A conformal phase change material and its preparation method

By adjusting the ratio of wax-based phase change material to binder, a conformal phase change material with good interfacial compatibility was prepared, solving the problem of easy powdering and difficult molding of paraffin phase change materials, and realizing the applicability of various application scenarios and improving the efficiency of industrial production.

CN123107630APending Publication Date: 2026-11-17YI JIANG FUTURE MATERIALS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611421651.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing paraffin phase change materials are prone to powdering and difficult to shape during the phase change process, resulting in high preparation costs, complex steps, and unstable product performance, and they cannot meet the needs of various conformal application scenarios.

Method used

By optimizing the composition ratio of wax-based phase change materials and binders, and using additives with specific structures such as 4-R1-2,2-dimethyl-1,3-dioxolane, combined with binders such as silicone rubber, resin glue, and acrylic glue, conformal phase change materials with good interfacial compatibility and chemical matching are prepared using a simple process of high-temperature mixing and pressing.

Benefits of technology

It enables flexible adjustment of various properties of the material, such as flexibility, resistance to high and low temperatures, and rapid curing ability, making it suitable for different application scenarios, reducing preparation costs, and improving industrial production efficiency and product versatility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107630A_ABST
    Figure CN123107630A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of phase change energy storage materials technology, specifically relating to a conformal phase change material and its preparation method. The conformal phase change material comprises the following components by weight fraction: 60-80% wax-based phase change material and 20-40% binder. The wax-based phase change material comprises the following components: a wax-based phase change substrate and additives, wherein the additives are added at 0.01%-0.05% of the mass of the wax-based phase change substrate. The binder includes any one of resin adhesive, silicone rubber, and acrylic adhesive. This invention, by optimizing the composition and preparation steps of the phase change material, can solve the technical problems of complex preparation methods and limited functionality in conformal application scenarios of existing paraffin phase change materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of phase change energy storage materials technology, specifically relating to a conformal phase change material and its preparation method. Background Technology

[0002] As electronic devices become increasingly miniaturized and powerful, the requirements for thermal management materials in fields such as power batteries, wearable devices, and irregularly shaped heat dissipation structures are becoming increasingly stringent. These materials not only need excellent low- and medium-temperature energy storage and temperature regulation capabilities, but also need to conform to irregular curved surfaces and confined spaces to achieve precise and efficient localized thermal management—that is, good conformability. Simultaneously, thermal management materials must also possess structural stability to prevent leakage during phase transitions and ensure long-term reliability.

[0003] Paraffin-based phase change materials (PCMs) have become the preferred materials for medium- and low-temperature thermal energy storage and temperature control due to their advantages such as high latent heat of phase change (150–250 J / g), good chemical stability, non-toxicity, odorlessness, low cost, and adjustable phase change temperature (15–100℃). They are widely used in electronic heat dissipation, power battery insulation, and building energy conservation. However, pure paraffin wax changes from solid to liquid above its phase change temperature, exhibiting fatal flaws such as easy flow, easy powdering, lack of structural strength, and inability to be directly molded. These flaws greatly limit their application in conformal thermal management scenarios.

[0004] To address the issues of pure paraffin wax being prone to powdering and difficult to mold, existing technologies generally employ the approach of preparing shaped phase change composite materials. This involves adding a carrier or binder to fix the paraffin wax into a fixed shape. Among these methods, the scheme of using wax-based phase change material powder as the energy storage body, combined with a polymer binder, and preparing phase change modules through pressing and heating processes has become one of the mainstream technical routes due to its simple equipment, high degree of molding freedom, and suitability for small-batch and irregularly shaped parts preparation.

[0005] For example, Chinese Patent CN112877036A discloses a phase change material and its preparation method and application. The phase change material includes expanded graphite composite phase change paraffin particles, thermally conductive powder, and hot melt adhesive powder. After heating, it softens and can be arbitrarily shaped under external force, exhibiting excellent thermal conductivity, fluidity, and stability. Another example is Chinese Patent CN115584242A, which discloses a method for preparing a phase change material with energy storage and a composite network structure. This method involves adding a pore-forming agent, a matrix binder, and functional fillers to the phase change material, and then pressing it using a physical mixing technique. This results in a phase change material with a random and uniform pore structure, good thermal conductivity and energy density, good energy storage effect, and structural stability.

[0006] However, existing technologies all use fillers or multi-component polymers to solve the problems of easy powdering and difficult molding of paraffin phase change materials. This leads to 1) high preparation costs, complex preparation steps and unstable product performance, making it difficult to become a reliable industrial production step; 2) the prepared phase change materials have fixed application scenarios and do not have the function of adapting to different application scenarios. Summary of the Invention

[0007] To address the technical problems of complex preparation methods and limited functionality in conformal applications of existing paraffin phase change materials, this invention provides a conformal phase change material and its preparation method. By optimizing the composition and preparation steps of the phase change material, the problems in the background technology can be effectively solved.

[0008] To achieve the above objectives, the present invention provides the following technical solution:

[0009] A conformal phase change material comprises the following components by weight: 60-80% wax-based phase change material and 20-40% binder; the wax-based phase change substrate comprises the following components: wax-based phase change substrate and additives, wherein the amount of additives added is 0.01%-0.05% of the mass of the wax-based phase change substrate; the binder comprises any one of resin adhesive, silicone rubber, and acrylic adhesive.

[0010] Inventive Concept: In practical work, the inventors of this application discovered that existing paraffin-based phase change energy storage materials often employ nanomaterial doping modification techniques to address the technical problems of weak shape retention and easy powdering during use. While this method can produce phase change materials with good performance indicators, its complexity and high cost due to nanomaterial doping modification make it difficult to adopt as a solution for large-scale industrial production. Furthermore, this approach is primarily designed for fixed, single application scenarios of paraffin-based phase change materials, lacking versatility when facing the preparation requirements of various composite scenarios, thus failing to meet actual industrial production needs. Therefore, the inventors have taken a different approach, starting from the physicochemical properties of the paraffin-based phase change substrate and binder. By innovating the component ratio of the paraffin-based phase change substrate and using additives to ensure that it has matching physicochemical properties with various binders, the invention allows for mixing with different binders during production, enabling application in different scenarios. Simultaneously, a unified preparation method allows for the preparation of different conformal phase change material modules using appropriate preparation parameters based on different binders.

[0011] Furthermore, the additive is 4-R1-2,2-dimethyl-1,3-dioxolane, where R1 represents a long-chain alkyl group with 11 to 23 carbon atoms.

[0012] Furthermore, the conformal phase change material comprises the following weight fraction composition schemes: 70-80% wax phase change material and 20-30% silicone rubber, or 60-70% wax phase change material and 30-40% resin adhesive, or 65-75% wax phase change material and 25-35% acrylic adhesive.

[0013] Furthermore, the silicone rubber includes any one of acetoxysilane rubber, methoxysilane rubber, and polyvinylsiloxane rubber; the linear expansion coefficient of the silicone rubber is 0.5% / °C. The phase change material prepared by mixing silicone rubber with a waxy phase change material in this invention possesses excellent flexibility and resistance to high and low temperatures, making it suitable for applications requiring the bonding of curved surfaces or flexible devices. It is also resistant to deformation above its phase change point and can recover its original shape after cooling.

[0014] Furthermore, the resin adhesive includes any one of water-based epoxy resin adhesive and polyurethane resin adhesive. The phase change material prepared by mixing the resin adhesive with the waxy phase change material in this invention possesses high strength and good dimensional stability, making it suitable for applications requiring structural support or for use in conductive material insulation applications.

[0015] Furthermore, the acrylic adhesive includes any one of polyacrylate or methacrylate adhesives. The phase change material prepared by mixing the acrylic adhesive with a waxy phase change material in this invention has the characteristics of fast curing speed and low cost, making it suitable for applications requiring rapid prototyping and the fabrication of thin modules.

[0016] This invention also provides a method for preparing a conformal phase change material, comprising the following steps: Step S1, mixing and reacting a wax-based phase change substrate and an additive at high temperature in an inert gas atmosphere, followed by cooling, curing, and pulverizing to obtain a wax-based phase change material powder; Step S2, mixing the wax-based phase change material powder and a binder in a certain proportion, placing the mixture into a mold, and pressing it into shape; Step S3, after molding, fixing and sealing the mold, placing it in an oven, and heating it at a temperature higher than the phase change temperature of the wax-based phase change material powder to set the shape, and after setting, cooling it to room temperature and demolding it to obtain the conformal phase change material.

[0017] Furthermore, in step S1, the high-temperature temperature is 100–150°C, and the reaction time is 30–60 min. The purpose of step S1 in this invention is to allow the wax-based phase change substrate and the additive to react fully at a high temperature, thereby altering the physicochemical properties of the wax-based phase change substrate. The high-temperature reaction temperature needs to be higher than the phase change temperature of the wax-based phase change substrate.

[0018] Furthermore, in step S2, the pressing pressure is 20-25t, and the pressing time is 10-30min.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] This invention innovates the composition ratio of wax-based phase change substrates by using 4-R1-2,2-dimethyl-1,3-dioxolane additives with a specific structure, enabling the wax-based phase change substrates to exhibit excellent interfacial compatibility and physicochemical matching with various types of adhesives (silicone rubber, resin adhesives, and acrylic adhesives). In actual production, only the ratio of wax-based phase change material to adhesive needs needs to be adjusted to adapt to different application scenarios: composite with silicone rubber provides excellent flexibility and high / low temperature resistance, suitable for bonding curved or flexible devices; composite with resin adhesives provides high strength and dimensional stability, suitable for scenarios requiring structural support or conductive insulation; and composite with acrylic adhesives provides rapid curing capability, suitable for the rapid fabrication of thin modules. A single formulation system can cover multiple conformal thermal management needs, significantly improving product versatility and industrial production efficiency.

[0021] 2. The density of the conformal phase change material prepared by this invention can be flexibly adjusted within the range of 0.88–0.95 g / cm³. Precise control of the material density can be achieved by adjusting the ratio of the wax-based phase change material to the binder, thus adapting to the differentiated requirements of material weight and heat storage density in different application scenarios. Compared to existing technologies that require the introduction of complex components such as nanomaterials, pore-forming agents, and multi-component polymers, this invention requires only three core components: a wax-based phase change substrate, trace additives, and a single binder. The preparation process involves only three steps: high-temperature mixing reaction, pressing, and heat setting. It is simple to operate, requires low equipment standards, and has controllable costs. Furthermore, the same preparation process only requires adjusting process parameters according to the type of binder to produce products with different properties, demonstrating good process versatility and prospects for large-scale production. Attached Figure Description

[0022] Figure 1 Here is a physical image of the conformal phase change material prepared in Example 1 of this invention;

[0023] Figure 2 Here is a physical image of the conformal phase change material prepared in Example 2 of this invention;

[0024] Figure 3 This is a DSC curve of the conformal phase change material prepared in Example 1 of the present invention;

[0025] Figure 4 This is a TGA curve of the conformal phase change material prepared in Example 1 of the present invention;

[0026] Figure 5 This is the DSC curve of the conformal phase change material prepared in Example 2 of the present invention. Detailed Implementation

[0027] To further illustrate the technical means and effects adopted by the present invention to achieve the intended purpose, the specific embodiments according to the present invention will be described in detail below with reference to the accompanying drawings and preferred embodiments.

[0028] The raw materials used in this invention are as follows:

[0029] Wax-based phase change substrate: Commercially available wax-based phase change substrate, composite paraffin or microencapsulated paraffin, purchased from Wuhan Zhongke Advanced Materials Technology Co., Ltd., with a phase change temperature of 70-80℃.

[0030] Additive: Synthesized by reacting 2,2-dimethyl-1,3-dioxolane-4-methanol with saturated fatty acids;

[0031] Silicone rubber: any one of acetoxysilane rubber, methoxysilane rubber and polyvinylsiloxane rubber, commercially available products, such as the acetoxysilane rubber of product model Loctite SI596;

[0032] Resin adhesives: including water-based epoxy resins, commercially available products, such as two-component resin adhesives with product models ZW-6105 and ZW-2870;

[0033] Acrylic adhesives: including any of the following: polyacrylate adhesives and methacrylate adhesives, commercially available products, such as acrylic structural adhesive model HZ-9017.

[0034] Example 1

[0035] This embodiment provides a conformal phase change material, comprising the following weight fraction components: 70% wax-based phase change material and 30% binder, wherein the binder is an organosilicon rubber, specifically acetoxysilane rubber, with a linear expansion coefficient of 0.5% / °C.

[0036] The wax-based phase change material includes a wax-based phase change substrate and an additive. The amount of additive added is 0.05% of the mass of the wax-based phase change substrate, and the additive is 4-octadecyl-2,2-dimethyl-1,3-dioxolane.

[0037] This embodiment also provides a method for preparing a conformal phase change material, including the following steps:

[0038] Step S1: After mixing and reacting the wax-based phase change substrate and additives at high temperature in an inert gas atmosphere, the mixture is cooled, cured, and pulverized to obtain wax-based phase change material powder.

[0039] Specifically, 100g of wax-based phase change material is weighed, and 0.05g of additive is added. The mixture is stirred at 100°C for 1 hour under a nitrogen atmosphere. After the reaction is complete, the mixture is allowed to cool naturally to room temperature to solidify. The solidified material is then pulverized and sieved to obtain wax-based phase change material powder.

[0040] Step S2: Mix the wax-based phase change material powder and binder evenly according to the ratio, place them into a mold, and press them into shape;

[0041] Specifically, the wax-based phase change material powder obtained above is mixed with acetoxysilane rubber at a ratio of 70% wax-based phase change material and 30% binder. After mixing, the mixture is thoroughly stirred to ensure uniform dispersion. The mixture is then sieved to ensure there are no large, lumpy particles. The sieved mixture is filled into a mold, maintaining uniform filling throughout the process. The mold is then placed under a press and pressed at a pressure of 25t for 10 minutes to form the final product.

[0042] Step S3: After molding, fix and seal the mold and place it in an oven. Heat and shape it at a temperature higher than that of the wax-based phase change material powder. After shaping, cool it to room temperature and demold to obtain the conformal phase change material.

[0043] Specifically, the pressed mold is removed and tightened to prevent deformation of the molding material due to subsequent heating and expansion. The mold is then placed in an oven and heated at 80°C for 30 minutes to set the shape. After heating and curing, the mold is allowed to cool naturally at room temperature. Once cooled, it can be demolded to obtain the conformal phase change material.

[0044] Example 2

[0045] This embodiment provides a conformal phase change material, comprising the following components by weight: 80% wax-based phase change material and 20% binder, wherein the binder is a resin adhesive, specifically an aqueous epoxy resin.

[0046] The wax-based phase change material includes a wax-based phase change substrate and an additive. The amount of additive added is 0.01% of the mass of the wax-based phase change substrate, and the additive is 4-dodecyl-2,2-dimethyl-1,3-dioxolane.

[0047] This embodiment also provides a method for preparing a conformal phase change material, including the following steps:

[0048] Step S1: After mixing and reacting the wax-based phase change substrate and additives at high temperature in an inert gas atmosphere, the mixture is cooled, cured, and pulverized to obtain wax-based phase change material powder.

[0049] Specifically, 100g of wax-based phase change substrate is weighed, and 0.01g of additive is added. The mixture is stirred at 100°C for 1 hour under a nitrogen atmosphere. After the reaction is complete, the mixture is allowed to cool naturally to room temperature to solidify. The solidified material is then pulverized and sieved to obtain wax-based phase change material powder.

[0050] Step S2: Mix the wax-based phase change material powder and binder evenly according to the ratio, place them into a mold, and press them into shape;

[0051] Specifically, the wax-based phase change material powder obtained above is mixed with acetoxysilane rubber at a ratio of 80% wax-based phase change material and 20% binder. After mixing, the mixture is thoroughly stirred to ensure uniform dispersion. The mixture is then sieved to ensure there are no large, lumpy particles. The sieved mixture is filled into a mold, maintaining uniform filling throughout the process. The mold is then placed under a press and pressed at a pressure of 25t for 10 minutes to form the final product.

[0052] Step S3: After molding, fix and seal the mold and place it in an oven. Heat and shape it at a temperature higher than that of the wax-based phase change material powder. After shaping, cool it to room temperature and demold to obtain the conformal phase change material.

[0053] Specifically, remove the pressed mold and tighten it to prevent deformation of the molding material due to subsequent heating and expansion. Place the mold in an oven and heat at 80°C for 30 minutes to set the shape.

[0054] After the heating, curing and shaping are completed, the mold is placed in a room temperature environment to cool naturally. After cooling, the mold can be demolded to obtain the conformal phase change material.

[0055] Example 3

[0056] This embodiment provides a conformal phase change material, comprising the following components by weight: 75% wax-based phase change material and 25% binder, wherein the binder is an acrylic adhesive, specifically polyacrylate.

[0057] The wax-based phase change material includes a wax-based phase change substrate and an additive. The amount of additive added is 0.03% of the mass of the wax-based phase change substrate. The additive is 4-octadecyl-2,2-dimethyl-1,3-dioxolane.

[0058] This embodiment also provides a method for preparing a conformal phase change material, including the following steps:

[0059] Step S1: After mixing and reacting the wax-based phase change substrate and additives at high temperature in an inert gas atmosphere, the mixture is cooled, cured, and pulverized to obtain wax-based phase change material powder.

[0060] Specifically, 100g of wax-based phase change material is weighed, and 0.03g of additive is added. The mixture is stirred at 100°C for 1 hour under a nitrogen atmosphere. After the reaction is complete, the mixture is allowed to cool naturally to room temperature to solidify. The solidified material is then pulverized and sieved to obtain wax-based phase change material powder.

[0061] Step S2: Mix the wax-based phase change material powder and binder evenly according to the ratio, place them into a mold, and press them into shape;

[0062] Specifically, the wax-based phase change material powder obtained above is mixed with acetoxysilane rubber at a ratio of 80% wax-based phase change material and 20% binder. After mixing, the mixture is thoroughly stirred to ensure uniform dispersion. The mixture is then sieved to ensure there are no large, lumpy particles. The sieved mixture is filled into a mold, maintaining uniform filling throughout the process. The mold is then placed under a press and pressed at a pressure of 25t for 10 minutes to form the final product.

[0063] Step S3: After molding, fix and seal the mold and place it in an oven. Heat and shape it at a temperature higher than that of the wax-based phase change material powder. After shaping, cool it to room temperature and demold to obtain the conformal phase change material.

[0064] Specifically, the pressed mold is removed and tightened to prevent deformation of the molding material due to subsequent heating and expansion. The mold is then placed in an oven and heated at 80°C for 30 minutes to set the shape. After heating and curing, the mold is allowed to cool naturally at room temperature. Once cooled, it can be demolded to obtain the conformal phase change material.

[0065] Comparative Example 1

[0066] The difference between this comparative example and Example 1 is that no additives were used in the wax-based phase change material in the conformal phase change material, and step S1 was not used in the preparation method. The other steps and components are the same as in the example.

[0067] Comparative Example 2

[0068] The difference between this comparative example and Example 1 is that the conformal phase change material includes the following components by weight fraction: 50% wax-based phase change material and 50% binder, while the other steps and components are the same as in the example.

[0069] Comparative Example 3

[0070] The difference between this comparative example and Example 1 is that the conformal phase change material includes the following components by weight fraction: 90% wax-based phase change material and 10% binder, while the other steps and components are the same as in the example.

[0071] Comparative Example 4

[0072] The difference between this comparative example and Example 1 is that the amount of additive added is 0.1% of the mass of the wax-based phase change substrate, while the other steps and components are the same as in the example.

[0073] Example and comparative performance tests:

[0074] Thermogravimetric analysis: The experimental method was carried out in accordance with ISO 11358-1:2022.

[0075] Enthalpy of fusion: The experimental method was carried out in accordance with GB / T 19466.3-2004 standard.

[0076] Density: The experimental method was carried out in accordance with GB / T 1463 standard.

[0077] The test results are shown in Table 1 and Appendix 2 below. Figure 3-5 As shown:

[0078] Table 1 Performance Test Table for Examples & Comparative Examples

[0079]

[0080] From the above experimental results, we can conclude that:

[0081] The conformal phase change material prepared by this invention has a melting enthalpy of up to 169 J / g, and the enthalpy retention rate of the original wax-based phase change substrate can reach up to 94.7%, indicating that the preparation process of this invention has minimal impact on the heat storage performance of the phase change material and effectively preserves the material's latent heat storage capacity. In contrast, in Comparative Example 2, due to the excessive amount of binder (50%), the melting enthalpy dropped sharply to 98 J / g, and the enthalpy retention rate was only 54.4%; in Comparative Example 3, due to the excessive amount of binder (10%), although the enthalpy was high, the thermal weight loss was severe (12.6%), which could not meet the requirements for practical use. The above results indicate that the ratio range of 60-80% wax-based phase change material to 20-40% binder described in this invention is the optimal range for balancing heat storage density and structural stability.

[0082] Existing technologies for preparing phase change material (PCM) plates are prone to cracking and bulging upon heating, primarily due to a mismatch in the thermal expansion coefficients of the PCM and the binder, leading to expansion misalignment during heating. This invention addresses this by selecting a binder with a thermal expansion coefficient matching that of the wax-based PCM, forming a stable three-dimensional network skeleton during molding. This binder expands synchronously with the PCM during heating, effectively preventing cracking and bulging caused by expansion misalignment. Thermogravimetric analysis shows that the product of this invention experiences only 4.5%–5.7% mass loss at 260℃, demonstrating excellent thermal stability and meeting long-term usage requirements under normal operating conditions. In Comparative Example 1, the product without additives experienced a thermal weight loss of 8.3%, indicating that additives significantly improve the material's thermal stability. In Comparative Example 4, excessive additives also led to a thermal weight loss of 6.2%, suggesting that the additive dosage should be controlled within the preferred range of 0.01%–0.05%.

[0083] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.

Claims

1. A conformal phase change material, characterized in that: It comprises the following components by weight: 60-80% wax-based phase change material and 20-40% binder; the wax-based phase change material comprises the following components: wax-based phase change substrate and additives, wherein the amount of additives added is 0.01%-0.05% of the mass of the wax-based phase change substrate; the binder comprises any one of resin glue, silicone rubber, and acrylic glue.

2. The conformal phase change material according to claim 1, characterized in that, The additive is 4-R1-2,2-dimethyl-1,3-dioxolane, where R1 represents a long-chain alkyl group with 11 to 23 carbon atoms.

3. The conformal phase change material according to claim 1, characterized in that, The conformal phase change material comprises the following weight fraction composition schemes: 70-80% wax phase change material and 20-30% silicone rubber, or 60-70% wax phase change material and 30-40% resin adhesive, or 65-75% wax phase change material and 25-35% acrylic adhesive.

4. The conformal phase change material according to claim 1, characterized in that, The silicone rubber includes any one of acetoxysilane rubber, methoxysilane rubber, and polyvinylsiloxane rubber; the linear expansion coefficient of the silicone rubber is 0.5% / °C.

5. The conformal phase change material according to claim 1, characterized in that, The resin adhesive includes any one of water-based epoxy resin adhesive and polyurethane resin adhesive.

6. The conformal phase change material according to claim 1, characterized in that, The acrylic adhesive includes any one of polyacrylate or methacrylate adhesives.

7. A method for preparing a conformal phase change material, characterized in that, Includes the following steps: Step S1: Mix the wax-based phase change substrate and additives at high temperature in an inert gas atmosphere, then cool, solidify, and pulverize to obtain wax-based phase change material powder; Step S2: Mix the wax-based phase change material powder and binder evenly in proportion, place them in a mold, and press to form; Step S3: After forming, fix and seal the mold and place it in an oven to heat and shape at a temperature higher than the phase change temperature of the wax-based phase change material powder. After shaping, cool to room temperature and demold to obtain conformal phase change material.

8. The method for preparing conformal phase change materials according to claim 7, characterized in that, In step S1, the high temperature is 100-150℃ and the reaction time is 30-60 min.

9. The method for preparing conformal phase change materials according to claim 7, characterized in that, In step S2, the pressing pressure is 20-25t, and the pressing time is 10-30min.

Citation Information

Patent Citations

  • Phase change material as well as preparation method and application thereof

    CN112877036A

  • Preparation method of phase change material with energy storage and composite network structure

    CN115584242A