masterbatch and 0.5 to 15 parts of curing component, wherein the curing component includes at least one of isocyanate curing agent and epoxy curing agent.
[0041] In one preferred embodiment, the thickness of the pressure-sensitive adhesive layer 2 is 1–10 μm. The pressure-sensitive adhesive layer 2 is resistant to N-methylpyrrolidone or the solvents used in the corresponding electrode paste, and does not undergo significant swelling, dissolution, bubbling, or adhesive layer transfer during electrode coating and drying.
[0042] Acrylic masterbatch includes acrylic copolymers formed by copolymerization of flexible segment monomers, rigid segment monomers and functional monomers.
[0043] In one preferred embodiment, the flexible segment monomer includes at least one selected from ethyl acrylate, butyl acrylate, isobutyl acrylate, 2-ethylhexyl acrylate, lauryl acrylate, and octadecyl acrylate.
[0044] In one preferred embodiment, the rigid segment monomer includes at least one of methyl acrylate, methyl methacrylate, ethyl methacrylate, isobutyl methacrylate, cyclohexyl methacrylate, isobornyl methacrylate, styrene, acrylonitrile, and vinyl acetate.
[0045] In one preferred embodiment, the functional monomer includes at least one selected from acrylic acid, methacrylic acid, itaconic acid, maleic acid, maleic anhydride, hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, acrylamide, methacrylamide, N-hydroxymethylacrylamide, and diacetone acrylamide. The functional monomer contains at least one selected from carboxyl, hydroxyl, amide, and acid anhydride groups.
[0046] The curing components are selected based on the type and content of functional groups contained in the acrylate masterbatch. Hydroxyl-containing acrylate masterbatches can undergo cross-linking reactions with isocyanate curing agents; carboxyl- and / or anhydride-containing acrylate masterbatches can undergo ring-opening reactions with epoxy curing agents. By adjusting the type and amount of curing components and curing agents, the degree of cross-linking, wetting ability, and cohesive strength of the pressure-sensitive adhesive layer 2 can be adjusted.
[0047] In one preferred embodiment, the isocyanate curing agent includes at least one of hexamethylene diisocyanate (HDI) or its trimer, toluene diisocyanate (TDI) or its trimer, 4,4'-dicyclohexylmethane diisocyanate (HMDI), isophorone diisocyanate (IPDI), and isocyanurate; and the epoxy curing agent includes at least one of difunctional, trifunctional, or tetrafunctional glycidylamine type epoxy resins, preferably 4,4'-methylenebis(N,N-diglycidylaniline).
[0048] It is understood that the above-mentioned curing components are preferably mixed with the solvent first, diluted to a certain solid content, and then used. That is to say, the weight parts of the above-mentioned 0.5 to 15 parts of curing components are calculated based on the total weight of the curing agent and solvent after solvent dilution. The solvent includes at least one of ethyl acetate, butyl acetate, and toluene. The solid content range of the curing agent is determined according to the specific type of curing agent, and is preferably 2% to 80%.
[0049] The aforementioned acrylic masterbatch can be sourced from commercially available sources or prepared in-house.
[0050] The adhesion force F1 of the pressure-sensitive adhesive layer 2 to the bonded object is 1 to 20 gf / inch, and the interfacial bonding force F2 between the pressure-sensitive adhesive layer 2 and the substrate layer 1 is ≥50×F1.
[0051] In one preferred embodiment, the adhesion force F1 of the pressure-sensitive adhesive layer 2 to the electrode current collector is 2 to 10 gf / inch. By controlling F1, the pressure-sensitive adhesive layer 2 maintains temporary fixation to the electrode current collector during the bonding, conveying, slurry coating, and drying stages, while ensuring that this adhesion force can be overcome by the elastic recovery force of the substrate layer 1 after cold pressing. By making F2 not less than 50 times F1, when the tape detaches, interfacial separation preferentially occurs between the pressure-sensitive adhesive layer 2 and the electrode current collector, and the pressure-sensitive adhesive layer 2 is removed as a whole along with the substrate layer 1.
[0052] (3) Release layer 3, disposed on the side of pressure-sensitive adhesive layer 2 away from substrate layer 1, with a thickness of 12-100 μm, including single-sided release film or double-sided release film. Release layer 3 is used to isolate and protect pressure-sensitive adhesive layer 2 during tape storage, winding, die-cutting and conveying, and to support subsequent die-cutting and transfer operations as a continuous carrier. In use, release layer 3 is peeled off from the surface of pressure-sensitive adhesive layer 2, exposing pressure-sensitive adhesive layer 2 and bonding it to electrode current collector.
[0053] In one preferred embodiment, the release layer 3 is made of PET film, PE film, or other film material that can withstand the coating and drying temperatures of the adhesive layer, whether it has been treated with silicone oil release or not.
[0054] In one preferred embodiment, the release force on the side of the release layer 3 that contacts the pressure-sensitive adhesive layer 2 is no greater than 15 gf / inch. When the tape also includes a hot melt adhesive layer 4, and the back side of the release layer 3 contacts the hot melt adhesive layer 4 in the wound state, the release force on the back side of the release layer 3 is no greater than 10 gf / inch.
[0055] like Figure 1 As shown, in one specific embodiment, the self-removing adhesive tape includes a release layer 3, a pressure-sensitive adhesive layer 2, and a substrate layer 1 stacked sequentially from one side to the other. Before use, the release layer 3 is peeled off, and the pressure-sensitive adhesive layer 2 is adhered to the reserved tab area of the electrode current collector.
[0056] In addition to the release layer 3, the pressure-sensitive adhesive layer 2, and the substrate layer 1, the self-removing tape preferably includes (4) a hot melt adhesive layer 4, disposed on the side of the substrate layer 1 opposite to the pressure-sensitive adhesive layer 2, such as... Figure 2 As shown, the thickness of the hot melt adhesive layer 4 is 0.5–20 μm, the elongation at break is not less than 150%, preferably not less than 300%, and the room temperature elastic modulus is not less than 1 MPa. It includes at least one of rubber-based adhesives, polyolefin-based adhesives, polyester-based adhesives, epoxy-based adhesives, and silicone-based adhesives. The elongation at break allows the hot melt adhesive layer 4 to bend and curl with the substrate layer 1 without easily breaking; the room temperature elastic modulus provides the hot melt adhesive layer 4 with the necessary cohesive strength and stress transmission capability.
[0057] In one preferred embodiment, the thickness of the hot melt adhesive layer 4 is 1–10 μm. The hot melt adhesive layer 4 is resistant to N-methylpyrrolidone or the solvent used in the actual electrode paste, has low surface tack at room temperature, and its room temperature adhesion to stainless steel plates is no greater than 20 gf / inch. The hot melt adhesive layer 4 softens or is thermally activated at the electrode paste drying temperature and bonds with the electrode active material covering the tape surface, allowing the tape to carry away the electrode active material covering it when it is removed after cold pressing.
[0058] In one preferred embodiment, the hot melt adhesive layer 4 comprises, by weight: 20-60 parts of polyolefin resin; 20-80 parts of tackifying resin; 0-20 parts of elastic component; Viscosity modifier 0-20 parts; 0-10 parts of color paste; Polyolefin resins include at least one of EVA resin, α-olefin polymer resin, and modified polyolefin resin. α-olefin polymer resins include at least one of polyethylene, polypropylene, ethylene-octene copolymer, and amorphous polyα-olefin resin. Modified polyolefin resins include at least one of maleic anhydride-modified α-olefin polymer resin, acrylic acid-modified α-olefin polymer resin, ethylene-acrylic acid copolymer, and ethylene-methacrylic acid copolymer.
[0059] In a more preferred embodiment, the vinyl acetate content in the EVA resin is 10-50%, and the melt mass flow rate at 190°C and 2.16 kg is 5-500 g / 10 min.
[0060] The tackifying resin includes at least one of rosin resin, terpene resin, and petroleum resin. The elastic component includes at least one of SBS, SIS, and SEBS. In a more preferred embodiment, the melt mass flow rate of the elastic component at 230°C and 2.16 kg is 5–500 g / 10 min. The viscosity modifier includes white oils of different molecular weights.
[0061] When a transparent film layer is selected as the substrate layer, color paste can be added to the hot melt adhesive layer to facilitate tape identification. The color paste is a commonly used type of color paste in this field.
[0062] like Figure 3 As shown, on the side of the hot melt adhesive layer 4 facing away from the substrate layer 1, the self-removing tape may optionally include (5) an anti-stick layer 5 with a thickness of not more than 10 μm. The anti-stick layer 5 includes at least one of ceramic coating, epoxy coating, acrylic coating, polyolefin coating, emulsion microsphere coating, PET film layer, PI film layer, BOPP film layer and PE film layer.
[0063] Specifically, the emulsion microsphere coating includes at least one of styrene-acrylic emulsion, pure acrylic emulsion, polyolefin emulsion, modified polyolefin emulsion, and crystalline polyester emulsion. The particle size (D50) of the emulsion microspheres (tested by laser diffraction) is 0.01-2 μm, preferably 0.01-1.5 μm, and more preferably 0.01-0.8 μm.
[0064] In one preferred embodiment, the thickness of the anti-adhesion layer 5 is no greater than 8 μm. The anti-adhesion layer 5 is resistant to N-methylpyrrolidone or the solvent used in the actual electrode paste, and its room temperature adhesion to the stainless steel plate is no greater than 15 gf / inch, or it does not exhibit measurable adhesion to the stainless steel plate.
[0065] The anti-stick layer 5 forms a low-tack or non-stick surface on the outside of the hot melt adhesive layer 4 to prevent the tape or the die-cut bonding unit 10 from being adhered to and carried away by the process rollers during unwinding, conveying, drying and cold pressing. When the anti-stick layer 5 is a coating, it can be directly applied to the surface of the hot melt adhesive layer 4; when the anti-stick layer 5 is a film, it can be bonded to the hot melt adhesive layer 4.
[0066] The dimensions of the bonding unit 10 in the length direction X and width direction Y are determined according to the shape and size of the reserved tab area. During die cutting, the release layer 3 is retained as a continuous carrier tape, and the pressure-sensitive adhesive layer 2, substrate layer 1, hot melt adhesive layer 4 and optional anti-stick layer 5 above the release layer 3 are cut off and removed, thereby forming a roll material that can be continuously picked up by an automatic laminating equipment.
[0067] like Figure 4 and Figure 5 As shown, in one specific embodiment, a plurality of adhesive units 10 are spaced apart on one side surface of the continuous release layer 3. Each adhesive unit 10 includes a pressure-sensitive adhesive layer 2, a substrate layer 1, and a hot melt adhesive layer 4 stacked sequentially from the release layer 3 outwards. When the tape includes an anti-stick layer 5, each adhesive unit 10 may also include an anti-stick layer 5 disposed outside the hot melt adhesive layer 4.
[0068] The present invention also provides a method for preparing the above-mentioned self-removing adhesive tape for lithium batteries, specifically including the following steps: Step 1: Prepare pressure-sensitive adhesive coating solution: After diluting the acrylic masterbatch and optional solvent, add the curing component, stir, and let stand to remove bubbles.
[0069] Specifically, acrylate masterbatch and solvent are added to a mixing tank and stirred at 150-250 rpm for 5-15 minutes to uniformly dilute the acrylate masterbatch. A curing agent matching the functional groups in the acrylate masterbatch is weighed, and the curing agent is first mixed with a certain amount of solvent and diluted to obtain a certain solid content (e.g., approximately 2%-80%) to form a cured component. Then, the diluted acrylate masterbatch is added, and the mixture is stirred at 200-400 rpm for 10-20 minutes. After stirring, the mixture is allowed to stand for 5-15 minutes to remove bubbles, resulting in a pressure-sensitive adhesive coating solution. The solvent includes at least one of ethyl acetate, butyl acetate, and toluene.
[0070] Step 2: Select a suitable micro-grooving roller according to the solid content of the pressure-sensitive adhesive coating liquid and the target thickness of the pressure-sensitive adhesive layer 2, apply the pressure-sensitive adhesive coating liquid to the release layer 3, and dry to form a pressure-sensitive adhesive layer 2 with a thickness of 1 to 20 μm.
[0071] Specifically, release layer 3 is positioned at one end of the coating line. Pressure-sensitive adhesive liquid is continuously coated onto the release surface of release layer 3 using a selected micro-grooved roller. After coating, release layer 3 is passed through an oven to remove solvents and allow the acrylate masterbatch and curing agent to cross-link and solidify. The line count, cell volume, and coating speed of the micro-grooved roller are determined based on the solid content of the pressure-sensitive adhesive liquid, the wet film thickness, and the target dry film thickness.
[0072] Step 3: Unwind the substrate layer 1 and bond the substrate layer 1 to the pressure-sensitive adhesive layer 2 to obtain a self-removing tape for lithium batteries, which includes the substrate layer 1, the pressure-sensitive adhesive layer 2, and the release layer 3 stacked together.
[0073] Specifically, the substrate layer 1 is positioned at the second unwinding position on the coating line and continuously bonded to the dried pressure-sensitive adhesive layer 2. During the bonding process, the unwinding tension, bonding pressure, and bonding speed of the substrate layer 1 and the release layer 3 are controlled to prevent the substrate layer 1 from being overstretched or to avoid the formation of air bubbles at the bonding interface. After bonding, the substrate layer 1 is wound up and cured according to the crosslinking requirements of the pressure-sensitive adhesive system.
[0074] In one preferred embodiment, the tape includes a hot melt adhesive layer 4, meaning that after step three, the process further includes preparing a hot melt adhesive coating liquid and forming the hot melt adhesive layer 4. The hot melt adhesive coating layer is prepared according to step four: (1) To prepare the hot melt adhesive coating liquid, add solvent to the reaction vessel and start stirring. The initial stirring speed is 10-30 rpm. Add the elastic component, tackifying resin and polyolefin resin in sequence, and control the temperature of the reaction vessel at 80±10℃ according to the softening point of the resin used. After the addition is completed, increase the stirring speed to 250-400 rpm and continue stirring for 100-150 min until the mixture is clear and there are no obvious swellings or particles. Detect the solid content of the mixture. After the material is cooled to no higher than 60℃, filter it through a metal filter and a magnetic iron removal device to obtain the hot melt adhesive coating liquid. The solvent includes at least one of ethyl acetate, butyl acetate and toluene.
[0075] (2) Apply hot melt adhesive liquid directly to the side of the substrate layer 1 away from the pressure-sensitive adhesive layer 2, dry to form a hot melt adhesive layer 4 with a thickness of 0.5 to 20 μm, and roll it up to obtain a self-detachable tape for lithium batteries.
[0076] The direct coating refers to the process of directly contacting the hot melt adhesive coating liquid with the surface of the substrate layer 1 and drying it to form the hot melt adhesive layer 4, without pre-forming the hot melt adhesive coating liquid into an independent adhesive film and then transferring it.
[0077] Optionally, in step five, an anti-stick coating is applied or an anti-stick film is bonded to the side of the hot melt adhesive layer 4 away from the substrate layer 1 to form an anti-stick layer 5 with a thickness of no more than 10 μm.
[0078] Optionally, in step six, each layer located on one side of release layer 3 and other than release layer 3 is die-cut and waste is removed to form multiple adhesive units 10 at intervals on the continuous release layer 3.
[0079] This invention also provides a method for manufacturing electrode sheets using the above-mentioned self-detaching adhesive tape for lithium batteries, wherein the operation process of the self-detaching adhesive tape from bonding to automatic detachment is as follows: Figure 6 As shown, the specific steps include: S1. The pressure-sensitive adhesive layer 2, made of self-removing adhesive tape, is bonded to the electrode current collector 100 to cover the reserved tab area 200. See [reference needed]. Figure 6 Figure (a) and Figure (b).
[0080] Specifically, the release layer 3 is peeled off, and the pressure-sensitive adhesive layer 2 is adhered to the pre-defined tab area 200 on the electrode current collector 100. During adhesion, the edge of the adhesive tape is aligned with the boundary of the pre-defined tab area 200, and air bubbles between the pressure-sensitive adhesive layer 2 and the electrode current collector 100 are removed. When manufacturing the positive electrode, the electrode current collector 100 can be aluminum foil; when manufacturing the negative electrode, the electrode current collector 100 can be copper foil.
[0081] S2. Apply electrode slurry to the surfaces of the electrode current collector 100 and the self-removing adhesive tape, and dry the electrode slurry to form the electrode active material layer 300. (See below) Figure 6 (c) diagram.
[0082] The electrode paste can be either a positive electrode paste or a negative electrode paste. During the drying process, the substrate layer 1 maintains dimensional stability at the drying temperature, and the pressure-sensitive adhesive layer 2 remains temporarily adhered to the electrode current collector 100, so that the tape continuously covers the reserved tab area 200 before entering the cold pressing process.
[0083] S3. Apply a rolling pressure of over 20 tons to the electrode active material layer 300 for cold pressing. See below. Figure 6 Figure (d) shows that the substrate layer 1 is subjected to force to produce elastic deformation, which causes the pressure-sensitive adhesive layer 2 to separate from the electrode current collector 100, so that the self-detaching tape curls and automatically falls off on the electrode current collector 100, exposing the reserved electrode tab area 200. See Figure (d). Figure 6 (e) diagram.
[0084] In one preferred embodiment, the nominal total pressure of the cold pressing equipment (such as cold pressing rollers) is 20 to 150 tons. In a more preferred embodiment, the nominal total pressure of the cold pressing equipment is 50 to 130 tons.
[0085] After the substrate layer 1 enters the cold-pressing roller gap, it undergoes bending or compressive elastic deformation. After leaving the roller gap, it elastically recovers and forms a peeling torque at the edge of the tape. When the peeling torque overcomes the adhesive force F1 between the pressure-sensitive adhesive layer 2 and the electrode current collector 100, the tape curls from the edge and gradually separates from the electrode current collector 100. Since the interfacial bonding force F2 between the pressure-sensitive adhesive layer 2 and the substrate layer 1 is not less than 50 times F1, the pressure-sensitive adhesive layer 2 remains on the surface of the substrate layer 1 and is removed along with the entire substrate layer 1.
[0086] When the tape includes a hot melt adhesive layer 4 but not an anti-stick layer 5, the hot melt adhesive layer 4 bonds with the electrode active material covering the tape surface during the drying stage, and carries this portion of the electrode active material away with it when the tape is detached. When the tape includes an anti-stick layer 5, the material and surface condition of the anti-stick layer 5 should be selected according to the actual electrode slurry system to ensure that it is neither adhered to by the process rollers nor leaves any electrode active material residue in the reserved tab area 200.
[0087] S4. Form an electrode tab in the exposed reserved electrode tab area 200 to obtain an electrode sheet.
[0088] After the tape falls off, the reserved tab area 200 can be slit, punched, laser cut, welded or otherwise adapted according to the electrode structure to form the tab.
[0089] In one preferred embodiment, the pressure-sensitive adhesive layer 2 has a 180° peel force of 1 to 20 gf / inch against the electrode current collector 100, the nominal total pressure of the cold pressing equipment is 20 to 150 tons, the self-detaching tape quickly bounces off after leaving the cold pressing roller gap in its area, and completely separates from the electrode current collector 100, the time of bounce-off is less than 60s, and the increase in the thickness of the electrode active material layer at the edge of the reserved tab area 200 is less than 8 μm.
[0090] In a more preferred embodiment, the time for the tape to spring off after cold pressing is less than 30 seconds, and the increase in edge thickness ΔH is less than 5 μm; in a further preferred embodiment, the time for the tape to spring off after cold pressing is less than 15 seconds, and the increase in edge thickness ΔH is less than 2 μm.
[0091] Examples 1-1 to Examples 1-3 like Figure 1 As shown, the self-releasing tapes of Examples 1-1 to 1-3 all include a substrate layer 1, a pressure-sensitive adhesive layer 2, and a release layer 3 stacked sequentially, with the pressure-sensitive adhesive layer 2 located between the substrate layer 1 and the release layer 3. The difference between the above embodiments lies in the material composition, as shown in Table 1 (unit: parts): Table 1
[0092] In Examples 1-3, the acrylate masterbatch was prepared using the following method: 500g of ethyl acetate was added to a 5L reactor equipped with a stirrer, reflux condenser, thermometer, and nitrogen inlet pipe, and nitrogen was introduced for 30 minutes. 895g of 2-ethylhexyl acrylate, 50g of methyl methacrylate, 50g of hydroxypropyl acrylate, 5g of acrylic acid, 1.5g of azobisisobutyronitrile, and 900g of ethyl acetate were mixed to obtain a dropwise solution; the reactor temperature was raised to 78°C, and the dropwise addition was completed within 3 hours, followed by a reaction at this temperature for 4 hours; then a supplementary solution consisting of 0.5g of azobisisobutyronitrile and 100g of ethyl acetate was added, and the reaction was continued at this temperature for 2 hours. After cooling to 25°C, an acrylate masterbatch with a solid content of 40.0% was obtained.
[0093] The respective detachable adhesive tapes of Examples 1-1 to 1-3 were prepared using the following steps: Step 1: Preparation of pressure-sensitive adhesive coating solution: Take 100g of the acrylate masterbatch, add 20g of ethyl acetate, and stir at 200rpm for 10min; add the appropriate amount of curing components, which include isocyanate curing agent and epoxy curing agent. The isocyanate curing agent (TG-1) is an ethyl acetate solution of hexamethylene diisocyanate trimer, which is added directly. The epoxy curing agent (AG-80) is a toluene solution of 4,4'-methylenebis(N,N-diglycidylaniline) with a solid content of 5%. Stir at 300rpm for 15min, and let stand for 10min to remove bubbles to obtain the pressure-sensitive adhesive coating solution.
[0094] Step 2: Forming the pressure-sensitive adhesive layer: using a line count of 100 lines / inch and a liquid loading of 22 cm³. 3 / m 2 The micro-grooved roller applies pressure-sensitive adhesive liquid to the release surface of a single-sided silicone oil release PET film with a thickness of 50μm at a speed of 8m / min. The film is then passed through three oven zones with temperatures of 60℃, 80℃ and 100℃, and each zone is held for 40s to form a pressure-sensitive adhesive layer 2 with a dry film thickness of 3μm.
[0095] Step 3: Laminating the Substrate Layer: A 25μm thick biaxially oriented heat-set green PET film is used as the substrate layer 1. The adhesive-coating surface of substrate layer 1 is corona-treated to achieve a surface tension of 50mN / m. Under the conditions of a lamination temperature of 40℃, a lamination line pressure of 0.25MPa, a line speed of 8m / min, and an unwinding tension of 20N, the corona-treated surface of substrate layer 1 is laminated with pressure-sensitive adhesive layer 2 and cured at 50℃ for 48 hours to obtain the desired result. Figure 1 The self-removing tape shown in the figure has the following relationship: the adhesive force F1 of the pressure-sensitive adhesive layer to the bonded object and the interfacial bonding force F2 between the pressure-sensitive adhesive layer and the substrate layer both satisfy the following condition: F2≥50×F1.
[0096] The positive electrode sheet is manufactured using the obtained self-detachable adhesive tape. The specific steps are as follows: S1. Using 15μm thick aluminum foil as electrode current collector, cut the self-removing tape into 20mm×12mm rectangles, peel off the release PET film, attach the pressure-sensitive adhesive layer 2 to the reserved electrode tab area of the aluminum foil, and press it back and forth twice with a 2kg rubber pressure roller.
[0097] S2. Add 94g of lithium iron phosphate, 3g of conductive carbon black and 3g of polyvinylidene fluoride to 82g of N-methylpyrrolidone to prepare a positive electrode slurry with a solid content of 54.9%. The positive electrode slurry is continuously coated on the surface of aluminum foil and self-removing adhesive tape at a speed of 3m / min and a wet film thickness of 150μm. It is then passed through three oven sections with temperatures of 80℃, 100℃ and 120℃ in sequence, with a total residence time of 8min.
[0098] S3. Using a cold pressing roller with a diameter of 400mm and a surface width of 300mm, the dried positive electrode sheet is cold pressed with a nominal total pressure of 60 tons, a linear speed of 2m / min and a roller gap of 75μm. Timing starts when the self-detaching tape completely leaves the cold pressing roller gap until the tape completely bounces off. All samples complete self-detachment within 20-30s.
[0099] S4. After the self-detaching tape has completely detached, the exposed reserved tab area is cut to obtain the positive electrode sheet.
[0100] Examples 2-1 to 2-5 like Figure 2 As shown, the self-releasable tapes of Examples 2-1 to 2-5 all include a hot melt adhesive layer 4, a substrate layer 1, a pressure-sensitive adhesive layer 2, and a release layer 3 stacked sequentially. The differences in structure and material composition between the above examples are shown in Table 2 (unit: parts): Table 2
[0101] The difference between Examples 2-1 to 2-5 and Example 1-1 in the preparation steps of the self-removing adhesive tape is as follows: Following step three, the process further includes preparing the hot melt adhesive coating liquid and forming the hot melt adhesive layer 4. The hot melt adhesive coating layer is prepared according to step four: (1) To prepare the hot melt adhesive coating liquid, add 300g of toluene to the reactor and start stirring. The initial stirring speed is 20rpm. Add the optional elastic component, tackifying resin and polyolefin resin, and optional color paste in sequence. Control the reactor temperature at about 80℃. After the addition is completed, increase the stirring speed to 300rpm and continue stirring for 120min until the mixture is clear and there are no obvious swellings or particles. The solid content of the mixture is about 25%. After the material is cooled to no more than about 55℃, filter it through a metal filter and a magnetic iron removal device to obtain the hot melt adhesive coating liquid. (2) Use a line count of 120 lines / inch and a liquid loading of 24 cm³. 3 / m 2 A micro-concave roller applies hot melt adhesive liquid to the side of the substrate layer 1 away from the pressure-sensitive adhesive layer 2 at a speed of 8 m / min. The mixture is then sequentially passed through three drying oven sections at temperatures of 70℃, 90℃, and 110℃, with each section holding the liquid for 40 seconds. This process dries the mixture to form a 4 μm thick hot melt adhesive layer 4, which is then wound up. Figure 2 The lithium battery shown is a self-removing adhesive tape.
[0102] The specific steps for manufacturing positive electrode sheets using the self-detaching tapes obtained in Examples 2-1 to 2-5 are the same as those in Example 1-1. In step S3, timing begins when the area where the self-detaching tape is located completely leaves the gap between the cold pressing rollers until the tape completely bounces off. All samples complete self-detachment within 5-15 seconds.
[0103] Examples 3-1 to 3-3 like Figure 3 As shown, the self-removing adhesive tapes of Examples 3-1 to 3-3 all include, in sequence, an anti-adhesive layer 5, a hot melt adhesive layer 4, a substrate layer 1, a pressure-sensitive adhesive layer 2, and a release layer 3. The differences between the above examples are shown in Table 3 (unit: parts): Table 3
[0104] The difference between Examples 3-1 to 3-3 and Example 2-1 in the preparation steps of the self-removing adhesive tape is that, after step four, step five is also included: Using a line count of 150 lines / inch and a liquid loading of 10 cm³ 3 / m 2 A micro-concave roller is used to apply the obtained anti-stick coating liquid to the side of the hot melt adhesive layer 4 away from the substrate layer 1 at a speed of 8 m / min. The coating is then sequentially passed through three oven sections at temperatures of 60℃, 80℃, and 100℃, with each section holding for 30 seconds. Finally, the coating is cured at 50℃ for 24 hours to form an anti-stick layer 5 with a dry film thickness of 0.5 μm. Figure 3 The self-removing tape shown has a solid content of 5% in both the crystalline polyester emulsion and the modified polyolefin emulsion.
[0105] In Examples 3-2 and 3-3, a self-made modified polyolefin emulsion was used to form the anti-stick layer 5. The anti-stick coating liquid consisted of a self-made modified polyolefin emulsion with a solid content of 5%, which was a maleic anhydride-grafted polypropylene emulsion. The particle size (D50) of the emulsion was 0.50 μm. The preparation of the maleic anhydride-grafted polypropylene emulsion was carried out according to Comparative Example 1 in CN121518068A. By adjusting the shear conditions and the amount of emulsifier, emulsions with different particle sizes could be obtained.
[0106] The specific steps for manufacturing positive electrode sheets using the self-detaching tapes obtained in Examples 3-1 to 3-3 are the same as those in Example 2-1. In step S3, timing begins when the area where the self-detaching tape is located completely leaves the gap between the cold pressing rollers until the tape completely bounces off. All samples complete self-detachment within 20-30 seconds.
[0107] In Example 3-3, the adhesive strength of the hot melt adhesive layer reaches 8.6 gf / inch, which is more than twice that of the pressure-sensitive adhesive layer. At this time, the hot melt adhesive layer cannot be used directly as the outermost layer, otherwise the tape will be easily stuck off during the process. In this example, after the anti-stick layer 5 is laminated on its outer side, the adhesive strength of its outermost non-adhesive surface is reduced to about 0.8 gf / inch. The tape can achieve a good self-detachment effect while preventing sticking.
[0108] Example 4 This embodiment uses the laminated material prepared in Examples 2-3, and sets the width of the release layer 3 to 120mm.
[0109] A rotating circular cutter is used to cut the hot melt adhesive layer 4, the substrate layer 1, and the pressure-sensitive adhesive layer 2 in half to a depth of approximately 32 μm, while retaining the release layer 3 with a thickness of 50 μm as continuous and intact. The die-cutting speed is 10 m / min, and the hot melt adhesive layer 4, the substrate layer 1, and the pressure-sensitive adhesive layer 2 between adjacent bonding units 10 are removed, forming multiple bonding units 10 on the continuous release layer 3.
[0110] Each adhesive unit 10 has a length dimension of 12 mm in the X direction and a width dimension of 20 mm in the Y direction. The center pitch between adjacent adhesive units 10 is 30 mm, and the winding tension is 15 N, resulting in... Figure 4 and Figure 5 The continuous roll material shown.
[0111] During electrode manufacturing, an automatic labeling device is used to sequentially peel off the adhesive units 10 from the continuous release layer 3 at a speed of 20 units / min, and then attach the pressure-sensitive adhesive layer 2 of the adhesive unit 10 to the reserved tab area of the aluminum foil. Subsequently, the positive electrode slurry coating, drying, cold pressing, and reserved tab area cutting are completed according to S2 to S4 of Example 1-1. In step S3, timing begins when the self-detaching tape completely leaves the gap of the cold pressing rollers until the tape completely springs off, and all samples complete self-detachment within 12 seconds.
[0112] Comparative Example 1 The difference between this comparative example and Examples 2-3 is that a 25μm thick cast polypropylene film (25μm BOPP, Jintian) with a storage modulus of 238MPa at 120°C was used instead of a biaxially oriented heat-set PET film as the substrate layer 1. The remaining materials, preparation conditions, and electrode manufacturing conditions were the same as in Examples 2-3. Timing for the tape sample of Comparative Example 1 began when the area was completely away from the cold-pressing roller gap; it did not completely detach from the aluminum foil even after 2 minutes.
[0113] Comparative Example 2 The difference between this comparative example and Examples 2-3 lies in the composition of the pressure-sensitive adhesive layer. In Comparative Example 2, there were 100 parts of acrylate masterbatch, only 0.05 parts of isocyanate curing agent, and only 0.03 parts of epoxy curing agent. The remaining materials, preparation conditions, and electrode manufacturing conditions were the same as in Examples 2-3. Timing for the tape sample of Comparative Example 2 began when the area was completely away from the cold-pressing roller gap, and it still hadn't completely detached from the aluminum foil after more than 2 minutes.
[0114] Comparative Example 3 The difference between this comparative example and Examples 2-3 lies in the composition of the hot melt adhesive layer. In Comparative Example 3, there were 90 parts of tackifying resin, 5 parts each of the two polyolefin resins, 3 parts of blue pigment, and 1 part of white pigment. The remaining materials, preparation conditions, and electrode manufacturing conditions were the same as in Examples 2-3. Timing for the tape sample of Comparative Example 3 began when the area was completely separated from the cold press roller gap. It did not completely detach from the aluminum foil after more than 1 minute, but it was able to detach on its own after about 2 minutes.
[0115] Test methods 1. Pressure-sensitive adhesive layer adhesion F1 and non-adhesive surface adhesion (hot melt adhesive layer / anti-stick layer): The sample was conditioned for 24 hours at 23±1℃ and 50±5% relative humidity. After the pressure-sensitive adhesive layer of the 25mm wide adhesive tape sample was bonded to the SUS board, it was pressed back and forth 3 times by a 2kg roller and allowed to stand for 30 minutes. Then, it was peeled off at 200mm / min at 180°. The average force of the stable section was taken as the pressure-sensitive adhesive layer adhesion F1, with the unit being gf / inch. After the outermost layer (hot melt adhesive layer or anti-stick layer) of the 25mm wide adhesive tape sample was bonded to the SUS board, it was pressed back and forth 3 times by a 2kg roller and allowed to stand for 30 minutes. Then, it was peeled off at 200mm / min at 180°. The average force of the stable section was taken as the non-adhesive surface adhesion.
[0116] Using a similar method, the interfacial bonding force F2 between the pressure-sensitive adhesive layer and the substrate layer of the tape sample was tested. The interfacial bonding force F2 of all embodiments exceeded 260gf / inch, satisfying F2≥50×F1.
[0117] 2. Mechanical properties of the layers: The substrate layer was subjected to dynamic mechanical analysis in tensile mode according to GB / T 33061.4-2023. The test frequency was 1Hz and the heating rate was 3℃ / min. The storage modulus E′ at 120℃ was recorded as the elastic modulus. The hot melt adhesive layer was prepared into a 50μm film by independent film forming test. The room temperature elastic modulus of the hot melt adhesive layer was tested according to the above method. At the same time, the film prepared by the hot melt adhesive layer was stretched at 23℃ and 50mm / min using a universal tensile testing machine. The elongation at break of the hot melt adhesive layer was recorded.
[0118] 3. Automatic detachment and post-detachment status: After completing the adhesive application, slurry coating, drying and cold pressing according to each embodiment, start timing from the time the tape leaves the cold pressing roller gap and record the time of complete bounce-off; use a 50x stereomicroscope to check the residual adhesive and slurry penetration in the reserved tab area, and record whether the active material on the tape is completely removed with the tape.
[0119] 4. Edge thickness increase ΔH: A white light interferometer is used to scan 5mm along the direction perpendicular to the edge of the reserved tab area, with a measurement point spacing of 10μm; the difference between the maximum thickness Hedge within 1mm from the edge and the average thickness Hnormal of the normal area 3-5mm from the edge is taken, and calculated according to ΔH=Hedge-Hnormal, with the unit being μm.
[0120] Test Results The test data for each embodiment and comparative example are shown in Table 4: Table 4
[0121] As can be seen from the test results in Table 4, the adhesion force F1 of the pressure-sensitive adhesive layer to the bonded object in each embodiment is 1-20 gf / inch, especially 1-10 gf / inch, and the interfacial bonding force F2 between the pressure-sensitive adhesive layer and the substrate layer all exceed 260 gf / inch, meeting the requirement of F2≥50×F1. It can control the tape to separate preferentially at the electrode current collector interface by the difference between the adhesion force of the pressure-sensitive adhesive layer to the electrode current collector and the interfacial bonding force between the pressure-sensitive adhesive layer and the substrate layer, so that the pressure-sensitive adhesive layer can be removed as a whole with the substrate layer, reducing the risk of residual adhesive and adhesive layer transfer. In contrast, due to the excessively high adhesion force of the pressure-sensitive adhesive layer to the bonded object in Comparative Example 2, residual adhesive is easily left when peeling off, and even though the pressure-sensitive adhesive layer also has a high adhesion force to the substrate layer, it is not conducive to the rapid bounce and detachment of the pressure-sensitive adhesive layer and the bonded object during cold pressing.
[0122] According to the test results of each embodiment, the elastic modulus of the substrate layer at 120°C is not less than 400 MPa, preferably not less than 600 MPa. This not only enables the tape to remain stable during the electrode slurry coating and drying stages and reduces the disturbance caused by the thermal deformation of the tape to the edge slurry that has not been completely dried, but also utilizes the elastic recovery of the substrate layer after cold pressing to quickly trigger the tape to curl and fall off. In contrast, the elastic modulus of the substrate layer in Comparative Example 1 is insufficient, making it difficult to achieve rapid automatic fall off.
[0123] In each embodiment with a hot melt adhesive layer, the elongation at break of the hot melt adhesive layer is not less than 150%, preferably not less than 300%. The elongation at break makes the hot melt adhesive layer more likely to automatically detach as it bends and curls with the substrate layer. However, the elongation at break of the hot melt adhesive layer in Comparative Example 3 is too low, and its deformability with the substrate layer is low, which hinders the tape from curling up and detaching as a whole.
[0124] Based on the discovery that the residue-free self-detachment property of tape in the electrode manufacturing process has, but is not limited to, excellent advantages in continuous production and quality assurance, this invention obtains a stable detachment and centralized collection scheme for self-detaching tape used in lithium batteries by selecting materials and controlling the performance of each layer, such as the substrate layer and the pressure-sensitive adhesive layer. This effectively solves the technical problems of existing heat-triggered tapes, such as premature deformation during the drying stage, easy disturbance of undried slurry, and insufficient stability in overall detachment and centralized collection. It provides important material support for the efficient, continuous, and automated manufacturing of battery electrodes and has great industrial value and broad application prospects.
[0125] Although preferred embodiments of the invention have been described, those skilled in the art, upon learning the basic inventive concept, can make other changes and modifications to these embodiments. Therefore, the appended claims are intended to be interpreted as including both the preferred embodiments and all changes and modifications falling within the scope of the invention. Clearly, those skilled in the art can make various alterations and modifications to the invention without departing from its spirit and scope. Thus, if these modifications and modifications of the invention fall within the scope of the claims and their equivalents, the invention is also intended to include these modifications and modifications.
Claims
1. A self-removing adhesive tape for lithium batteries, characterized in that, It includes a substrate layer and a pressure-sensitive adhesive layer disposed on one side of the substrate layer; The thickness of the pressure-sensitive adhesive layer is 1-20 μm, including acrylic pressure-sensitive adhesives, which, by weight, are formed by crosslinking and curing the following raw materials: 80-100 parts of acrylic masterbatch; Curing component: 0.5-15 parts; The curing component includes at least one of isocyanate curing agent and epoxy curing agent; The adhesive force F1 of the pressure-sensitive adhesive layer to the bonded object is 1-20 gf / inch, and the interfacial bonding force F2 between the pressure-sensitive adhesive layer and the substrate layer is ≥50×F1; The thickness of the substrate layer is 5-50μm, and the elastic modulus at 120℃ is not less than 400MPa; The substrate layer undergoes elastic deformation under roller pressure of over 20 tons, causing the pressure-sensitive adhesive layer to separate from the bonded object, thus allowing the tape to fall off automatically.
2. The self-removing adhesive tape for lithium batteries as described in claim 1, characterized in that, The acrylate masterbatch includes an acrylate copolymer formed by copolymerization of flexible segment monomers, rigid segment monomers and functional monomers; The functional monomer contains at least one of carboxyl, hydroxyl, amide, and acid anhydride groups.
3. The self-removing adhesive tape for lithium batteries according to claim 2, characterized in that, The flexible segment monomer includes at least one of ethyl acrylate, butyl acrylate, isobutyl acrylate, 2-ethylhexyl acrylate, lauryl acrylate, and octadecyl acrylate. The rigid segment monomers include at least one of methyl acrylate, methyl methacrylate, ethyl methacrylate, isobutyl methacrylate, cyclohexyl methacrylate, isobornyl methacrylate, styrene, acrylonitrile, and vinyl acetate. The functional monomers include at least one of acrylic acid, methacrylic acid, itaconic acid, maleic acid, maleic anhydride, hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, acrylamide, methacrylamide, N-hydroxymethylacrylamide, and diacetone acrylamide.
4. The self-removing adhesive tape for lithium batteries according to any one of claims 1-3, characterized in that, The self-removable adhesive tape for lithium batteries further includes at least one of the following layers: 1) A hot melt adhesive layer is disposed on the side of the substrate layer away from the pressure-sensitive adhesive layer, with a thickness of 0.5 to 20 μm, an elongation at break of not less than 150%, and a room temperature elastic modulus of not less than 1 MPa. The hot melt adhesive layer includes at least one of rubber adhesives, polyolefin adhesives, polyester adhesives, epoxy adhesives, and silicone adhesives. 2) Release layer, disposed on the side of the pressure-sensitive adhesive layer away from the substrate layer, with a thickness of 12 to 100 μm, including single-sided release film or double-sided release film.
5. The self-removing adhesive tape for lithium batteries according to claim 4, characterized in that, A hot melt adhesive layer is included on the side of the substrate layer facing away from the pressure-sensitive adhesive layer, and the hot melt adhesive layer is the outermost layer; The hot melt adhesive layer comprises, by weight: 20-60 parts of polyolefin resin; 20-80 parts of tackifying resin; 0-20 parts of elastic component; Viscosity modifier 0-20 parts; 0-10 parts of color paste; The polyolefin resin includes at least one of EVA resin, α-olefin polymer resin and modified polyolefin resin, and the elastic component includes at least one of SBS, SIS and SEBS.
6. The self-removing adhesive tape for lithium batteries according to claim 4, characterized in that, An anti-stick layer is provided on the side of the hot melt adhesive layer away from the substrate layer, and the thickness of the anti-stick layer is not greater than 10 μm. The anti-stick layer includes at least one of the following: ceramic coating, epoxy coating, acrylic coating, polyolefin coating or emulsion microsphere coating, PET film layer, PI film layer, BOPP film layer, and PE film layer.
7. The self-removing adhesive tape for lithium batteries according to claim 4, characterized in that, The self-removing adhesive tape for lithium batteries includes multiple adhesive units spaced apart on the side of the release layer. Each adhesive unit includes the pressure-sensitive adhesive layer, the substrate layer, and the hot melt adhesive layer stacked sequentially from the release layer outwards.
8. A method for preparing a self-removing adhesive tape for lithium batteries as described in any one of claims 1-7, characterized in that, Includes the following steps: Step 1: Prepare pressure-sensitive adhesive coating solution: After diluting the acrylic masterbatch and optional solvent by stirring, add the curing component, stir, and let stand to remove bubbles; Step 2: Based on the solid content of the pressure-sensitive adhesive coating liquid and the target thickness of the pressure-sensitive adhesive layer, select an appropriate micro-grooved roller, apply the pressure-sensitive adhesive coating liquid onto the release layer, and dry it to form a pressure-sensitive adhesive layer. Step 3: Unwind the substrate layer and bond it to the pressure-sensitive adhesive layer to obtain a self-removing tape for lithium batteries comprising a substrate layer and a pressure-sensitive adhesive layer.
9. The preparation method according to claim 8, characterized in that, After bonding the substrate layer to the pressure-sensitive adhesive layer, the following steps are also included: Prepare a hot melt adhesive coating liquid, apply the hot melt adhesive coating liquid to the side of the substrate layer away from the pressure-sensitive adhesive layer, dry to form a hot melt adhesive layer, and roll up to obtain a self-detachable tape for lithium batteries. Optionally, after drying to form the hot melt adhesive layer, an anti-stick layer may be applied or bonded to the side of the hot melt adhesive layer away from the substrate layer; Optionally, each layer on the side of the release layer can be die-cut to form multiple bonding units at intervals.
10. A method for manufacturing an electrode using the self-detachable adhesive tape for lithium batteries according to any one of claims 1-7, characterized in that, Includes the following steps: S1. The pressure-sensitive adhesive layer of the self-removing tape is bonded to the electrode current collector to cover the reserved electrode tab area; S2. Apply electrode slurry to the surface of the electrode current collector and the self-detachable adhesive tape, and dry the electrode slurry to form an electrode active material layer; S3. Apply a roller pressure of more than 20 tons to the electrode active material layer for cold pressing. The substrate layer undergoes elastic deformation under force, which causes the pressure-sensitive adhesive layer to separate from the electrode current collector, so that the tape curls on the electrode current collector and automatically falls off, exposing the reserved tab area on the electrode current collector. S4. Forming a tab in the reserved tab area to obtain the electrode sheet.
Citation Information
Patent Citations
Lithium battery foaming adhesive tape as well as preparation process and preparation device thereof
CN115232570A
Heat-shrinkable adhesive tape for lithium ion battery tab welding position, application of heat-shrinkable adhesive tape and preparation method of lithium ion battery pole piece
CN120888248A