A carbon nanotube / molybdenum disulfide@carbon foam-paraffin composite phase change material, its preparation method and application
By constructing a continuous, low-thermal-resistance three-dimensional thermally conductive network using carbon nanotubes/molybdenum disulfide@carbon foam-paraffin composite material, the leakage and thermal conductivity problems of paraffin phase change materials are solved, enabling efficient thermal management applications.
Patent Information
- Application Number
- CN202611350060.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-02
- Publication Date
- 2026-11-17
AI Technical Summary
Existing paraffin phase change materials suffer from problems such as easy leakage, low thermal conductivity, and slow thermal response, making them difficult to apply in efficient thermal management systems.
A continuous, low-thermal-resistance three-dimensional thermally conductive network was constructed using carbon nanotubes/molybdenum disulfide@carbon foam-paraffin composite material through modification reaction and vacuum impregnation, pressing, coating and encapsulation processes. This combined the three-dimensional pore network of carbon foam and the synergistic thermal conductivity of carbon nanotubes/molybdenum disulfide.
The thermal conductivity is significantly improved to 0.275 W/(m·K), and leakage is prevented through a dual liquid-locking mechanism. The material is flexible and fits irregular surfaces, reducing interfacial contact thermal resistance.
Smart Images

Figure CN123107629A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of interface materials technology for phase change energy storage and thermal management, and particularly to a carbon nanotube / molybdenum disulfide@carbon foam-paraffin composite phase change material, its preparation method and application. Background Technology
[0002] With the rapid development of electronic communications, new energy batteries, and high-power chip industries, the heat flux density generated by equipment during operation has increased dramatically. Achieving efficient heat dissipation and temperature control has become a key bottleneck restricting the performance and lifespan of sophisticated equipment. Phase change thermal energy storage materials (PCMs), utilizing their ability to absorb or release large amounts of latent heat during phase transitions, can effectively achieve "peak shaving and valley filling" temperature regulation, making them highly favored in the field of thermal management.
[0003] Paraffin wax has great application development value due to its high phase transition enthalpy, stable chemical properties, and low cost. However, pure paraffin wax faces two inherent technical defects in practical applications: first, it is prone to liquid leakage during solid-liquid phase transition, posing a serious safety hazard; second, its intrinsic thermal conductivity is extremely low, resulting in a slow internal thermal response and limiting its heat storage and release rates.
[0004] To address the leakage problem, porous carbon foam can be used as a supporting framework to physically encapsulate paraffin. However, a simple "carbon foam + paraffin" system cannot completely solve the leakage problem, and its thermal conductivity remains low (typically only around 0.12 W / (m·K)). To improve thermal conductivity, researchers have tried adding highly thermally conductive inorganic fillers (such as simple two-dimensional sheet materials). However, inorganic fillers are prone to agglomeration or "face-to-face" stacking (i.e., π-π interactions) in organic matrices. This not only significantly reduces the effective specific surface area of the filler but also leads to huge interfacial contact thermal resistance between fillers, causing severe scattering of phonons (the carriers of heat transfer) during transmission, thus hindering the improvement of thermal conductivity.
[0005] Therefore, how to break the stacking limitation of single fillers in the phase change system through the design and compounding of microstructures and construct a continuous, low thermal resistance, three-dimensional high-efficiency heat conduction network is a technical problem that urgently needs to be solved in this field. Summary of the Invention
[0006] In view of this, the present invention provides a method for preparing carbon nanotube / molybdenum disulfide@carbon foam-paraffin composite phase change material to solve the problems of easy leakage, extremely low intrinsic thermal conductivity, and slow thermal response of existing paraffin phase change materials.
[0007] To achieve the above objectives, the present invention adopts the following technical solution: A method for preparing a carbon nanotube / molybdenum disulfide@carbon foam-paraffin composite phase change material includes the following steps: 1) Carbon nanotubes, molybdenum disulfide, silane coupling agent and mixed solvent are mixed and modified to obtain surface-modified thermally conductive filler. 2) The surface-modified thermally conductive filler is melt-mixed with paraffin wax to obtain a modified paraffin wax phase change material; 3) The foamed carbon was immersed in the molten modified paraffin phase change material and vacuum melt impregnation was performed to obtain the carbon nanotube / molybdenum disulfide@foamed carbon-paraffin composite phase change material precursor; 4) The carbon nanotube / molybdenum disulfide@carbon foam-paraffin composite phase change material precursor is sequentially pressed and coated to obtain the carbon nanotube / molybdenum disulfide@carbon foam-paraffin composite phase change material.
[0008] Preferably, the mass-to-volume ratio of carbon nanotubes, molybdenum disulfide, silane coupling agent, and mixed solvent in step 1) is 1~5g: 1~10g: 0.5~1g: 100mL; The modification reaction is carried out at a temperature of 60-70°C for 3-5 hours.
[0009] Preferably, the carbon nanotubes have a diameter of 30-50 nm and a length of 10-20 μm; The particle size of the molybdenum disulfide is 6~8μm; The silane coupling agent includes one or more of γ-(methacryloyloxy)propyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, and γ-aminopropyltriethoxysilane. The mixed solvent includes an alcohol-water mixed solvent, wherein the volume ratio of alcohol to water in the alcohol-water mixed solvent is 90~98:2~10.
[0010] Preferably, the mass ratio of the surface-modified thermally conductive filler to paraffin wax in step 2) is 1:8~10; The melting and mixing temperature is 90~100℃.
[0011] Preferably, the vacuum degree of the vacuum melt impregnation in step 3) is -0.2 to -0.01 MPa, and the time is 1.8 to 2.5 h.
[0012] Preferably, the pressing pressure in step 4) is 7~12MPa.
[0013] Preferably, the coating and encapsulation in step 4) involves coating the surface of the pressed carbon nanotube / molybdenum disulfide@carbon foam-paraffin composite phase change material with a water-based polyurethane protective layer.
[0014] Another objective of this invention is to provide a carbon nanotube / molybdenum disulfide@carbon foam-paraffin composite phase change material prepared by the above-described preparation method.
[0015] Another object of the present invention is to provide an application of carbon nanotube / molybdenum disulfide@carbon foam-paraffin composite phase change material in power battery thermal management systems, high-power chip heat dissipation, or thermal energy regulation of microelectronic packaging devices.
[0016] As can be seen from the above technical solution, compared with the prior art, the present invention has the following beneficial effects: 1. Significant Thermal Conductivity: A "line-surface" synergistic multidimensional thermal conductivity pathway is constructed using one-dimensional carbon nanotubes (CNTs) and two-dimensional MoS2. CNTs act as a "physical spacer," preventing layer stacking and building thermal bridges between layers, significantly reducing interfacial contact thermal resistance. This results in a jump in the thermal conductivity of the composite material from 0.12 W / (m·K) of the unmodified PW composite phase change material to 0.275 W / (m·K), an increase of up to 129%.
[0017] 2. Excellent leak-proof performance: The well-developed three-dimensional pore network inside the foamed carbon exerts a strong capillary confinement effect on the liquid paraffin. Combined with the surface coating and encapsulation, it forms a dual liquid-locking mechanism, so that the material has almost no mass loss after multiple phase change cycles.
[0018] 3. Excellent flexibility and fit: The flattening process breaks through the rigidity limitations of traditional foam carbon. Combined with flexible coating and encapsulation, the material can perfectly fit the surface of irregular heat sources, greatly reducing the interfacial contact thermal resistance in practical applications. Attached Figure Description
[0019] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the provided drawings without creative effort.
[0020] Figure 1 This is a schematic diagram of the structure of the carbon nanotube / molybdenum disulfide@carbon foam-paraffin composite phase change material prepared in this invention. Detailed Implementation
[0021] This invention provides a method for preparing a carbon nanotube / molybdenum disulfide@carbon foam-paraffin composite phase change material, comprising the following steps: 1) Carbon nanotubes, molybdenum disulfide, silane coupling agent and mixed solvent are mixed and modified to obtain surface-modified thermally conductive filler. 2) The surface-modified thermally conductive filler is melt-mixed with paraffin wax to obtain a modified paraffin wax phase change material; 3) The foamed carbon was immersed in the molten modified paraffin phase change material and vacuum melt impregnation was performed to obtain the carbon nanotube / molybdenum disulfide@foamed carbon-paraffin composite phase change material precursor; 4) The carbon nanotube / molybdenum disulfide@carbon foam-paraffin composite phase change material precursor is sequentially pressed and coated to obtain the carbon nanotube / molybdenum disulfide@carbon foam-paraffin composite phase change material.
[0022] In this invention, the mass-volume ratio of carbon nanotubes, molybdenum disulfide, silane coupling agent and mixed solvent in step 1) is 1~5g:1~10g:0.5~1g:100mL, preferably 2~4g:2~8g:0.6~0.9g:100mL, more preferably 3g:4~6g:0.7~0.8g:100mL, and even more preferably 3g:5g:0.75g:100mL.
[0023] In this invention, the mass ratio of carbon nanotubes to molybdenum disulfide can be 1:1, 1:2, 1:3, 1:4, 1:5, 1:7, or 1:10.
[0024] In this invention, the temperature of the modification reaction is 60~70℃, specifically 62℃, 64℃, 65℃, 66℃, or 68℃; the time is 3~5h, specifically 3.5h, 4h, or 4.5h.
[0025] In this invention, the carbon nanotubes have a diameter of 30-50 nm, specifically 32 nm, 35 nm, 38 nm, 40 nm, 42 nm, 45 nm, or 48 nm; and a length of 10-20 μm, specifically 12 μm, 14 μm, 15 μm, 16 μm, or 18 μm; the molybdenum disulfide has a particle size of 6-8 μm, specifically 6.2 μm, 6.5 μm, 6.8 μm, 7 μm, 7.2 μm, 7.5 μm, or 7.8 μm; and the silane coupling agent includes one or more of γ-(methacryloyloxy)propyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, and γ-aminopropyltriethoxysilane.
[0026] In this invention, the mixed solvent includes an alcohol-water mixed solvent, wherein the volume ratio of alcohol to water in the alcohol-water mixed solvent is 90~98:2~10, preferably 92~96:4~8, and more preferably 95:5; the alcohol is preferably ethanol. In this invention, the alcohol in the alcohol-water system is responsible for dissolving, wetting, and dispersing, while the water is responsible for the hydrolysis of the silane coupling agent.
[0027] In this invention, the mass ratio of the surface-modified thermally conductive filler to paraffin wax in step 2) is 1:8~10, preferably 1:8.5~9.5, and more preferably 1:9.
[0028] In this invention, the melting and mixing temperature is 90~100℃, specifically 92℃, 94℃, 95℃, 96℃, or 98℃.
[0029] In this invention, the vacuum degree of vacuum melt impregnation in step 3) is -0.2 to -0.01 MPa, specifically -0.18 MPa, -0.15 MPa, -0.12 MPa, -0.1 MPa, -0.08 MPa, -0.05 MPa, or -0.02 MPa; the time is 1.8 to 2.5 h, specifically 1.9 h, 2 h, 2.1 h, 2.2 h, 2.3 h, or 2.4 h.
[0030] In this invention, the pressing pressure in step 4) is 7~12MPa, specifically 8MPa, 9MPa, 10MPa, or 11MPa. The pressing described in this invention is a surface flattening process, specifically flattening the surface of the composite phase change material precursor without damaging the structure of the carbon foam.
[0031] In this invention, the coating and encapsulation described in step 4) involves coating the surface of the pressed carbon nanotube / molybdenum disulfide@carbon foam-paraffin composite phase change material with an aqueous polyurethane protective layer.
[0032] In this invention, the thickness of the waterborne polyurethane protective layer is preferably 1 to 3 mm, specifically 1.2 mm, 1.5 mm, 1.8 mm, 2 mm, 2.2 mm, 2.5 mm, or 2.8 mm.
[0033] The present invention also provides a carbon nanotube / molybdenum disulfide@carbon foam-paraffin composite phase change material prepared by the above preparation method.
[0034] This invention also provides an application of carbon nanotube / molybdenum disulfide@carbon foam-paraffin composite phase change material in power battery thermal management systems, high-power chip heat dissipation, or thermal energy regulation of microelectronic packaging devices.
[0035] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0036] Example 1
[0037] S1. Foamed carbon pretreatment: Immerse commercially available foamed carbon completely in anhydrous ethanol, ultrasonically clean for 15 minutes, remove and place in an 80℃ oven to dry thoroughly for later use.
[0038] S2. Surface Modification of Thermally Conductive Filler: Add 100 mL of an ethanol / water mixture (anhydrous ethanol to water volume ratio of 95:5) to a beaker, and drop in 0.5 g of KH570 silane coupling agent. Stir mechanically at room temperature for 0.5 h. Add 10 g of thermally conductive filler, wherein the mass ratio of one-dimensional tubular CNTs (diameter 30-50 nm, length 10-20 μm) to two-dimensional sheet-like MoS2 (particle size 6-8 μm) is 1:1. Heat the system to 65 °C and continue heating and stirring for 4 h. After the reaction is complete, centrifuge to separate the lower solid phase, and dry in an oven for 12 h to obtain the surface-modified thermally conductive filler.
[0039] S3. Preparation of composite phase change matrix: The surface-modified thermally conductive filler and solid paraffin are accurately weighed and mixed at a mass ratio of 1:9, placed in a 90℃ oven to melt, and mechanically stirred to disperse them evenly to obtain the modified paraffin phase change material.
[0040] S4. Vacuum Impregnation: Keep the modified paraffin phase change material in a molten state at 90℃, immerse the pretreated foamed carbon in it, and then perform vacuum treatment in a vacuum oven at a vacuum degree of -0.1 MPa for 2 hours. After removing the vacuum, wipe off the excess paraffin from the surface while it is still hot.
[0041] S5. Flattening and Coating Encapsulation: The sample is placed between two smooth steel plates and flattened under a pressure of 10 MPa. Then, waterborne polyurethane (WPU) is uniformly coated onto both sides of the sample and allowed to cure statically to form a 2 mm thick film, creating a polyurethane encapsulation layer. This yields a highly thermally conductive carbon nanotube / molybdenum disulfide@foamed carbon-paraffin composite phase change material, as shown in the schematic diagram below. Figure 1 As shown.
[0042] Example 2
[0043] The only difference between this embodiment and Embodiment 1 is that the mass ratio of one-dimensional tubular CNTs to two-dimensional sheet MoS2 is adjusted to 1:2.
[0044] Example 3
[0045] The only difference between this embodiment and Embodiment 1 is that the mass ratio of one-dimensional tubular CNTs to two-dimensional sheet MoS2 is adjusted to 1:3.
[0046] Example 4
[0047] The only difference between this embodiment and Embodiment 1 is that the mass ratio of one-dimensional tubular CNTs to two-dimensional sheet MoS2 is adjusted to 1:4.
[0048] Example 5
[0049] The only difference between this embodiment and Embodiment 1 is that the mass ratio of one-dimensional tubular CNTs to two-dimensional sheet MoS2 is adjusted to 1:5.
[0050] Example 6
[0051] The only difference between this embodiment and Embodiment 1 is that the mass ratio of one-dimensional tubular CNTs to two-dimensional sheet MoS2 is adjusted to 1:7.
[0052] Example 7
[0053] The only difference between this embodiment and Embodiment 1 is that the mass ratio of one-dimensional tubular CNTs to two-dimensional sheet MoS2 is adjusted to 1:10.
[0054] Comparative Example 1
[0055] Pure "foamed charcoal + paraffin" system
[0056] The only difference between this comparative example and Example 1 is that no surface-modified thermally conductive filler is added.
[0057] Comparative Example 2
[0058] Unmodified filler control system
[0059] The only difference between this comparative example and Example 1 is that KH570 silane coupling agent is not added, and untreated CNTs and MoS2 (in the same amount as in Example 1) are directly mixed with paraffin for impregnation.
[0060] Performance testing
[0061] The composite phase change materials obtained in Examples 1-7 and Comparative Examples 1-2 were subjected to performance tests, including the determination of thermal conductivity: a TIM-Tester (TIM L58) thermal interface material tester from Lindsay, Germany, was used, and the test method was performed according to ASTM D5470 standard. The thermal conductivity of the material was determined by using a 25 mm diameter circular sample for the thermal interface material test, and the test was repeated three times, and the average value was taken. The phase change enthalpy of melting (kJ / kg) and crystallization enthalpy (kJ / kg) of the material were tested using a differential scanning calorimeter (METTLER TOLEDO), with a test temperature of 0-100℃, a heating rate of 10℃ / min, and nitrogen protection. The thermal cycling stability of the material was tested: after weighing, the composite phase change material was placed on a heating platform and heated from room temperature to 80℃, then naturally cooled to room temperature, and this was repeated 20 times, followed by weighing. The test results are shown in Table 1.
[0062] Table 1 Performance test results of composite phase change materials
[0063] As shown in Table 1, the thermal conductivity of Comparative Example 1 (pure carbon foam + paraffin) without the addition of thermally conductive filler is only 0.120 W / (m·K); while in Example 5, by introducing one-dimensional CNTs and two-dimensional MoS2 in a 1:5 ratio, the CNTs successfully interpenetrated the interlayer gaps, increasing the longitudinal thermal conductivity pathway, and the thermal conductivity of the composite material jumped to 0.275 W / (m·K), an increase of 129%.
[0064] Examples 1-7 show that the optimal geometrical overlap effect is achieved when the ratio of one-dimensional tubular packing to two-dimensional sheet packing is 1:5. A comparison between Comparative Example 2 and Example 1 reveals that inorganic packings without silane coupling agent modification exhibit extremely poor compatibility in organic phase change matrices, easily leading to micro-agglomeration and increased interfacial thermal resistance. Their thermal conductivity only increases to 0.162 W / (m·K), indicating that surface modification is crucial for constructing an efficient "line-to-surface" thermal conductivity network.
[0065] Meanwhile, all samples that underwent “foamed carbon confinement + flattening + WPU coating” showed a mass loss rate of approximately 0.2% after 20 thermal cycles at 80℃, demonstrating excellent shape stability and low leakage characteristics, and are capable of meeting the application requirements in fields such as power battery thermal management and high-power device heat dissipation.
[0066] The various embodiments in this specification are described in a progressive manner, with each embodiment focusing on the differences from other embodiments. The same or similar parts between the various embodiments can be referred to each other.
[0067] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A preparation method of carbon nanotube / molybdenum disulfide@foam carbon-paraffin composite phase change material, characterized in that, Includes the following steps: 1) Carbon nanotubes, molybdenum disulfide, silane coupling agent and mixed solvent are mixed and modified to obtain surface-modified thermally conductive filler. 2) The surface-modified thermally conductive filler is melt-mixed with paraffin wax to obtain a modified paraffin wax phase change material; 3) The foamed carbon was immersed in the molten modified paraffin phase change material and vacuum melt impregnation was performed to obtain the carbon nanotube / molybdenum disulfide@foamed carbon-paraffin composite phase change material precursor; 4) The carbon nanotube / molybdenum disulfide@carbon foam-paraffin composite phase change material precursor is sequentially pressed and coated to obtain the carbon nanotube / molybdenum disulfide@carbon foam-paraffin composite phase change material. 2.The method of claim 1, wherein the carbon nanotube / molybdenum disulfide@foam carbon-paraffin composite phase change material is prepared by the following steps. The mass-to-volume ratio of carbon nanotubes, molybdenum disulfide, silane coupling agent, and mixed solvent in step 1) is 1~5g: 1~10g: 0.5~1g: 100mL; The modification reaction is carried out at a temperature of 60-70°C for 3-5 hours.
3. The preparation method of a carbon nanotube / molybdenum disulfide@carbon foam-paraffin composite phase change material according to claim 2, characterized in that, The carbon nanotubes have a diameter of 30-50 nm and a length of 10-20 μm; The particle size of the molybdenum disulfide is 6~8μm; The silane coupling agent includes one or more of γ-(methacryloyloxy)propyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, and γ-aminopropyltriethoxysilane. The mixed solvent includes an alcohol-water mixed solvent, wherein the volume ratio of alcohol to water in the alcohol-water mixed solvent is 90~98:2~10.
4. A method for preparing a carbon nanotube / molybdenum disulfide@carbon foam-paraffin composite phase change material according to any one of claims 1 to 3, characterized in that, The mass ratio of the surface-modified thermally conductive filler to paraffin wax in step 2) is 1:8~10; The melting and mixing temperature is 90~100℃.
5. The method for preparing a carbon nanotube / molybdenum disulfide@carbon foam-paraffin composite phase change material according to claim 4, characterized in that, The vacuum degree of the vacuum melt impregnation described in step 3) is -0.2 to -0.01 MPa, and the time is 1.8 to 2.5 h.
6. The method for preparing a carbon nanotube / molybdenum disulfide@carbon foam-paraffin composite phase change material according to claim 5, characterized in that, The pressing pressure described in step 4) is 7~12MPa.
7. The preparation method of the carbon nanotube / molybdenum disulfide@foam carbon-paraffin composite phase change material according to claim 5 or 6, characterized in that, The coating and encapsulation described in step 4) involves coating the surface of the pressed carbon nanotube / molybdenum disulfide@carbon foam-paraffin composite phase change material with a water-based polyurethane protective layer.
8. The carbon nanotube / molybdenum disulfide@carbon foam-paraffin composite phase change material prepared by the preparation method according to any one of claims 1 to 7.
9. The application of the carbon nanotube / molybdenum disulfide@carbon foam-paraffin composite phase change material as described in claim 8 in the thermal management system of power batteries, heat dissipation of high-power chips, or thermal energy regulation of microelectronic packaging devices.