Insulating high-temperature-resistant mica tape for battery and preparation method thereof

By combining epoxy-based phenyl polysiloxane and polar-group modified flake silica, and combining them with thermally conductive fillers, the structural stability and heat dissipation performance of mica tape for batteries at high temperatures are improved, and the problems of insufficient compatibility and aging resistance of adhesive layers in existing technologies are solved.

CN123107594APending Publication Date: 2026-11-17JIANGYIN YOUJIA PEARLESCENT MICA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611189233.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-06
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing mica tapes for batteries lack structural stability and heat dissipation performance at high temperatures, and the compatibility and aging resistance of the adhesive layer need to be improved.

Method used

By compounding epoxy-based phenyl polysiloxane with polar-modified flake silica, the compatibility and flexural strength of the adhesive layer are improved, and thermally conductive fillers are added to enhance the thermal conductivity and high-temperature structural stability of the adhesive layer.

Benefits of technology

It enhances the high-temperature resistance and heat dissipation capacity of the mica tape, and improves the structural stability of the adhesive layer and the bonding strength between the adhesive layer and the mica paper layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention discloses a high-temperature resistant insulating mica tape for batteries, comprising a mica paper layer, a reinforcing material layer, and an adhesive layer connecting the mica paper layer and the reinforcing material layer. By weight, the adhesive layer comprises 100 parts epoxy resin, 10-18 parts epoxy-phenyl polysiloxane, 20-30 parts first thermally conductive filler, 1-3 parts flake silica, 75-85 parts curing agent, and 0.1-0.3 parts accelerator. The flake silica contains amino and epoxy groups. The first thermally conductive filler comprises modified flake hexagonal boron nitride and modified spherical nano-alumina. Modifying the flake silica with polar groups improves the compatibility of inorganic particles in the adhesive system. Combined with epoxy-phenyl polysiloxane, it improves the flexural strength of the adhesive layer and optimizes its aging resistance and heat resistance. The thermally conductive filler improves the thermal conductivity of the adhesive layer and also enhances the structural stability of the adhesive layer and the mica paper layer at high temperatures.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of insulating materials technology, specifically to an insulating high-temperature resistant mica tape for batteries and its preparation method. Background Technology

[0002] In new energy vehicles, with the continuous improvement of battery system energy density and power, how to more efficiently dissipate the heat generated during normal battery operation or thermal runaway, and maintain the temperature stability of the battery pack.

[0003] Mica tape is a sandwich composite material, comprising: mica paper, the main material that provides insulation and high-temperature resistance; reinforcing material bonded to one or both sides of the mica paper, which mainly provides mechanical strength to prevent the mica tape from breaking during winding and use; and adhesive, which firmly bonds the mica paper and reinforcing material together. The performance of the adhesive has a significant impact on the overall temperature resistance of the mica tape. Summary of the Invention

[0004] One of the objectives of this invention is to overcome the deficiencies in the prior art and provide a high-temperature resistant insulating mica tape for batteries. By compounding epoxy-based phenyl polysiloxane and polar-group modified flake silica, the compatibility of inorganic particles in the adhesive system is improved, thereby increasing the flexural strength of the adhesive layer and optimizing its aging resistance and heat resistance. The thermal conductivity of the adhesive layer is improved by using thermally conductive fillers, which enhances heat dissipation performance and also improves the structural stability of the adhesive layer and the mica paper layer at high temperatures.

[0005] To achieve the above-mentioned process effects, the technical solution of the present invention is as follows: a battery insulating high-temperature resistant mica tape, comprising a mica paper layer, a reinforcing material layer, and an adhesive layer connecting the mica paper layer and the reinforcing material layer. By mass parts, the adhesive layer comprises 100 parts of epoxy resin, 10-18 parts of epoxy-phenyl polysiloxane, 20-30 parts of a first thermally conductive filler, 1-3 parts of flake silica, 75-85 parts of curing agent, and 0.1-0.3 parts of accelerator. The sheet-like silica contains amino and epoxy groups; The first thermally conductive filler comprises modified plate-shaped hexagonal boron nitride and modified spherical nano-alumina.

[0006] Furthermore, by weight, the adhesive layer comprises 100 parts epoxy resin, 12-17 parts epoxy phenyl polysiloxane, 22-28 parts first thermally conductive filler, 1-3 parts flake silica, 78-83 parts curing agent, and 0.1-0.3 parts accelerator.

[0007] A preferred technical solution is that the sheet-like silica is obtained by reacting a mixed coupling agent under acidic conditions, wherein the mixed coupling agent is a combination of tetraethyl orthosilicate, γ-aminopropyltriethoxysilane and γ-(2,3-epoxypropoxy)propyltrimethoxysilane in a molar ratio of 1:0.2:0.2.

[0008] The preferred technical solution is that the modifier of the modified plate-like hexagonal boron nitride is a polyaminosilane coupling agent and / or octaaminopropyl cage-type polysilsesquioxane; the modifier of the modified spherical nano-alumina is a polyaminosilane coupling agent and / or octaaminopropyl cage-type polysilsesquioxane.

[0009] The preferred technical solution is that the first thermally conductive filler is modified spherical nano-alumina and modified plate-shaped hexagonal boron nitride in a mass ratio of (30~40):(60~70).

[0010] Furthermore, the first thermally conductive filler is modified spherical nano-alumina and modified plate-like hexagonal boron nitride in a mass ratio of (32~38):(62~68).

[0011] A preferred technical solution is that the epoxy-based phenyl polysiloxane comprises linear epoxy-based phenyl polysiloxane and branched epoxy-based phenyl polysiloxane in a mass ratio of 1:(2~3); The linear epoxy phenyl polysiloxane is obtained by mixing equimolar amounts of 3-glycidyl etheroxypropyl dimethoxymethylsilane and diphenylsilanediol, and reacting them at 75-80°C under the action of a strong alkali. The branched epoxy phenyl polysiloxane is obtained by mixing hexamethyldisiloxane, 3-glycidyl etheroxypropyltriethoxysilane and tetraethyl orthosilicate in a molar ratio of 3:7:5 and reacting them in an acid solution at a temperature of 70-75°C.

[0012] A preferred technical solution is that the epoxy resin is a combination of solid bisphenol A epoxy resin, liquid bisphenol A epoxy resin and phenolic epoxy resin, and the mass ratio of the solid bisphenol A epoxy resin, liquid bisphenol A epoxy resin and phenolic epoxy resin is (1~1.2):1:(2~2.5).

[0013] The preferred technical solution is that the mica basis weight of the mica paper layer is 100-125 g / m³. 2 The mica paper layer comprises 97%–99% mica flakes and 1%–3% of a second thermally conductive filler; The mica flakes comprise 70%–85% mica flakes of 50–80 mesh, 15%–25% mica flakes of 80–120 mesh, and the remainder mica flakes of 120–200 mesh. The second thermally conductive filler comprises modified spherical nano-alumina and modified plate-shaped hexagonal boron nitride in a mass ratio of 1:(2~4).

[0014] The preferred technical solution is that the reinforcing material layer is an electrical-grade alkali-free glass fiber cloth, a polyester film, or a polyimide film.

[0015] The second objective of this invention is to overcome the deficiencies in the prior art and provide a method for preparing insulating high-temperature resistant mica tape for batteries, comprising the following steps: S1: Prepare the mica paper layer and reinforcing material layer; S2: Apply adhesive to the surface of the reinforcing material layer, then stack the mica paper layer on top of the uncured adhesive, apply pressure and heat to cure, and form a high-temperature resistant mica tape; In step S3, the pressure applied is 15-20 MPa, and the heating temperature is 230-250°C.

[0016] A preferred technical solution is that, in step S1, an adhesion layer is provided on the surface of the reinforcing material layer.

[0017] The advantages and beneficial effects of this invention are as follows: By modifying the flake silica with polar groups, the compatibility of inorganic particles in the adhesive system is improved. When compounded with epoxy-based phenyl polysiloxane, the flexural strength of the adhesive layer is improved, as well as the aging resistance and heat resistance are optimized. The thermal conductivity of the adhesive layer is improved by using thermally conductive fillers, which also improves the structural stability of the adhesive layer and the mica paper layer at high temperatures. Detailed Implementation

[0018] The specific embodiments of the present invention will be further described below with reference to examples. These examples are only used to more clearly illustrate the technical solutions of the present invention and should not be construed as limiting the scope of protection of the present invention.

[0019] sheet silica Flake silica is obtained by reacting a mixture of tetraethyl orthosilicate, γ-aminopropyltriethoxysilane and γ-(2,3-epoxypropoxy)propyltrimethoxysilane in a molar ratio of 1:0.2:0.2 under acidic conditions.

[0020] Specifically, firstly, the acidic solution was prepared by adjusting the pH of 10g of water to 2.5 using 2M hydrochloric acid; secondly, the mixed coupling agent was prepared by combining 10.4g (0.05mol) of tetraethyl orthosilicate, 2.21g (0.01mol) of γ-aminopropyltriethoxysilane, and 2.36g (0.01mol) of γ-(2,3-epoxypropoxy)propyltrimethoxysilane; thirdly, the mixed coupling agent was dissolved in the acidic solution, and 8g of Span 80 and 120g of toluene were added to react and form a silica shell. The mixture was heated to 72-78℃ and magnetically stirred. Finally, the reactants were centrifuged, washed, and dried.

[0021] The raw materials of silica nanosheets are oriented, with hydrophilic amino groups spontaneously facing the aqueous phase and hydrophobic epoxy groups facing the oil phase. Under acidic conditions, an interfacial sol-gel forms a silica shell. Span 80, as an oil-soluble surfactant, occupies a certain position at the interface. After the high-speed shearing stops, demulsification occurs due to osmotic pressure, causing the silica shell to rupture and form silica nanosheets. One end of the silica nanosheet contains an amino group, and the other end contains an epoxy group. Therefore, the amino groups on the silica nanosheets crosslink with the epoxy resin matrix, and the epoxy groups can crosslink with the epoxy resin matrix through a curing agent, which not only improves compatibility but also enhances the strength and toughness of the adhesive layer.

[0022] Modified plate-like hexagonal boron nitride The modifiers for modified plate-like hexagonal boron nitride are polyaminosilane coupling agents and / or octaaminopropyl cage-type polysilsesquioxane.

[0023] Furthermore, the polyaminosilane coupling agent is obtained by reacting N-β(aminoethyl)-γ-aminopropyltrimethoxysilane (KH-792 coupling agent) and p-chlorotoluene in an equimolar ratio under the action of the polymerization inhibitor hydroquinone and the acid-binding agent triethylamine. p-Chlorotoluene is grafted onto the aminoethyl group of N-β(aminoethyl)-γ-aminopropyltrimethoxysilane.

[0024] Specifically, KH-792 coupling agent and toluene were mixed to prepare a 50% reaction solution. The temperature was raised to 45°C, and the polymerization inhibitor was dissolved in p-chlorotoluene and added dropwise to the reaction solution. After the addition was complete, the temperature was raised to 60°C, and the reaction was maintained at this temperature with stirring for 4 hours. Then, the temperature was raised to 80°C, and an acid-binding agent was added. The reaction was maintained at this temperature with stirring for 1 hour. After the reaction was completed, the mixture was filtered, washed, and precipitated. The washing liquid and filtrate were then distilled under reduced pressure, and the distillate of the product was collected. The amount of polymerization inhibitor added was 0.1% of p-chlorotoluene, and the amount of acid-binding agent added was 66% of p-chlorotoluene. The optimal process route using toluene as a solvent resulted in a more transparent product without precipitation.

[0025] Polyaminosilane coupling agent was used to modify plate-like hexagonal boron nitride. Hexagonal boron nitride (from Henan Nitrogen-Boron New Material Technology Co., Ltd., boron oxide content <0.6%) was dissolved in a 6 mol / L sodium hydroxide solution to prepare a 6 g / L dispersion. The mixture was reacted at 110°C for 60 h, filtered, and washed until neutral. The hydroxyl-modified hexagonal boron nitride powder was then dried for later use. The polyaminosilane coupling agent was fully dissolved in anhydrous ethanol at a mass ratio of 1:10 (polyaminosilane coupling agent to anhydrous ethanol) and 1:30 (polyaminosilane coupling agent to plate-like hexagonal boron nitride). The plate-like hexagonal boron nitride was then dissolved in the ethanol mixture and stirred for 5 h to perform amino grafting modification. The mixture was then centrifuged, filtered, washed with anhydrous ethanol, and dried at 65°C for later use.

[0026] Octaaminopropyl cage-type polysilsesquioxane (Xi'an Qiyue Biotechnology Co., Ltd.) was used to modify flake-shaped hexagonal boron nitride (h-BN). Hexagonal boron nitride (Henan Nitrogen Boron New Materials Technology Co., Ltd., boron oxide content <0.6%) was dissolved in a 6 mol / L sodium hydroxide solution to prepare a 6 g / L dispersion. The mixture was reacted at 110℃ for 60 h, filtered, and washed until neutral. The hydroxyl-modified hexagonal boron nitride powder was then dried for later use. Next, 100 g of the dried hydroxyl-modified hexagonal boron nitride powder was dissolved in a 50% isopropanol aqueous solution, and 10 g of octaaminopropyl cage-type polysilsesquioxane was added. The mixture was reacted at a water bath temperature of 55±2℃ for 4 h. After the reaction, the mixture was centrifuged, washed with deionized water until neutral, and then dried, ground, and sieved for further use.

[0027] Modified spherical nano-alumina The modifiers for the modified spherical nano-alumina are polyaminosilane coupling agents and / or octaaminopropyl cage-type polysilsesquioxane.

[0028] Hydroxyl-modified alumina: 10.2g of alumina (nano-grade, Hubei Huifu Nanomaterials Co., Ltd.) was dissolved in 300ml of 45% isopropanol aqueous solution. The pH of the solution was adjusted to 8 with ammonia. After mixing and stirring evenly, the solution was sonicated for 3 hours to obtain a suspension.

[0029] Spherical nano-alumina was modified with a polyaminosilane coupling agent. The polyaminosilane coupling agent was fully dissolved in anhydrous ethanol to obtain a modification solution. The mass ratio of polyaminosilane coupling agent to anhydrous ethanol in the modification solution was 1:10, and the mass ratio of polyaminosilane coupling agent to nano-alumina in the suspension was 1:30. Hydroxyl-modified alumina was then added and stirred for 4 hours to perform amino grafting modification. The mixture was then centrifuged, filtered, washed with anhydrous ethanol, and dried at 65°C for later use.

[0030] Octaaminopropyl cage-type polysilsesquioxane modified spherical nano-alumina: Octaaminopropyl cage-type polysilsesquioxane was added to a suspension, with a mass ratio of nano-alumina to octaaminopropyl cage-type polysilsesquioxane of 20:1. The mixture was reacted fully at a water bath temperature of 55±2℃ for 4 hours. After the reaction was completed, the mixture was centrifuged, washed with deionized water until neutral, and then dried, ground, and sieved for later use.

[0031] In modified hexagonal boron nitride sheets and modified spherical nano-alumina, the secondary amine structure of the polyaminosilane coupling agent endows the coupling agent with the ability to chemically react with various reactive monomers, exhibiting excellent coupling effects, improving the compatibility of inorganic fillers in epoxy resin systems, and the aromatic system imparts excellent thermal stability. By introducing a large number of active amino groups onto the surface of h-BN or alumina using octaaminopropyl cage-like polysilsesquioxane, a strong chemical bond with epoxy resin is achieved. Furthermore, the nanocage-like structure of the octaaminopropyl cage-like polysilsesquioxane not only improves dispersibility but also further enhances the comprehensive mechanical and thermal properties of the adhesive layer.

[0032] Epoxyphenyl polysiloxane Epoxy-based phenyl polysiloxanes include linear epoxy-based phenyl polysiloxanes and branched epoxy-based phenyl polysiloxanes.

[0033] Linear epoxy-based phenyl polysiloxanes are obtained by preparing a first mixed siloxane using equimolar amounts of 3-glycidyl etheroxypropyl dimethoxymethylsilane and diphenylsilanediol, adding barium hydroxide at a total mass fraction of 0.2% of the first mixed siloxane, and reacting under strong alkali conditions at 78°C. Due to the steric hindrance of phenyl groups, self-condensation is difficult to occur, and non-hydrolysis reaction conditions can also inhibit the self-condensation of silanes, resulting in a linear epoxy-based phenyl polysiloxane with alternating straight-chain backbones of 3-glycidyl etheroxypropyl dimethoxymethylsilane and diphenylsilanediol.

[0034] Linear epoxy phenyl polysiloxanes contain epoxy groups and phenyl groups, which can improve compatibility with epoxy resins and increase the crosslinking density and heat resistance of the adhesive layer.

[0035] Branched epoxy-based polysiloxanes were prepared by mixing hexamethyldisiloxane, 3-glycidyl etheroxypropyltriethoxysilane, and tetraethyl orthosilicate in a molar ratio of 3:7:5 to form a second mixed siloxane. Anhydrous ethanol, glacial acetic acid, and deionized water were prepared in a mass ratio of 3:1:3.5 to form an acid solution. The mixed siloxane and acid solution were then mixed in a ratio of 2.2:1 and reacted at 73°C. Glacial acetic acid, acting as a catalyst, primarily promotes the hydrolysis reaction by protonating the oxygen atoms of the siloxane to lower the activation energy of the hydrolysis reaction. In addition, water molecules, acting as nucleophiles, can simultaneously lower the activation energies of hydrolysis and polycondensation. The synergistic effect of these two factors achieves the hydrolytic condensation of the polysiloxane. Under these reaction conditions, the epoxy groups are hardly induced to open.

[0036] Branched epoxy-based polysiloxanes offer higher crosslinking density and rigidity, forming a three-dimensional network structure while also exhibiting excellent heat resistance. Combining branched epoxy-based polysiloxanes balances toughening and rigidity, while ensuring the heat resistance of the adhesive layer.

[0037] Epoxy resin Epoxy resin is a combination of solid bisphenol A epoxy resin, liquid bisphenol A epoxy resin and phenolic epoxy resin.

[0038] In the combination, liquid bisphenol A epoxy resin (E-51) has a low viscosity and acts as a toughening resin, which can effectively reduce the viscosity of the entire adhesive system, improve the wettability of the mica paper layer and reinforcing materials, and provide good flexibility and adhesion after curing, preventing the mica tape from cracking during wrapping.

[0039] In the combination, solid bisphenol A epoxy resin (E-20) is a solid resin that acts as a tackifier, which can significantly improve the rigidity and cohesive strength of the adhesive layer. In mica tape, it can improve the stiffness and strength of the tape, making it easier to handle and wrap, and can also reduce the shrinkage rate of the system after curing.

[0040] In the combination, phenolic epoxy resin (F-44 or F-51) serves as the resin for heat resistance enhancement. It belongs to the category of multifunctional epoxy resins and has a crosslinking density much higher than that of ordinary bisphenol A type epoxy resins. Therefore, it can significantly improve the heat resistance, chemical resistance and dimensional stability of adhesives. In mica tape applications, it can achieve a heat resistance rating of F grade (155℃) or higher.

[0041] mica paper layer The mica paper layer comprises mica flakes and a second thermally conductive filler. The mica flakes include 50-80 mesh, 80-120 mesh, and 120-200 mesh flakes. Large-diameter, high aspect ratio mica flakes form the skeleton of the mica paper, determining the foundation of its mechanical strength and insulation properties. Finer flakes fill the gaps between the coarser flakes, forming a denser paper structure, improving uniformity and reducing porosity. This also facilitates the dispersion of the second thermally conductive filler within the gaps, enhancing the thermal conductivity of the mica paper layer. If the proportion of finer flakes is too low, it hinders the formation of the densest packing structure, negatively impacting the uniformity, electrical strength, and mechanical strength of the mica paper layer. Conversely, if the proportion is too high, it impedes the filling and dispersion of the second thermally conductive filler.

[0042] The second thermally conductive filler consists of modified spherical nano-alumina and modified flake-shaped hexagonal boron nitride, which improve the interfacial compatibility and bonding strength between the mica paper layer and the adhesive layer.

[0043] Reinforcing material layer The reinforcing material layer is electrical grade alkali-free glass fiber cloth, polyester film, or polyimide film.

[0044] Electrical-grade alkali-free fiberglass cloth is impregnated with a surface treatment agent and then dried to obtain an adhesion layer, thereby improving the bonding strength with the adhesive layer. The surface treatment agent is prepared by adding acetic acid to 100 mL of water at 20–30°C to adjust the pH to 2–3, obtaining an acidic solution. Then, 1%–3% of the aforementioned polyaminosilane coupling agent, 0.05%–0.1% of polyether-modified trisiloxane (CAS 67674-67-3), and 0.04%–0.08% of defoamer (BYK-028) are added to the acidic solution, and the mixture is stirred to obtain a clear and transparent fiberglass cloth surface treatment agent. The surfactant primarily enhances the penetration rate of the treatment agent, ensuring that it covers the fiberglass cloth surface quickly and within a short time. Impregnation modification: The fiberglass cloth is treated with acetone solution to remove surface slurry, washed, and dried for later use. The deslurried fiberglass cloth is then impregnated in the surface treatment agent for 8 hours, followed by drying, washing, and then drying again to obtain fiberglass cloth with an adhesion layer modification.

[0045] Polyester and polyimide films undergo surface corona treatment, with the corona layer serving as the adhesion layer. This improves the bond strength with the adhesive layer.

[0046] Example 1

[0047] The battery insulating high-temperature resistant mica tape includes a mica paper layer, a reinforcing material layer, and an adhesive layer connecting the mica paper layer and the reinforcing material layer.

[0048] By weight, the adhesive layer comprises 100 parts epoxy resin, 15 parts epoxy-based phenyl polysiloxane, 24 parts primary thermally conductive filler, 2 parts flake silica, 82 parts curing agent (methylhexahydrophthalic anhydride), and 0.2 parts accelerator (aluminum acetylacetonate). The adhesive content is 12 g / m³. 2 .

[0049] Flake silica is obtained by reacting a mixture of tetraethyl orthosilicate, γ-aminopropyltriethoxysilane and γ-(2,3-epoxypropoxy)propyltrimethoxysilane as a coupling agent in a molar ratio of 1:0.2:0.2 under acidic conditions.

[0050] The first thermally conductive filler is a mixture of modified spherical nano-alumina and modified plate-like hexagonal boron nitride in a mass ratio of 34:66.

[0051] Among them, the modifier for modified plate-like hexagonal boron nitride is a polyaminosilane coupling agent; the modifier for modified spherical nano-alumina is a polyaminosilane coupling agent.

[0052] Epoxyphenyl polysiloxanes include linear epoxyphenyl polysiloxanes and branched epoxyphenyl polysiloxanes in a mass ratio of 1:2.5. The linear epoxyphenyl polysiloxane is obtained by mixing equimolar amounts of 3-glycidyl etheroxypropyl dimethoxymethylsilane and diphenylsilanediol, and reacting them at 78°C under the action of a strong alkali. The branched epoxyphenyl polysiloxane is obtained by mixing hexamethyldisiloxane, 3-glycidyl etheroxypropyl triethoxysilane, and tetraethyl orthosilicate in a molar ratio of 3:7:5, and reacting them at 73°C under the action of an acid solution.

[0053] The epoxy resin is a combination of solid bisphenol A epoxy resin, liquid bisphenol A epoxy resin and phenolic epoxy resin in a mass ratio of 1:1:2.2.

[0054] The mica basis weight of the mica paper layer is 115 g / m³. 2 The mica paper layer comprises 98% mica flakes and 2% of a second thermally conductive filler; wherein, the mica flakes comprise 80% of 50-80 mesh mica flakes, 16% of 80-120 mesh mica flakes, and the remainder of 120-200 mesh mica flakes; the second thermally conductive filler comprises modified spherical nano-alumina and modified flake-shaped hexagonal boron nitride in a mass ratio of 1:3.

[0055] The reinforcing material layer has a basis weight of 28 g / m³. 2 Electrical grade alkali-free glass fiber cloth is obtained by impregnation and modification with the above-mentioned surface treatment agent.

[0056] The preparation method of high-temperature resistant insulating mica tape for batteries includes the following steps: S1: Prepare the mica paper layer and reinforcing material layer; S2: Apply adhesive to the surface of the reinforcing material layer, then stack the mica paper layer on top of the uncured adhesive, apply pressure and heat to cure, forming a high-temperature resistant mica tape. The pressure applied is 16 MPa, and the heating temperature is 240°C.

[0057] Example 2

[0058] Example 2 is based on Example 1, except that, by weight, the adhesive layer comprises 100 parts epoxy resin, 10 parts epoxy phenyl polysiloxane, 24 parts first thermally conductive filler, 2 parts flake silica, 82 parts curing agent (methylhexahydrophthalic anhydride), and 0.2 parts accelerator (aluminum acetylacetonate). Other components and processes remain unchanged.

[0059] Example 3

[0060] Example 3 is based on Example 1, except that, by weight, the adhesive layer comprises 100 parts epoxy resin, 18 parts epoxy-phenyl polysiloxane, 24 parts first thermally conductive filler, 2 parts flake silica, 82 parts curing agent (methylhexahydrophthalic anhydride), and 0.2 parts accelerator (aluminum acetylacetonate). The composition of other layers and the process remain unchanged.

[0061] Example 4

[0062] Example 4 is based on Example 1, except that the modifier for the modified plate-like hexagonal boron nitride is octaaminopropyl cage-type polysilsesquioxane; the modifier for the modified spherical nano-alumina is also octaaminopropyl cage-type polysilsesquioxane, while other components remain unchanged. The composition of the other layers and the process remain unchanged.

[0063] Example 5

[0064] Example 5 is based on Example 1, except that the epoxy-based phenyl polysiloxane is only a linear epoxy-based phenyl polysiloxane, while other components remain unchanged. The composition of the other layers and the process remain unchanged.

[0065] Example 6

[0066] Example 6 is based on Example 1, except that the epoxy-based phenyl polysiloxane is only a branched epoxy-based phenyl polysiloxane, while the other components remain unchanged. The composition of the other layers and the process remain unchanged.

[0067] Example 7

[0068] Example 7 is based on Example 1, except that the modifier for both the modified plate-like hexagonal boron nitride and the modified spherical nano-alumina is γ-aminopropyltriethoxysilane, while other components remain unchanged. The composition of the other layers and the process remain the same.

[0069] Example 8

[0070] Example 8 is based on Example 1, except that the epoxy resin is a combination of solid bisphenol A epoxy resin, liquid bisphenol A epoxy resin, and phenolic epoxy resin in a mass ratio of 1:1:1, while other components remain unchanged. The composition of the other layers and the process remain unchanged.

[0071] Comparative Example 1 Comparative Example 1 is based on Example 1, except that flake silica was not added to the adhesive layer, while other components remained unchanged. The composition of the other layers and the process remained the same.

[0072] Comparative Example 2 Comparative Example 2 is based on Example 1, except that, by weight, the adhesive layer comprises 100 parts epoxy resin, 4 parts epoxy-phenyl polysiloxane, 24 parts first thermally conductive filler, 2 parts flake silica, 82 parts curing agent (methylhexahydrophthalic anhydride), and 0.2 parts accelerator (aluminum acetylacetonate). The composition of other layers and the process remain unchanged.

[0073] Performance testing of mica tape in both the example and comparative examples: 1. Electrical strength: Measured according to GB / T 5019 standard; 2. Heat resistance: Tested according to GB / T 5019 standard; 3. Aging resistance: Performance retention rate after aging at 200℃ for 168 hours, as determined according to GB / T 5019 standard; 4. Bending strength: Measured according to GB / T 5019 standard; 5. Thermal conductivity: Measured according to GB / T 10297 standard.

[0074] The performance test results of the examples and comparative examples are as follows:

[0075] The electrical strength is mainly determined by the mica layer, but breakdown often occurs at relatively weak interfaces and adhesive layers. Therefore, the thermal stability of the adhesive layer is also crucial to the electrical strength.

[0076] Compared to Example 1, Example 2 has a reduced content of epoxy-based phenyl polysiloxane, which has a negative impact on aging resistance and flexural strength.

[0077] Compared to Example 1, Example 3 shows an increased content of epoxy-based phenyl polysiloxane, which negatively affects the crosslinking density of the epoxy resin system's crosslinking structure, and consequently has a negative impact on flexural strength and aging resistance.

[0078] Compared to Example 1, Example 4 shows that the octaaminopropyl cage-type polysilsesquioxane-modified sheet-like hexagonal boron nitride and spherical nano-alumina have better dispersibility of thermally conductive fillers and better performance improvement.

[0079] Compared to Example 1, Examples 5 and 6 show better performance when linear epoxy-based phenyl polysiloxane and branched epoxy-based phenyl polysiloxane are used in combination.

[0080] Compared to Example 1, Example 7 shows that the thermally conductive filler is more uniformly dispersed in γ-aminopropyltriethoxysilane-modified plate-like hexagonal boron nitride and spherical nano-alumina, but the crosslinking density is reduced, which has a negative impact on aging resistance.

[0081] Compared to Example 1, in Example 8, the content of phenolic epoxy resin in the epoxy resin combination is too low, which has a negative impact on heat resistance, flexural strength and aging resistance.

[0082] Compared to Example 1, Comparative Example 1 did not add flake silica to the adhesive layer, which negatively affected both flexural strength and aging resistance.

[0083] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the technical principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A high-temperature resistant insulating mica tape for batteries, comprising a mica paper layer, a reinforcing material layer, and an adhesive layer connecting the mica paper layer and the reinforcing material layer, characterized in that, By weight, the adhesive layer comprises 100 parts epoxy resin, 10-18 parts epoxy phenyl polysiloxane, 20-30 parts first thermally conductive filler, 1-3 parts flake silica, 75-85 parts curing agent and 0.1-0.3 parts accelerator; The sheet-like silica contains amino and epoxy groups; The first thermally conductive filler comprises modified plate-shaped hexagonal boron nitride and modified spherical nano-alumina.

2. The high-temperature resistant insulating mica tape for batteries according to claim 1, characterized in that, The sheet-like silica is obtained by reacting a mixed coupling agent under acidic conditions. The mixed coupling agent is a combination of tetraethyl orthosilicate, γ-aminopropyltriethoxysilane and γ-(2,3-epoxypropoxy)propyltrimethoxysilane in a molar ratio of 1:0.2:0.

2.

3. The high-temperature resistant insulating mica tape for batteries according to claim 1, characterized in that, The modifier for the modified plate-like hexagonal boron nitride is a polyaminosilane coupling agent and / or octaaminopropyl cage-type polysilsesquioxane; the modifier for the modified spherical nano-alumina is a polyaminosilane coupling agent and / or octaaminopropyl cage-type polysilsesquioxane.

4. The high-temperature resistant insulating mica tape for batteries according to claim 1 or 3, characterized in that, The first thermally conductive filler is modified spherical nano-alumina and modified plate-shaped hexagonal boron nitride in a mass ratio of (30~40):(60~70).

5. The high-temperature resistant insulating mica tape for batteries according to claim 1, characterized in that, The epoxy-based phenyl polysiloxane comprises linear epoxy-based phenyl polysiloxane and branched epoxy-based phenyl polysiloxane in a mass ratio of 1:(2~3); The linear epoxy phenyl polysiloxane is obtained by mixing equimolar amounts of 3-glycidyl etheroxypropyl dimethoxymethylsilane and diphenylsilanediol, and reacting them at 75-80°C under the action of a strong alkali. The branched epoxy phenyl polysiloxane is obtained by mixing hexamethyldisiloxane, 3-glycidyl etheroxypropyltriethoxysilane and tetraethyl orthosilicate in a molar ratio of 3:7:5 and reacting them in an acid solution at a temperature of 70-75°C.

6. The high-temperature resistant insulating mica tape for batteries according to claim 1 or 5, characterized in that, The epoxy resin is a combination of solid bisphenol A epoxy resin, liquid bisphenol A epoxy resin and phenolic epoxy resin, and the mass ratio of the solid bisphenol A epoxy resin, liquid bisphenol A epoxy resin and phenolic epoxy resin is (1~1.2):1:(2~2.5).

7. The high-temperature resistant insulating mica tape for batteries according to claim 3, characterized in that, The mica basis weight of the mica paper layer is 100-125 g / m³. 2 The mica paper layer comprises 97%–99% mica flakes and 1%–3% of a second thermally conductive filler; The mica flakes comprise 70%–85% mica flakes of 50–80 mesh, 15%–25% mica flakes of 80–120 mesh, and the remainder mica flakes of 120–200 mesh. The second thermally conductive filler comprises modified spherical nano-alumina and modified plate-shaped hexagonal boron nitride in a mass ratio of 1:(2~4).

8. The high-temperature resistant insulating mica tape for batteries according to claim 1, characterized in that, The reinforcing material layer is an electrical-grade alkali-free glass fiber cloth, polyester film, or polyimide film.

9. A method for preparing a high-temperature resistant insulating mica tape for batteries, characterized in that, Includes the following steps: S1: Prepare the mica paper layer and reinforcing material layer; S2: Apply adhesive to the surface of the reinforcing material layer, then stack the mica paper layer on top of the uncured adhesive, apply pressure and heat to cure, and form a high-temperature resistant mica tape; In step S3, the pressure applied is 15-20 MPa, and the heating temperature is 230-250°C.

10. The method for preparing high-temperature resistant insulating mica tape for batteries according to claim 9, characterized in that, In S1, an adhesion layer is provided on the surface of the reinforcing material layer.