Preparation method and application of sodium humate-based porous fiber soil dispersion material
The method for preparing sodium humate-based porous fiber materials solves the problem of low soil leaching efficiency under low water-to-soil ratio, achieves efficient dispersion of soil aggregates under low water-to-soil ratio, improves heavy metal removal rate, and is suitable for soil heavy metal pollution remediation.
Patent Information
- Application Number
- CN202611404723.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-10
- Publication Date
- 2026-11-17
AI Technical Summary
Existing soil leaching technologies for heavy metal contaminated soil are inefficient under low water-to-soil ratio conditions, making it difficult to effectively break down soil aggregates and resulting in a decrease in heavy metal removal rates. Furthermore, traditional fiber material preparation methods suffer from defects such as poor pore orientation, wide pore size distribution, and insufficient structural stability, making them unsuitable for large-scale applications.
Porous fiber soil dispersion material was prepared by using sodium humate, γ-polyglutamic acid, and carboxymethyl chitosan as the main components, through a combined method of sol-gel microbubble-microfluidic centrifugal spinning-gradient drying micro-etching-plasma water bath crosslinking, constructing an ordered porous structure and enhancing dispersion ability.
It effectively disperses soil aggregates under low water-to-soil ratio, improves heavy metal removal rate, reduces water-to-soil ratio during leaching, is environmentally friendly, has a simple preparation process, and is suitable for soil heavy metal leaching.
Smart Images

Figure CN123107700A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a method for preparing and applying a sodium humate-based porous fiber soil dispersion material, belonging to the field of heavy metal contaminated soil remediation. Background Technology
[0002] Heavy metal pollution in soil is characterized by its insidious, long-term, and irreversible nature, seriously threatening agricultural product safety and groundwater quality. Among numerous remediation technologies, soil leaching has attracted widespread attention due to its ability to rapidly remove heavy metals. However, this technology has long faced a key bottleneck: to ensure sufficient contact between the leaching agent and soil particles, a high water-to-soil ratio (typically 10:1 or even higher) is usually required. The large amount of water used not only increases remediation costs but also generates massive amounts of leaching wastewater requiring subsequent treatment, severely restricting the large-scale engineering application of leaching technology. The fundamental reason for this predicament is that heavy metals are not uniformly distributed in soil but are mainly concentrated in the internal pores of fine aggregates, the interlayer of mineral layers, and adsorption sites encapsulated by organic matter films. Under high water-to-soil ratio conditions, hydraulic shear and diffusion mass transfer can partially overcome the mass transfer resistance within aggregates. However, when the water-to-soil ratio decreases, the system transforms into a viscous paste or moist granular state, the free liquid phase decreases sharply, and capillary forces tightly bind the aggregates together, making it difficult for the leachate to penetrate the micropores within the aggregates, resulting in a significant decrease in heavy metal removal rate. Therefore, how to effectively disintegrate soil aggregates and expand internal mass transfer channels under low water-to-soil ratio conditions is the core challenge for achieving water-saving and efficiency-enhancing soil leaching.
[0003] Currently, researchers both domestically and internationally have explored two main directions to address the low efficiency of soil leaching under low water-to-soil ratio conditions. The first is process enhancement, including physical methods such as ultrasonic assistance, pulsed stirring, and freeze-thaw cycle pretreatment to break down aggregate structures. While these methods can improve heavy metal removal rates under low water-to-soil ratio conditions to some extent, their high energy consumption, complex processes, and difficulty in in-situ implementation limit their large-scale application. The second is the development of functional leaching agents, such as enhancing the penetration and dispersion capabilities of agents by compounding surfactants or dispersants with traditional chelating agents (EDTA, citric acid, etc.). In recent years, micro / nanofiber materials with ordered porous structures have shown great potential in adsorption and separation due to their high specific surface area and interconnected mass transfer channels. However, research on using ordered porous microfibers as dispersion-mass transfer enhancement units in soil leaching is scarce. Current fiber preparation methods generally suffer from poor pore orientation, wide pore size distribution, and insufficient structural stability, making it difficult to meet the practical needs of soil remediation for low-cost, high-volume, and precisely controllable materials. Therefore, developing a novel soil dispersing agent with a highly ordered structure, good pore connectivity, efficient dispersion of soil aggregates under low water-to-soil ratio, and economically controllable preparation process is a technological gap that urgently needs to be filled in the current field of soil leaching. Summary of the Invention
[0004] The purpose of this invention is to address the current status and existing problems of leaching heavy metal contaminated soil, and to propose a method for preparing and applying a sodium humate-based porous fiber soil dispersion material.
[0005] A porous fiber soil dispersion material is prepared by a combined method of sol-gel microbubble-microfluidic centrifugal spinning-gradient drying micro-etching-plasma water bath crosslinking, with sodium humate, γ-polyglutamic acid and carboxymethyl chitosan as the main components.
[0006] The preparation method of this porous fiber soil dispersion material is as follows:
[0007] (1) Preparation of composite sol from sol-gel microbubbles
[0008] Sodium humate, γ-polyglutamic acid, gellan gum, carboxymethyl chitosan, and deionized water were weighed and mixed in a constant temperature water bath to form a mixed solution. Then, microcrystalline cellulose and nano silica were weighed and mixed with the mixed solution and dispersed in a disperser to obtain a mixed slurry. The mixed slurry was then placed in an ice-water bath and stirred continuously. During the stirring process, ammonium bicarbonate and glacial acetic acid were added in sequence. Finally, the mixture was placed in a vacuum drying oven for vacuum degassing to obtain a composite sol.
[0009] (2) Preparation of wet fiber mat by microfluidic centrifugal spinning
[0010] The composite sol obtained in step (1) is used as the inner phase fluid. Calcium chloride, glutaraldehyde solution and deionized water are weighed and mixed to form the outer phase fluid. Then, the inner and outer phase fluids are injected into the centrifugal spinning machine simultaneously through a dual-channel microfluidic chip for spinning. During the spinning process, compressed air is used to stretch the fiber axially and an ultrasonic atomizer is used to atomize and spray the low-temperature ethanol aqueous solution to the fiber throwing area. After spinning, wet fiber felt is obtained.
[0011] (3) Gradient drying micro-etching to construct porous structures
[0012] The wet fiber felt obtained in step (2) was immersed in tert-butanol aqueous solution at a constant temperature, then freeze-dried in a freeze dryer, and then vacuum-dried at a constant temperature in a vacuum drying oven to obtain ordered porous fibers.
[0013] (4) Preparation of dispersion materials by plasma water bath crosslinking
[0014] The ordered porous fibers obtained in step (3) were placed in a plasma surface treatment instrument. The plasma surface treatment instrument was first evacuated, then oxygen was introduced, and then surface treatment was performed. The modified ordered porous fibers were then placed in a mixed solution of genipin, glutaraldehyde solution, ethanol and deionized water. After swelling at room temperature, the solution was heated in a water bath and then washed with deionized water. Finally, the solution was placed in a vacuum drying oven and vacuum dried to obtain the dispersed material.
[0015] In the above method: the CAS number of sodium humate mentioned in step (1) is 68131-04-4, the CAS number of γ-polyglutamic acid is 25513-46-6, the CAS number of gellan gum is 71010-52-1, the CAS number of carboxymethyl chitosan is 83512-85-0, the CAS number of microcrystalline cellulose is 9004-34-6, the CAS number of nano silica is 60676-86-0, and the mass ratio of sodium humate, γ-polyglutamic acid, gellan gum, carboxymethyl chitosan, microcrystalline cellulose, nano silica, ammonium bicarbonate, and deionized water is 1: (0.7~1.5): (0.2~0.5): (0.1~0.2): (0.03~0.06): (0.09~0.18): (0.15~0.25): (10~25).
[0016] In the above method: the amount of glacial acetic acid added in step (1) is to adjust the pH of the mixed slurry to 5.0~6.0, the temperature of the constant temperature water bath is 50~70℃, the stirring speed of the constant temperature water bath is 150~300rpm, the stirring time of the constant temperature water bath is 3~6h, the dispersion speed is 6000~8000rpm, the dispersion time is 15~30min, the continuous stirring speed is 50~100rpm, the continuous stirring time is 20~40min, the vacuum degassing pressure is -0.08~-0.05MPa, and the vacuum degassing time is 20~40min.
[0017] In the above method: the mass concentration of glutaraldehyde solution in step (2) is 20~30%, the mass ratio of ethanol to deionized water in low-temperature ethanol aqueous solution is 1:(0.15~0.25), the temperature of low-temperature ethanol aqueous solution is -20℃~-10℃, and the mass ratio of calcium chloride, glutaraldehyde solution and deionized water is 1:(2~4):(100~200).
[0018] In the above method: the rate of the internal phase fluid in the spinning process described in step (2) is 0.6~1.2 mL / min, the rate of the external phase fluid is 0.4~0.8 mL / min, the rotation speed of the centrifugal spinning machine is 4000~6000 rpm, the pressure of the compressed air is 0.02~0.04 MPa, the power of the ultrasonic atomizer is 10~20 W, and the atomization rate of the ultrasonic atomizer is 0.3~0.6 mL / min.
[0019] In the above method: the mass fraction of tert-butanol in the aqueous solution of tert-butanol in step (3) is 30%~50%, the mass ratio of wet fiber felt to aqueous solution of tert-butanol is 1:(20~40), the temperature of constant temperature impregnation is 1~3℃, and the time of constant temperature impregnation is 20~40min.
[0020] In the above method: the freeze-drying temperature in step (3) is -50~-40℃, the freeze-drying time is 24~36h, the constant temperature vacuum drying temperature is 30~40℃, and the constant temperature vacuum drying time is 6~12h.
[0021] In the above method: the oxygen filling rate in step (4) is 30~50mL / min, the surface treatment power is 80~120W, the surface treatment time is 3~6min, the mass ratio of modified ordered porous fiber, genipin, glutaraldehyde solution, ethanol and deionized water is 1:(0.1~0.5):(10~20):(100~200):(10~20), and the mass concentration of glutaraldehyde solution is 20~30%.
[0022] In the above method: the room temperature swelling time in step (4) is 10~20 min, the water bath heating reaction temperature is 40~60℃, the water bath heating reaction time is 2~4 h, the vacuum drying temperature is 60~80℃, the vacuum drying gauge pressure is -0.09~-0.06 MPa, and the vacuum drying time is 3~6 h.
[0023] A porous fiber soil dispersion material, which is prepared by the method described above.
[0024] The dispersing materials prepared by the above method are used for soil dispersion in the process of leaching heavy metal contaminated soil.
[0025] Experimental conditions and results of the present invention: 100 g of clay was mixed with 2000 mL of deionized water, dried, and passed through a 2 mm sieve for the preparation of clean soil before use; 10 mg of cadmium carbonate was moistened with 3 mL of deionized water and sprayed onto 100 g of air-dried clean soil. The sample was then homogenized and aged at room temperature (25 °C) for 2 months to obtain simulated contaminated soil; 2 g of dispersion material, 200 g of deionized water, and 100 g of simulated contaminated soil were mixed, shaken with a vortex shaker for 2 min, and then allowed to stand vertically. After 10 min, the boundary between the supernatant and the sediment was recorded, and the stability dispersion index was calculated based on the percentage of the height of the supernatant to the total height of the liquid column. The stability dispersion index of the dispersion agent was between 35% and 40%.
[0026] Beneficial effects:
[0027] (1) Traditional spinning solution preparation usually involves simple mechanical stirring to mix the components evenly, followed by standing or vacuum degassing. The goal is only to obtain a homogeneous spinnable fluid, without giving the spinning solution additional structural template function. This invention constructs a composite sol system rich in microbubble templates using a three-in-one strategy of "in-situ chemical reaction to create pores - nanoparticle interface stabilization - selective vacuum degassing". Using ammonium bicarbonate and glacial acetic acid as foaming pairs, the core advantage is that the two can undergo a mild acid-base reaction under low-temperature ice-water bath conditions, generating carbon dioxide microbubbles in situ inside the sol. Compared with external gas injection or high-speed mechanical stirring foaming, in-situ gas generation through chemical reaction can make the bubbles nucleate evenly between the cross-linking points of the polymer network, resulting in smaller size and narrower distribution. Through microcrystalline fibers As co-dispersed components, silica and nano-silica not only enhance the filler but also spontaneously adsorb onto the bubble-liquid film interface due to their high surface energy, effectively inhibiting Ostwald ripening and agglomeration instability of microbubbles. Finally, vacuum degassing is used to selectively remove unstable macrobubbles that are large in size, have thin liquid films, and are not fully covered by nanoparticles. At the same time, the microbubbles adsorbed by nanoparticles expand moderately under negative pressure to homogenize their size distribution. Compared with conventional direct vacuum degassing or simple chemical foaming, the final composite sol avoids fiber breakage or defects caused by macrobubbles in subsequent spinning while preserving a high-density, uniformly sized microbubble community as an initial pore-forming template within the fiber, laying the foundation for the subsequent construction of an ordered porous structure.
[0028] (2) Traditional single-channel electrospinning or centrifugal spinning relies solely on solvent evaporation or coagulation bath immersion to achieve phase change solidification during fiber formation. The fiber formation process and the structure control process are separated, making it difficult to complete the synergistic construction of the multi-level fiber structure in a single step. This invention achieves the simultaneous completion of the "forming-skin crosslinking-internal pore formation-subsurface phase separation" of nascent fibers by integrating microfluidic dual-channel co-extrusion, high-speed centrifugal stretching, gas-assisted refining, and non-solvent vapor-induced phase separation. Gellan gum is selected as the calcium ion-responsive gel component. Its carboxyl-rich helical domains can instantaneously undergo ion bridging and conformational folding to form a dense gel skin after contacting calcium ions in the external calcium chloride solution, giving the nascent fibers wet strength to resist high centrifugal force and airflow stretching. Shearing action prevents fiber breakage; glutaraldehyde undergoes Schiff base crosslinking with the free amino groups of carboxymethyl chitosan in the cortex region, helping to strengthen the cortex stiffness and integrity; low-temperature ethanol-water solution is used as a non-solvent micro-mist, and ethanol, as a strong non-solvent for γ-polyglutamic acid, can instantly reduce the local solvent mass fraction when diffused into the high-temperature jet, initiating liquid-liquid phase separation to form precursors of polymer-poor nanodroplets. The low temperature not only allows the phase separation morphology to be instantly frozen and fixed, but also establishes a radial temperature gradient inside the fiber, pre-setting the directionality for the subsequent directional nucleation and growth of ice crystals; compared with the conventional serial process of spinning first and then performing phase separation or freezing treatment separately, the synergistic strategy of this invention shortens the process chain and avoids structural relaxation and morphological degradation caused by transfer operations between steps;
[0029] (3) Traditional porous fiber pore-forming technology often relies on adding water-soluble salts or polymers as sacrificial templates, which are removed by washing with water or solvent extraction after spinning. This has inherent defects such as incomplete template removal, easy collapse of pores, poor permeability, and difficulty in forming an ordered arrangement. This invention adopts a gradient drying strategy of "solvent replacement-step sublimation etching". It utilizes the unique physicochemical properties of tert-butanol molecules, which have high vapor pressure, high melting point, and needle-like crystallization habit, to use tert-butanol aqueous solution as solvent replacement medium, so that the deionized water in the fiber can be fully permeated and replaced without freezing. During the freeze-drying process, tert-butanol preferentially crystallizes to form needle-like whiskers with high aspect ratio, which induces the residual water to grow epitaxially along the same crystal axis direction into a bundle-like ice crystal array. Then, the ice crystals are sublimated in situ to leave an axially permeable micron-level main channel. Then, under room temperature vacuum, the tert-butanol molecules adsorbed in the polymer dense phase slowly escape, thereby etching nanoscale side pores in situ.
[0030] (4) Conventional fiber materials often employ two methods for crosslinking and curing after pore formation: thermal curing or solution crosslinking. Thermal curing requires placing the fiber in a high-temperature environment for a long time, which not only consumes a lot of energy, but more seriously, the high temperature will cause the finely constructed ordered porous structure to collapse due to the intensified thermal motion of polymer chain segments. Solution crosslinking usually involves immersing the entire fiber in a crosslinking agent solution and heating it back to the reflux. The crosslinking reaction progresses from the fiber surface to the core in a gradient, which can easily lead to an uneven state of excessive crosslinking in the skin and insufficient crosslinking in the core. Furthermore, the inner wall of the pores becomes rough due to the large amount of crosslinking agent adhering to it, and may even block the pore openings. This invention combines plasma surface activation and water bath crosslinking technology in the post-processing of ordered porous fibers. It utilizes high-energy oxygen free radicals to target the fiber surface and the inner wall of the pores. The bombardment can simultaneously achieve surface cleaning, high-density grafting of oxygen-containing polar functional groups (carboxyl, hydroxyl, carbonyl) and nanoscale physical etching. Furthermore, the peroxide free radicals and alkyl free radicals generated by the plasma on the polymer backbone will act as grafting initiation active sites in the subsequent crosslinking reaction, thereby achieving a seamless connection between physical activation and chemical curing. The crosslinking method uses genipin as the main crosslinking agent and glutaraldehyde to synergistically construct a three-dimensional network. Genipin preferentially undergoes mild Schiff base crosslinking with the free amino groups of carboxymethyl chitosan, while glutaraldehyde further forms acetal bridges between the hydroxyl groups of γ-polyglutamic acid and the phenolic hydroxyl groups of sodium humate. The synergy of the two extends the crosslinking from a single amino targeting to a "amino-hydroxyl-carboxyl" multi-component co-crosslinking system.
[0031] Therefore, the porous fiber soil dispersion material prepared by this invention is environmentally friendly and has a simple preparation process. It can effectively reduce the water-soil ratio during soil leaching and has the advantage of synergistic removal of heavy metals from the soil. This product can be widely used in the field of soil heavy metal leaching. Attached Figure Description
[0032] Figure 1 This is a scanning electron microscope image of the dispersion material prepared in Example 1;
[0033] Figure 2 The graph shows the stability dispersion index performance of the dispersion materials prepared in Examples 1-2 and Comparative Examples 1-6. Detailed Implementation
[0034] The present invention will be further described below with reference to the embodiments. The embodiments are implemented under the premise of the technical solution of the present invention, and detailed implementation methods and specific operation processes are given. However, the protection scope of the present invention is not limited to the following embodiments.
[0035] Example 1
[0036] (1) Preparation of composite sol from sol-gel microbubbles
[0037] Weigh out 10g sodium humate, 7g γ-polyglutamic acid, 2g gellan gum, 1g carboxymethyl chitosan, and 100g deionized water, mix them, and stir in a 50℃ constant temperature water bath for 6 hours (stirring speed of 150 rpm) to form a mixed solution. Then weigh out 0.3g microcrystalline cellulose and 0.9g nano silica, mix them with the mixed solution, and disperse them in a disperser (dispersion speed of 6000 rpm, dispersion time of 30 min) to obtain a mixed slurry. Then place the mixed slurry in an ice-water bath and stir continuously at a speed of 50 rpm for 40 min. During the stirring process, add 1.5g ammonium bicarbonate and adjust the pH of the mixed slurry to 5.0 with glacial acetic acid. Finally, place the mixture in a vacuum drying oven for vacuum degassing for 40 min (vacuum degassing pressure of -0.05MPa) to obtain a composite sol.
[0038] (2) Preparation of wet fiber mat by microfluidic centrifugal spinning
[0039] The composite sol obtained in step (1) was used as the inner phase fluid. 1g of calcium chloride, 2g of glutaraldehyde solution (CAS number 111-30-8, mass fraction of glutaraldehyde 25%), and 100g of deionized water were weighed and mixed to form the outer phase fluid. Then, the inner and outer phase fluids were simultaneously injected into a centrifugal spinning machine via a dual-channel microfluidic chip for spinning (the rate of the inner phase fluid during spinning was 0.6 mL / min, and the rate of the outer phase fluid was 0.4 mL / min). The rotating cup rotates at 4000 rpm. After the inner phase fluid is consumed, the outer phase fluid is stopped being injected simultaneously. During the spinning process, compressed air (pressure 0.02 MPa) is used to stretch the fiber axially. An ultrasonic atomizer (power 10W, atomization rate 0.3 mL / min) is used to atomize and spray a low-temperature ethanol aqueous solution (mass ratio of ethanol to deionized water 1:0.15, temperature -20℃) to the fiber throwing area. After spinning, a wet fiber mat is obtained.
[0040] (3) Gradient drying micro-etching to construct porous structures
[0041] 20g of the wet fiber felt obtained in step (2) was placed in 400g of 30% tert-butanol aqueous solution and immersed at a constant temperature (the temperature of the constant temperature immersion was 1℃ and the time of the constant temperature immersion was 20min). Then it was placed in a freeze dryer and freeze-dried at -50℃ for 24h. Then it was placed in a vacuum drying oven and vacuum-dried at 30℃ for 12h to obtain ordered porous fibers.
[0042] (4) Preparation of dispersion materials by plasma water bath crosslinking
[0043] The ordered porous fibers obtained in step (3) were placed in a plasma surface treatment instrument. The plasma surface treatment instrument was first evacuated, and then oxygen was introduced (the oxygen introduction rate was 30 mL / min). Then, surface treatment was performed (the surface treatment power was 80 W, and the surface treatment time was 6 min). Then, 10 g of the modified ordered porous fibers were placed in a mixed solution of 1 g genipin, 100 g glutaraldehyde solution (the CAS number of the glutaraldehyde solution was 111-30-8, and the mass fraction of glutaraldehyde was 25%), 1000 g ethanol, and 100 g deionized water. After swelling at room temperature for 10 min, the solution was heated in a water bath at 40 °C for 4 h. Then, the solution was washed with deionized water and finally placed in a vacuum drying oven at 60 °C for 6 h (the gauge pressure of the vacuum drying was -0.06 MPa) to obtain the dispersion material (the scanning electron microscope image of the dispersion material is shown in Figure 1). Figure 1 (as shown)
[0044] (5) Dispersion performance test
[0045] Clay (100 g) was mixed with deionized water (2000 mL), dried, and passed through a 2 mm sieve for use in preparing clean soil. 10 mg of cadmium carbonate was moistened with 3 mL of deionized water and sprayed onto 100 g of air-dried clean soil. The sample was then homogenized and aged at room temperature (25 ℃) for 2 months to obtain simulated contaminated soil. 2 g of dispersion material, 200 g of deionized water, and 100 g of simulated contaminated soil were mixed, vortexed for 2 min, and then allowed to stand vertically. After 10 min, the boundary between the supernatant and the sediment was recorded. The stability dispersion index was calculated based on the percentage of the supernatant height to the total liquid column height. The stability dispersion index of the dispersant was 36%.
[0046] Example 2
[0047] (1) Preparation of composite sol from sol-gel microbubbles
[0048] Weigh out 10g sodium humate, 15g γ-polyglutamic acid, 5g gellan gum, 2g carboxymethyl chitosan, and 250g deionized water, mix them, and stir in a 70℃ constant temperature water bath for 3 hours (stirring speed of 300 rpm) to form a mixed solution. Then weigh out 0.6g microcrystalline cellulose and 1.8g nano silica, mix them with the mixed solution, and disperse them in a disperser (dispersion speed of 8000 rpm, dispersion time of 15 min) to obtain a mixed slurry. Then place the mixed slurry in an ice-water bath and stir continuously at 100 rpm for 20 min. During the stirring process, add 2.5g ammonium bicarbonate and adjust the pH of the mixed slurry to 6.0 with glacial acetic acid. Finally, place the mixture in a vacuum drying oven for vacuum degassing for 20 min (vacuum degassing pressure of -0.08MPa) to obtain a composite sol.
[0049] (2) Preparation of wet fiber mat by microfluidic centrifugal spinning
[0050] The composite sol obtained in step (1) was used as the inner phase fluid. 1.5g of calcium chloride, 6g of glutaraldehyde solution (CAS number of glutaraldehyde solution is 111-30-8, mass fraction of glutaraldehyde is 25%), and 300g of deionized water were weighed and mixed to form the outer phase fluid. Then, the inner and outer phase fluids were simultaneously injected into a centrifugal spinning machine for spinning through a dual-channel microfluidic chip (the rate of the inner phase fluid during spinning was 1.2mL / min, and the rate of the outer phase fluid was 0.8mL / min, centrifugal spinning). The rotating cup of the machine rotates at 6000 rpm. After the inner phase fluid is consumed, the outer phase fluid stops being injected synchronously. During the spinning process, compressed air (pressure 0.04 MPa) is used to stretch the fiber axially. An ultrasonic atomizer (power 20W, atomization rate 0.6 mL / min) is used to atomize and spray a low-temperature ethanol aqueous solution (mass ratio of ethanol to deionized water 1:0.25, temperature -10℃) to the fiber throwing area. After spinning, a wet fiber mat is obtained.
[0051] (3) Gradient drying micro-etching to construct porous structures
[0052] 20g of the wet fiber felt obtained in step (2) was placed in 800g of 50% tert-butanol aqueous solution and immersed at a constant temperature (the temperature of the constant temperature immersion was 3℃ and the time of the constant temperature immersion was 40min). Then it was placed in a freeze dryer and freeze-dried at -40℃ for 36h. Then it was placed in a vacuum drying oven and vacuum-dried at 40℃ for 6h to obtain ordered porous fibers.
[0053] (4) Preparation of dispersion materials by plasma water bath crosslinking
[0054] The ordered porous fibers obtained in step (3) were placed in a plasma surface treatment instrument. The plasma surface treatment instrument was first evacuated, and then oxygen was introduced (the oxygen introduction rate was 50 mL / min). Then, surface treatment was performed (the surface treatment power was 120 W, and the surface treatment time was 3 min). Then, 10 g of the modified ordered porous fibers were placed in a mixed solution of 5 g genipin, 200 g glutaraldehyde solution (the CAS number of the glutaraldehyde solution was 111-30-8, and the mass fraction of glutaraldehyde was 25%), 2000 g ethanol and 200 g deionized water. The fibers were swollen at room temperature for 20 min, and then heated in a water bath at 60 °C for 2 h. After that, the fibers were washed with deionized water and finally placed in a vacuum drying oven at 80 °C for 3 h (the expression for vacuum drying is -0.09 MPa) to obtain the dispersion material.
[0055] (5) Dispersion performance test
[0056] Clay (100 g) was mixed with deionized water (2000 mL), dried, and passed through a 2 mm sieve for use in preparing clean soil. 10 mg of cadmium carbonate was moistened with 3 mL of deionized water and sprayed onto 100 g of air-dried clean soil. The sample was then homogenized and aged at room temperature (25 ℃) for 2 months to obtain simulated contaminated soil. 2 g of dispersion material, 200 g of deionized water, and 100 g of simulated contaminated soil were mixed, vortexed for 2 min, and then allowed to stand vertically. After 10 min, the boundary between the supernatant and the sediment was recorded, and the stability dispersion index was calculated based on the percentage of the supernatant height to the total liquid column height. The stability dispersion index of the dispersant was 39%.
[0057] Comparative Example 1
[0058] (1) Preparation of dispersion materials
[0059] Commercially available sodium humate (CAS No. 68131-04-4) was used as the dispersing material;
[0060] (2) Rinsing performance test
[0061] Clay (100 g) was mixed with deionized water (2000 mL), dried, and passed through a 2 mm sieve for use in preparing clean soil. 10 mg of cadmium carbonate was moistened with 3 mL of deionized water and sprayed onto 100 g of air-dried clean soil. The sample was then homogenized and aged at room temperature (25 ℃) for 2 months to obtain simulated contaminated soil. 2 g of dispersion material, 200 g of deionized water, and 100 g of simulated contaminated soil were mixed, vortexed for 2 min, and then allowed to stand vertically. After 10 min, the boundary between the supernatant and the sediment was recorded. The stability dispersion index was calculated based on the percentage of the supernatant height to the total liquid column height. The stability dispersion index of the dispersant was 63%.
[0062] Comparative Example 2
[0063] (1) Preparation of dispersion materials
[0064] Commercially available sodium dodecyl sulfate (CAS No. 151-21-3) was used as the dispersant.
[0065] (2) Rinsing performance test
[0066] Clay (100 g) was mixed with deionized water (2000 mL), dried, and passed through a 2 mm sieve for use in preparing clean soil. 10 mg of cadmium carbonate was moistened with 3 mL of deionized water and sprayed onto 100 g of air-dried clean soil. The sample was then homogenized and aged at room temperature (25 ℃) for 2 months to obtain simulated contaminated soil. 2 g of dispersion material, 200 g of deionized water, and 100 g of simulated contaminated soil were mixed, vortexed for 2 min, and then allowed to stand vertically. After 10 min, the boundary between the supernatant and the sediment was recorded. The stability dispersion index was calculated based on the percentage of the supernatant height to the total column height. The stability dispersion index of the dispersant was 13%.
[0067] Comparative Example 3
[0068] (1) Rinsing performance test
[0069] Clay (100 g) was mixed with deionized water (2000 mL), dried, and passed through a 2 mm sieve for use in preparing clean soil. 10 mg of cadmium carbonate was moistened with 3 mL of deionized water and sprayed onto 100 g of air-dried clean soil. The sample was then homogenized and aged at room temperature (25 ℃) for 2 months to obtain simulated contaminated soil. 200 g of deionized water and 100 g of simulated contaminated soil were mixed, vortexed for 2 min, and then allowed to stand vertically. After 10 min, the boundary between the supernatant and the sediment was recorded. The stability dispersion index was calculated based on the percentage of the supernatant height to the total liquid column height. The stability dispersion index was 84%.
[0070] Comparative Example 4
[0071] (1) Preparation of dispersion materials
[0072] Except that ammonium bicarbonate and glacial acetic acid are not added in step (1), the other conditions are the same as in Example 1;
[0073] (2) Rinsing performance test
[0074] Clay (100 g) was mixed with deionized water (2000 mL), dried, and passed through a 2 mm sieve for use in preparing clean soil. 10 mg of cadmium carbonate was moistened with 3 mL of deionized water and sprayed onto 100 g of air-dried clean soil. The sample was then homogenized and aged at room temperature (25 ℃) for 2 months to obtain simulated contaminated soil. 2 g of dispersion material, 200 g of deionized water, and 100 g of simulated contaminated soil were mixed, vortexed for 2 min, and then allowed to stand vertically. After 10 min, the boundary between the supernatant and the sediment was recorded, and the stability dispersion index was calculated based on the percentage of the supernatant height to the total liquid column height. The stability dispersion index of the dispersant was 59%.
[0075] Comparative Example 5
[0076] (1) Preparation of dispersion materials
[0077] Except for step (3), which does not use a constant temperature immersion in tert-butanol aqueous solution, the other conditions are the same as in Example 1;
[0078] (2) Rinsing performance test
[0079] Clay (100 g) was mixed with deionized water (2000 mL), dried, and passed through a 2 mm sieve for use in preparing clean soil. 10 mg of cadmium carbonate was moistened with 3 mL of deionized water and sprayed onto 100 g of air-dried clean soil. The sample was then homogenized and aged at room temperature (25 ℃) for 2 months to obtain simulated contaminated soil. 2 g of dispersion material, 200 g of deionized water, and 100 g of simulated contaminated soil were mixed, vortexed for 2 min, and then allowed to stand vertically. After 10 min, the boundary between the supernatant and the sediment was recorded, and the stability dispersion index was calculated based on the percentage of the supernatant height to the total liquid column height. The stability dispersion index of the dispersant was 67%.
[0080] Comparative Example 6
[0081] (1) Preparation of dispersion materials
[0082] Except for the absence of plasma treatment in step (4), the other conditions are the same as in Example 2;
[0083] (2) Rinsing performance test
[0084] Clay (100 g) was mixed with deionized water (2000 mL), dried, and passed through a 2 mm sieve for use in preparing clean soil. 10 mg of cadmium carbonate was moistened with 3 mL of deionized water and sprayed onto 100 g of air-dried clean soil. The sample was then homogenized and aged at room temperature (25 °C) for 2 months to obtain simulated contaminated soil. 2 g of dispersion material, 200 g of deionized water, and 100 g of simulated contaminated soil were mixed, vortexed for 2 min, and then allowed to stand vertically. After 10 min, the boundary between the supernatant and the sediment was recorded. The stability dispersion index was calculated based on the percentage of the supernatant height to the total column height. The stability dispersion index of the dispersant was 49%.
[0085] Comparative analysis of Comparative Examples 1 to 3
[0086] In conventional heavy metal soil leaching processes, water and clay are first mixed, then leaching agents are added to complex the heavy metals, and finally, the soil and waste liquid are separated by filtration. Under these conditions, adding commercially available sodium humate with a high stability and dispersion index (which only chemically disperses and cannot physically break down aggregates, resulting in rapid sedimentation) or not adding any dispersant can lead to an excessively high stability and dispersion index in the slurry (Comparative Example 1 and Comparative Example 3). This can result in the leaching agent not being able to fully contact the soil particles, requiring a high water-to-soil ratio, which leads to a large amount of water consumption and the generation of a huge amount of leached waste liquid. On the other hand, if commercially available sodium dodecyl sulfate with a low stability and dispersion index is added (Comparative Example 2), although sodium dodecyl sulfate, as a small molecule surfactant, can quickly reduce interfacial tension and suspend fine particles to maintain slurry stability, after leaching, it is difficult to achieve rapid separation of clear water and sludge through natural sedimentation or centrifugation, which significantly increases the cost and time of subsequent wastewater treatment.
[0087] Comparative analysis of Comparative Examples 4 to 6
[0088] Compared to Example 1, Comparative Example 4 did not add ammonium bicarbonate and glacial acetic acid, so microbubbles could not be generated in situ in the composite sol. Therefore, the process of secondary gas release to form initial micropores triggered by the acidic external phase crosslinking bath was missing during spinning in step (2). Although the final fiber can still form an axially penetrating main channel through the directional ice template in step (3), the number of side holes on the pore wall is significantly reduced, resulting in a significant decrease in the specific surface area of the fiber. The mechanical interlocking and wedging dismantling ability of the fiber with soil aggregates is reduced, resulting in a significant increase in the stability dispersion index, which is not conducive to soil dispersion.
[0089] Compared with Example 1, Comparative Example 5 did not use tert-butanol aqueous solution for constant temperature impregnation. The free water inside the fiber froze into dendritic random ice crystals. After sublimation, the remaining channels were curved, had poor orientation, low penetration rate, and lacked nano-side pores in the tube wall. The specific surface area also decreased significantly. The physical wedging and mass transfer capacity of the fiber and soil aggregates were reduced, resulting in a significant increase in the stability dispersion index, which was not conducive to soil dispersion.
[0090] Compared with Example 2, Comparative Example 6 did not use plasma treatment, and the fiber surface lacked high-abundance oxygen-containing functional groups. The hydrophilicity and electronegativity were significantly reduced, which weakened the chemical dispersion effect and thus improved the stability dispersion index.
Claims
1. A method of making a porous fibrous soil-dispersing material, characterized by: The method includes the following steps: (1) Preparation of composite sol from sol-gel microbubbles Sodium humate, γ-polyglutamic acid, gellan gum, carboxymethyl chitosan, and deionized water were mixed and stirred in a constant temperature water bath to form a mixed solution. Microcrystalline cellulose and nano silica were mixed with the mixed solution and dispersed in a disperser to obtain a mixed slurry. The mixed slurry was then placed in an ice-water bath and stirred continuously. During the stirring process, ammonium bicarbonate and glacial acetic acid were added in sequence to obtain a mixture. Finally, the mixture was placed in a vacuum drying oven for vacuum degassing to obtain a composite sol. (2) Preparation of wet fiber mat by microfluidic centrifugal spinning The composite sol obtained in step (1) is used as the inner phase fluid. Calcium chloride, glutaraldehyde solution and deionized water are weighed and mixed to form the outer phase fluid. Then, the inner and outer phase fluids are injected into the centrifugal spinning machine simultaneously through a dual-channel microfluidic chip for spinning. During the spinning process, compressed air is used to stretch the fiber axially and an ultrasonic atomizer is used to atomize and spray the low-temperature ethanol aqueous solution to the fiber throwing area. After spinning, wet fiber felt is obtained. (3) Gradient drying micro-etching to construct porous structures The wet fiber felt obtained in step (2) was immersed in tert-butanol aqueous solution at a constant temperature, then freeze-dried in a freeze dryer, and then vacuum-dried at a constant temperature in a vacuum drying oven to obtain ordered porous fibers. (4) Preparation of dispersion materials by plasma water bath crosslinking The ordered porous fibers obtained in step (3) were placed in a plasma surface treatment instrument. The plasma surface treatment instrument was first evacuated, then oxygen was introduced, and then surface treatment was performed. The modified ordered porous fibers were then placed in a mixed solution of genipin, glutaraldehyde solution, ethanol and deionized water. After swelling at room temperature, the solution was heated in a water bath and then washed with deionized water. Finally, the solution was placed in a vacuum drying oven and vacuum dried to obtain the dispersed material.
2. The method of claim 1, wherein: In step (1), the mass ratio of sodium humate, γ-polyglutamic acid, gellan gum, carboxymethyl chitosan, microcrystalline cellulose, nano silica, ammonium bicarbonate, and deionized water is 1: (0.7~1.5): (0.2~0.5): (0.1~0.2): (0.03~0.06): (0.09~0.18): (0.15~0.25): (10~25).
3. The preparation method according to claim 1, characterized in that: The amount of glacial acetic acid added in step (1) is to adjust the pH of the mixed slurry to 5.0~6.0; The temperature of the constant temperature water bath is 50~70℃, the stirring speed is 150~300rpm, and the stirring time is 3~6h. The dispersion rate of the disperser is 6000~8000 rpm, and the dispersion time is 15~30 min; The stirring speed is 50~100 rpm, and the stirring time is 20~40 min; the vacuum degassing pressure is -0.08~-0.05 MPa, and the vacuum degassing time is 20~40 min.
4. The preparation method according to claim 1, characterized in that: In step (2), the mass ratio of ethanol to deionized water in the low-temperature ethanol aqueous solution is 1:(0.15~0.25), and the temperature of the low-temperature ethanol aqueous solution is -20℃~-10℃; The mass ratio of calcium chloride, glutaraldehyde solution, and deionized water is 1:(2~4):(100~200), and the mass concentration of glutaraldehyde solution is 20~30%.
5. The preparation method according to claim 1, characterized in that: In step (2), the rate of the internal phase fluid during the spinning process is 0.6~1.2 mL / min, the rate of the external phase fluid is 0.4~0.8 mL / min, the rotation speed of the centrifugal spinning machine is 4000~6000 rpm, the pressure of the compressed air is 0.02~0.04 MPa, the power of the ultrasonic atomizer is 10~20 W, and the atomization rate of the ultrasonic atomizer is 0.3~0.6 mL / min.
6. The preparation method according to claim 1, characterized in that: In step (3), the mass fraction of tert-butanol in the aqueous solution is 30%~50%, the mass ratio of wet fiber felt to aqueous solution of tert-butanol is 1:(20~40), the temperature of constant temperature impregnation is 1~3℃, and the time of constant temperature impregnation is 20~40min.
7. The preparation method according to claim 1, characterized in that: The freeze-drying temperature in step (3) is -50~-40℃ and the freeze-drying time is 24~36h; the constant temperature vacuum drying temperature is 30~40℃ and the constant temperature vacuum drying time is 6~12h.
8. The preparation method according to claim 1, characterized in that: The oxygen filling rate in step (4) is 30-50 mL / min, the surface treatment power is 80-120 W, the surface treatment time is 3-6 min, the mass ratio of the modified ordered porous fiber, genipin, glutaraldehyde solution, ethanol and deionized water is 1:(0.1-0.5):(10-20):(100-200):(10-20); the mass concentration of glutaraldehyde solution is 20-30%. The room temperature swelling time in step (4) is 10~20 min, the water bath heating reaction temperature is 40~60℃, the water bath heating reaction time is 2~4 h, the vacuum drying temperature is 60~80℃, the vacuum drying gauge pressure is -0.09~-0.06 MPa, and the vacuum drying time is 3~6 h.
9. A porous fiber soil dispersion material, characterized in that, The dispersion material is prepared by the method described in any one of claims 1 to 8.
10. The application of the dispersing material according to claim 9 in soil dispersion during the leaching of heavy metal contaminated soil.