A co-doped mechanoluminescent material, its preparation method, and fluorescent composite materials

By co-doping CaGa4O7 mechanoluminescent materials with Tb and Dy ions and Cr ions, and combining them with high-temperature solid-state sintering and PDMS composite, multiple luminescence modes are formed, solving the problem of single luminescence characteristics of existing mechanoluminescent materials and achieving a multi-mode dynamic response encryption effect.

CN123107680APending Publication Date: 2026-11-17CIVIL AVIATION UNIV OF CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611348823.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-02
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing mechanoluminescent materials are mainly single piezoelectric luminescence and triboelectric luminescence, with emission colors concentrated in the visible or near-infrared bands. They lack multi-mode dynamic response, resulting in poor encryption effect.

Method used

The co-doped mechanoluminescent material Ca1-xy-zTbxDyyCrzGa4O7 was used. By doping Tb and Dy ions with Cr ions, combined with high-temperature solid-state sintering and PDMS composite, multiple luminescence modes were formed, including piezoelectric mechanoluminescence and triboelectric mechanoluminescence.

Benefits of technology

It achieves multiple luminescence characteristics of near-infrared dynamic excitation, including dynamic light changes from blue to yellow to red to near-infrared and temperature-varying photoluminescence from blue to green to white, enhancing the speed and security of information transmission.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107680A_ABST
    Figure CN123107680A_ABST
Patent Text Reader

Abstract

This invention provides a co-doped mechanoluminescent material, its preparation method, and a fluorescent composite material thereof. The chemical formula of the co-doped mechanoluminescent material is Ca. 1‑x‑y‑z Tb x Dy y Cr z The Ga4O7 matrix contains 0 < x ≤ 0.02, 0 < y ≤ 0.05, and 0 < z ≤ 0.01. The co-doped mechanoluminescent material of this invention, by introducing Tb, Dy, and Cr elements into a CaGa4O7 mechanoluminescent material matrix, forms a co-doped mechanoluminescent material with excellent luminescence performance. Compared with most existing mechanoluminescent materials, this co-doped mechanoluminescent material achieves near-infrared dynamic excitation, dynamic light emission from blue to yellow to red to near-infrared, and temperature-varying photoluminescence from blue to green to white.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of luminescent materials, and in particular relates to a co-doped mechanoluminescent material, its preparation method, and a fluorescent composite material. Background Technology

[0002] Optical materials, due to their excitation methods and emission colors, have become key factors in information encryption and anti-counterfeiting, attracting widespread attention in their application. However, their single emission characteristics limit their ability to perform only simple encryption, resulting in less than ideal encryption effects. Based on the unique response mechanism of multi-mode luminescent materials, dynamic response encryption of information transmission can be achieved under external environmental stimuli, thereby enhancing the speed and security of information transmission.

[0003] Currently, most mechanoluminescent materials are mainly single piezoelectric and triboelectric luminescence, and the emission color is mainly concentrated in the visible light band or entirely manifested in the near-infrared band. There is relatively little research on materials with dynamic color changes from blue light to near-infrared (350nm-900nm) band and materials with piezoelectric-triboelectric dual-mode mechanoluminescence. Summary of the Invention

[0004] In view of this, the present invention aims to overcome the defects in the prior art and proposes a co-doped mechanoluminescent material, its preparation method and fluorescent composite material.

[0005] To achieve the above objectives, the technical solution of the present invention is implemented as follows: This invention provides a co-doped mechanoluminescent material, wherein the chemical formula of the co-doped mechanoluminescent material is Ca. 1-x-y-z Tb x Dy y Cr z Ga4O7, where 0 < x ≤ 0.02, 0 < y ≤ 0.05, and 0 < z ≤ 0.01. Since single-doped Cr ions do not exhibit mechanoluminescence, while the luminescent energy levels of Tb, Dy, and Cr ions exhibit energy transfer, their energy levels correspond to: 5 D j (j= 3, 4)→ 7 F k (k=3, 4, 5, 6), 4 F 9 / 2 → 6 H l (l= 9 / 2, 11 / 2, 13 / 2, 15 / 2), 4 T2 / 2 E→ 4 A2 can effectively transfer energy from the matrix to the Cr ion energy level via Tb and Dy ions, thereby promoting Cr ion luminescence.

[0006] Furthermore, x is 0.01-0.02; y is 0.01-0.05; and z is 0.005-0.01.

[0007] Preferably, x is 0.01, 0.015, or 0.02; y is 0.01, 0.02, 0.03, 0.04, or 0.05; and z is 0.005, 0.075, or 0.01.

[0008] This invention also provides a method for preparing a co-doped mechanoluminescent material, comprising the following steps: (1) Grind CaCO3, Ga2O3, Tb2O3, Dy2O3 and Cr2O3 separately, and then mix the powders obtained from grinding to obtain a mixture; (2) The mixture is calcined to obtain the co-doped mechanoluminescent material.

[0009] Furthermore, the calcination step in step (2) includes pre-calcination, calcination and cooling.

[0010] Furthermore, the specific parameters for the pre-firing are: heating to 550-650℃ at a heating rate of 3-5℃ / min.

[0011] Furthermore, the specific parameters for calcination are: heating to 1300-1500℃ at a heating rate of 3-5℃ / min.

[0012] Furthermore, the specific cooling parameters are as follows: cooling to 500-550℃ at a cooling rate of 3-4℃ / min, and then naturally cooling to room temperature.

[0013] The present invention also provides a fluorescent composite material, wherein the material comprises the co-doped metronome material and the organosilicon polymer in a mass ratio of 1:3-15.

[0014] Furthermore, the organosilicon polymer is PDMS.

[0015] The dynamic luminescence encryption principle of the co-doped mechanoluminescent material is as follows: Since the luminescent material has multiple response luminescence modes (254nm-cyan, 305nm-orange-red, 351nm-yellow-green, 575nm intrinsic yellow-green light-strong near-infrared luminescence, ML-near-infrared, irradiation temperature-dependent color change), primary encryption is performed by collecting the luminescence color and near-infrared signal, and secondary encryption is performed by ML and temperature control.

[0016] Compared with the prior art, the present invention has the following advantages: The co-doped mechanoluminescent material of this invention introduces Tb, Dy, and Cr elements into a CaGa4O7 mechanoluminescent material matrix, forming a co-doped mechanoluminescent material with excellent luminescence performance. Under PET testing, it exhibits piezoelectric mechanoluminescence characteristics with near-infrared emission, and under mixed testing with PDMS, it exhibits mechanoluminescence with both visible and near-infrared emission. Compared with most existing mechanoluminescent materials, the mechanoluminescence of this co-doped mechanoluminescent material achieves near-infrared dynamic excitation, dynamic light emission from blue to yellow to red to near-infrared, and temperature-varying photoluminescence from blue to green to white.

[0017] The co-doped mechanoluminescent material described in this invention has a variety of luminescence response characteristics: (1) It has different luminescence characteristics under 254nm, 305nm and 351nm ultraviolet lamps, and has near-infrared luminescence characteristics in a wide wavelength range of 254-600nm, wherein the near-infrared excitation peaks are located at 320nm, 454nm and 595nm, and also has a special long afterglow phenomenon under 254nm and 305nm ultraviolet lamp irradiation; (2) Under 254nm ultraviolet lamp irradiation, the luminescent material has irradiation temperature change color from blue to green at 30℃-180℃, and has stable green luminescence at 180℃-210℃; (3) The luminescent material only displays near-infrared luminescence signal characteristics under stress.

[0018] This invention prepares fluorescent composite materials with piezoelectric and triboelectric properties by high-temperature solid-state sintering, and then dops them with Tb, Dy, and Cr ions, followed by molding and PDMS composite preparation to obtain luminescence properties under different materials.

[0019] The preparation method of the fluorescent composite material described in this invention is mild, simple and easy to operate, low in cost, and has high material durability, and can be widely used in multi-level optical encryption in different scenarios. Attached Figure Description

[0020] Figure 1 The X-ray diffraction pattern of the mechanoluminescent material described in the embodiments of the present invention; Figure 2 The changes in PET mechanoluminescence with and without Cr ion doping are described in Example 1 and Comparative Example 1 of this invention; Figure 3 The near-infrared mechanoluminescence changes of Cr ions in PET under different rare earth doping compositions are described in Example 1 and Comparative Examples 2-4 of this invention. Figure 4 This refers to the near-infrared mechanoluminescence of PET with different concentrations of the same doped ions as described in Examples 1 and 2 of this invention; Figure 5 As described in Embodiment 2 of the present invention, at 5π rad •s -1Mechanoluminescence cycle for 1 minute under the specified conditions; Figure 6 This is a piezoelectric microscope test image as described in Embodiment 2 of the present invention; Figure 7 This refers to the mechanoluminescence change of the PET film and PDMS composite material under a 10N test as described in Example 2 of the present invention; Figure 8 This refers to the PDMS triboelectric voltage test described in Embodiment 2 of the present invention; Figure 9 The images are CIE diagrams of the composite material described in Example 2 of this invention under ultraviolet light irradiation at 254 nm, 305 nm and 351 nm, respectively. Figure 10 This refers to the change in mechanoluminescence intensity under 254 nm ultraviolet lamp irradiation as described in Embodiment 2 of the present invention; Figure 11 This refers to the change in mechanoluminescence intensity under 305 nm ultraviolet lamp irradiation as described in Embodiment 2 of the present invention; Figure 12 This is a schematic diagram of the mechanoluminescence intensity under 254 nm ultraviolet lamp irradiation as described in Embodiment 2 of the present invention, showing the change in luminescence intensity after 1500 rubbing cycles; Figure 13 This refers to the color change of the material at different temperatures under 254 nm ultraviolet light irradiation, as described in Embodiment 2 of the present invention. Figure 14 This is the near-infrared emission pattern of the material at 30°C and 180°C under 254 nm ultraviolet light irradiation as described in Embodiment 2 of the present invention; Figure 15 The secondary encryption application described in Embodiment 2 of the present invention includes: (a) the emission color of the material under different excitation wavelengths and the emission intensity in the near-infrared band; and (b) the optical Morse code table. Detailed Implementation

[0021] Unless otherwise defined, the technical terms used in the following embodiments have the same meanings as commonly understood by those skilled in the art. Unless otherwise specified, the experimental reagents used in the following embodiments are conventional biochemical reagents; and the experimental methods described are conventional methods.

[0022] The present invention will be described in detail below with reference to embodiments.

[0023] Example 1 S1. Place CaCO3, Ga2O3, Tb2O3, Dy2O3 and Cr2O3 in a mortar and hand-grind for 20 minutes to obtain a mixture; S2. Place the mixture obtained in S1 in an alumina crucible and calcine it in a muffle furnace at a heating rate of 4℃ / min to 600℃ for 24h. Then, cool it down to 550℃ at a cooling rate of 3℃ / min and allow it to cool naturally to room temperature. Grind the mixture and then heat it up to 1400℃ at a heating rate of 4℃ / min for 12h. Finally, cool it down to 550℃ at a cooling rate of 3℃ / min and allow it to cool naturally to room temperature. S3. Transfer the precursor obtained in S2 to a mortar and grind it thoroughly into a fine powder until there is no obvious graininess, thus obtaining Ca. 0.97 Tb 0.01 Dy 0.01 Cr 0.01 Ga4O7 powder.

[0024] A method for preparing a thin film sample includes the following steps: The synthesized luminescent material was ultrasonically dispersed with a UV curing agent (LEAFTOP 9307) at a weight ratio of 5:1 in 4 mL of anhydrous ethanol. The mixture was rapidly transferred to a 2 cm × 2 cm square mold, which was placed on a polyethylene terephthalate (PET) film covered with ethylene-vinyl acetate (EVA). After the ethanol evaporated, the mold was removed, covered with two layers of EVA-PET film, sealed using a heat-sealing machine, and cured under a UV lamp to finally form an encapsulated stress-induced luminescent film.

[0025] Example 2 A method for preparing a co-doped mechanoluminescent material includes the following steps: S1. Place CaCO3, Ga2O3, Tb2O3, Dy2O3 and Cr2O3 in a mortar and hand-grind for 20 minutes to obtain a mixture; S2. Place the mixture obtained in S1 in an alumina crucible and calcine it in a muffle furnace at a heating rate of 4℃ / min to 600℃ for 24h. Then, cool it down to 550℃ at a cooling rate of 3℃ / min and allow it to cool naturally to room temperature. Grind the mixture and then heat it up to 1400℃ at a heating rate of 4℃ / min for 12h. Finally, cool it down to 550℃ at a cooling rate of 3℃ / min and allow it to cool naturally to room temperature. S3. Transfer the precursor obtained in S2 to a mortar and grind it thoroughly into a fine powder until there is no obvious graininess, thus obtaining Ca. 0.94 Tb 0.015 Dy 0.04 Cr 0.005 Ga4O7 powder.

[0026] A method for preparing a thin film sample is the same as in Example 1.

[0027] A method for preparing a fluorescent composite material includes the following steps: Polydimethylsiloxane PDMS (SYLGARD 184) and PDMS curing agent were mixed at a weight ratio of 10:1. Then, 10% of the weight of the luminescent material powder was added to the mixture. The mixture was stirred in a 20 mm cylindrical mold and then placed in a vacuum oven at an ambient temperature of 80°C for 2 hours. The fluorescent composite material was then demolded.

[0028] Comparative Example 1 A co-doped mechanoluminescent material, namely Ca 0.98 Tb 0.01 Dy 0.01 Ga4O7 powder.

[0029] A method for preparing a thin film sample is the same as in Example 1.

[0030] Comparative Example 2 A co-doped mechanoluminescent material, namely Ca 0.98 Tb 0.01 Cr 0.01 Ga4O7 powder.

[0031] A method for preparing a thin film sample is the same as in Example 1.

[0032] Comparative Example 3 A co-doped mechanoluminescent material, namely Ca 0.98 Dy 0.01 Cr 0.01 Ga4O7 powder.

[0033] A method for preparing a thin film sample is the same as in Example 1.

[0034] Comparative Example 4 A co-doped mechanoluminescent material, namely Ca 0.99 Cr 0.01 Ga4O7 powder.

[0035] A method for preparing a thin film sample is the same as in Example 1.

[0036] Performance testing: I. X-ray diffraction experiment: X-ray diffraction tests were performed on the mechanoluminescent materials prepared in each embodiment and comparative example to obtain the XRD patterns of the materials.

[0037] Figure 1 X-ray diffraction pattern of mechanoluminescent material.

[0038] XRD results showed that the synthesized Ca 1-x-y-z Tb x Dy yCr z For Ga4O7 (0 < x ≤ 0.02, 0 < y ≤ 0.05, 0 < z ≤ 0.01), the XRD patterns of the materials with different doping concentrations are not significantly different from the standard cards of the matrix, proving that the doped material is still a pure phase.

[0039] II. Mechanoluminescence performance test: Thin film sample preparation: The synthesized luminescent material and UV curing agent (LEAFTOP 9307) were ultrasonically dispersed in 4 mL of anhydrous ethanol at a weight ratio of 5:1. The mixture was rapidly transferred to a 2 cm × 2 cm square mold, which was placed on a polyethylene terephthalate (PET) film covered with ethylene-vinyl acetate (EVA). After the ethanol evaporated, the mold was removed, covered with two layers of EVA-PET film, sealed using a heat-sealing machine, and cured under a UV lamp to finally form an encapsulated stress-induced luminescence film.

[0040] The aforementioned plastic sealant was fixed onto the testing device, and a push-pull force gauge with an optical fiber testing end was fixed onto the plastic sealant at the test start position. The required force was applied, and a force-induced luminescence test was performed in a dark environment.

[0041] Depend on Figure 2 It can be concluded that the mechanoluminescence colors of PET doped with Tb and Dy are significantly different from those of PET doped with Tb, Dy and Cr. When Tb and Dy are co-doped, the characteristic mechanoluminescence of Tb and Dy is exhibited. When Tb, Dy and Cr are doped, only the near-infrared mechanoluminescence of Cr ions is displayed, realizing the conversion of yellow-green light in the visible light region into near-infrared light emission, proving that Tb and Dy ions can transfer energy to Cr ions.

[0042] Figure 3 It can be concluded that, under different rare earth ion doping conditions, the near-infrared emission of Cr ions gradually increases from non-existent to present, and the intensity gradually increases from Dy and Cr co-doping to Tb and Cr doping. The emission is strongest when the doping conditions are Tb, Dy, and Cr.

[0043] Figure 4 It can be concluded that the strongest ion doping concentration for mechanoluminescence obtained through concentration adjustment is 1.5%Tb+4%Dy+0.5%Cr.

[0044] Figure 5 For 5π rad •s -1 Under the experimental conditions, after a 1-minute mechanoluminescence cycle, the material still exhibited near-infrared mechanoluminescence of Cr ions after 300 rubs.

[0045] Figure 6 For Ca 0.94 Tb 0.015 Dy 0.04 Cr0.005 The PFM test results for Ga4O7 show a butterfly-shaped curve and hysteresis characteristic of piezoelectric materials, proving that the material exhibits piezoelectric properties after ion doping.

[0046] Figure 7 It can be concluded that Ca 0.94 Tb 0.015 Dy 0.04 Cr 0.005 Ga4O7 exhibits different luminescence properties in PET films and PDMS. In PDMS, the material not only exhibits near-infrared mechanoluminescence of Cr ions, but also visible light luminescence of Tb, Dy, and the matrix, proving that the material in PDMS has not only piezoelectric properties but also triboelectric electroluminescence properties.

[0047] Figure 8 Triboelectric measurements of PDMS showed that the triboelectricity of the composite material increased with increasing force, indicating that the composite material prepared with PDMS possesses triboelectric electroluminescence properties.

[0048] Figure 9 The images show the CIE images of the composite material under UV light irradiation at 254 nm, 305 nm, and 351 nm. The emission color of the material changes from blue to red and then to yellow. Under 254 nm irradiation, it exhibits four characteristic photoluminescence properties of matrix, Tb, Dy, and Cr ions. Under 305 nm irradiation, it only shows the characteristic photoluminescence of Cr ions. Under 351 nm irradiation, it exhibits the characteristic photoluminescence of Dy and Cr ions.

[0049] Figure 10-11 As can be seen, the intensity changes of mechanoluminescence under 254 nm and 305 nm ultraviolet light irradiation are observed. Under 254 nm irradiation, the visible light region of the material is enhanced by 3600% compared to conventional photoluminescence with the application of force, while under 305 nm irradiation, the enhancement of photoluminescence by force is 278% compared to conventional photoluminescence.

[0050] Figure 12 This is a schematic diagram of the mechanoluminescence intensity under 254 nm ultraviolet light irradiation. After 1500 rubbing cycles, the luminescence intensity decreased by 7.08%.

[0051] Figure 13 As can be seen under 254 nm UV irradiation, due to the different thermal quenching resistance of each energy level, the matrix blue light continuously weakens with increasing temperature, and the subsequent blue light portion is mainly composed of Tb ions. 5 D3→ 7 F6 provides, while Tb ions 5 D3→ 7 F5 / 7F4 has insufficient resistance to thermal quenching, quenching at 180℃, while Dy ions... 4 F 9 / 2 → 6 H 13 / 2 Along with the decrease in emission intensity, there is a slight redshift. The NIR-I luminescence of Cr ions also gradually weakens with increasing temperature. However, when the temperature rises from 30℃ to 180℃, the NIR-I luminescence of Tb ions... 5 D4→ 7 F5, on the contrary, will steadily increase. The material's resistance to thermal quenching enables the color to change from blue to green at different temperatures, and finally to white light quenching.

[0052] Figure 14 We can observe the near-infrared emission patterns of the material at 30℃ and 180℃ under 254 nm ultraviolet light irradiation. We can see that the near-infrared emission intensity decreases as the material temperature increases.

[0053] Figure 15 For Level 2 encryption applications, Figure 15 (a) Shows the emission color and near-infrared emission intensity of the material under different excitation wavelengths. Figure 15 (b) is the encoding table.

[0054] Encryption principle: Since this luminescent material has multiple response emission modes (254nm-cyan, 305nm-orange-red, 351nm-yellow-green, 575nm intrinsic yellow-green light-strong near-infrared emission, ML-near-infrared, irradiation-temperature-variable color change), primary encryption is performed by collecting emission color and near-infrared signal, and secondary encryption is performed by ML and temperature control.

[0055] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A co-doped mechanoluminescent material, characterized in that: The chemical formula of the co-doped mechanoluminescent material is Ca. 1-x-y-z Tb x Dy y Cr z Ga4O7, where 0 < x ≤ 0.02, 0 < y ≤ 0.05, and 0 < z ≤ 0.

01.

2. The co-doped mechanoluminescent material according to claim 1, characterized in that: The x value is 0.01-0.02; the y value is 0.01-0.05; and the z value is 0.005-0.

01.

3. The co-doped mechanoluminescent material according to claim 2, characterized in that: The x is 0.01, 0.015, or 0.02; the y is 0.01, 0.02, 0.03, 0.04, or 0.05; and the z is 0.005, 0.075, or 0.

01.

4. The method for preparing the co-doped mechanoluminescent material according to any one of claims 1-3, characterized in that: Includes the following steps: (1) Grind CaCO3, Ga2O3, Tb2O3, Dy2O3 and Cr2O3 separately, and then mix the powders obtained from grinding to obtain a mixture; (2) The mixture is calcined to obtain the co-doped mechanoluminescent material.

5. The method for preparing the co-doped mechanoluminescent material according to claim 4, characterized in that: The calcination step in step (2) includes pre-calcination, calcination and cooling.

6. The method for preparing the co-doped mechanoluminescent material according to claim 5, characterized in that: The specific parameters for the pre-firing are: heating to 550-650℃ at a heating rate of 3-5℃ / min.

7. The method for preparing the co-doped mechanoluminescent material according to claim 5, characterized in that: The specific parameters for calcination are: heating to 1300-1500℃ at a heating rate of 3-5℃ / min.

8. The method for preparing the co-doped mechanoluminescent material according to claim 5, characterized in that: The specific cooling parameters are as follows: the temperature is reduced to 500-550℃ at a cooling rate of 3-4℃ / min, and then naturally cooled to room temperature.

9. A fluorescent composite material, characterized in that: The materials described include the co-doped metronome material and organosilicon polymer of any one of claims 1-3 in a mass ratio of 1:3-15.

10. The fluorescent composite material according to claim 9, characterized in that: The organosilicon polymer is PDMS.