A method for improving the high-temperature tensile properties of FGH99 alloy inertial friction welded joints
The high-temperature tensile properties of FGH99 alloy inertial friction welded joints were improved by two-stage aging heat treatment, which solved the problem of performance degradation caused by γ′ phase decomposition after welding, and achieved the improvement of high-temperature tensile properties and the maintenance of component dimensional accuracy.
Patent Information
- Application Number
- CN202611521341.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-29
- Publication Date
- 2026-11-17
AI Technical Summary
After inertial friction welding, the γ′ phase decomposes at the welding interface and near-weld zone of nickel-based powder superalloys, resulting in a decrease in the high-temperature tensile properties and elongation of the weld joint. Existing heat treatment methods are difficult to effectively increase the precipitation of strengthening phases without affecting the dimensional accuracy of the components.
A two-stage aging heat treatment method is adopted. The first stage aging temperature is 800℃ to 820℃, and the second stage aging temperature is 760℃ to 780℃, both of which are lower than the solution temperature. Combined with inertial friction welding, a metallurgical bond is formed, which promotes the full precipitation of the γ′ phase in the weld area and maintains a fine-grained structure.
The high-temperature tensile strength, yield strength and elongation of nickel-based powder superalloy inertial friction welded joints were improved, the residual stress and heat treatment crack risk were reduced, and the dimensional accuracy of the components was maintained.
Smart Images

Figure CN123108271A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of inertial friction welding and heat treatment technology, and more specifically, to a method for improving the high-temperature tensile properties of FGH99 alloy inertial friction welded joints. Background Technology
[0002] As turbine inlet temperatures in aero-engine design specifications continue to rise, the materials used in high-pressure compressor rotor assemblies are gradually transitioning from wrought superalloys to powder metallurgy superalloys. Powder metallurgy superalloys possess characteristics such as uniform microstructure, minimal macroscopic segregation, high alloying degree, high yield strength, and excellent fatigue resistance, making them crucial materials for key hot-end components such as high-pressure compressor disks and turbine disks in advanced aero-engines. Among these, third-generation nickel-based powder metallurgy superalloys, with a γ-phase as the matrix and a γ′-phase as the main reinforcing phase, are highly alloyed nickel-based powder metallurgy superalloys with a high volume fraction of reinforcing phases. Their high-temperature strength largely depends on the dispersed strengthening effect of the γ′-phase and is highly sensitive to the precipitation state of the reinforcing phase. Rotor assemblies manufactured using this type of alloy typically require long-term service at high temperatures, and the components are often pre- or nearly pre-machined before welding, thus placing high demands on the high-temperature mechanical properties of the welded joints and the dimensional accuracy of the components.
[0003] Inertial friction welding is a typical solid-state joining technology. This process involves rotating one workpiece at high speed with a flywheel to store rotational kinetic energy, then applying pressure and friction to the end face of a stationary workpiece. This rotational kinetic energy is converted into interfacial frictional heat, causing the weld interface metal to plastically soften at a temperature below the melting point of the base metal. Under the coupled action of high temperature, axial pressure, and torsional shear, the thermoplastic metal at the interface is extruded to form flash, and the original oxide film and inclusions at the interface are expelled with the flash. Simultaneously, dynamic recrystallization and solid-state microstructure transformation occur at the weld interface, ultimately achieving metallurgical bonding. Because the metal does not melt during the entire welding process, inertial friction welding effectively avoids solidification defects such as hot cracking, porosity, and compositional segregation that are prone to occur in fusion welding processes such as electron beam welding. Therefore, it has become one of the commonly used processes for achieving high-quality joining of nickel-based powder superalloys.
[0004] However, when the above-mentioned nickel-based powder superalloys are joined by inertial friction welding, the welding interface and its near-weld zone undergo high-temperature thermal cycling and severe plastic deformation during the welding process. The temperature can reach or even exceed the dissolution temperature of the main strengthening phase. The precipitated γ′ phase undergoes extensive decomposition or even re-dissolution. The volume fraction of the strengthening phase in the weld zone is significantly lower than that of the base material, and the high-temperature tensile properties and elongation of the joint decrease accordingly.
[0005] To address the issue of post-weld re-dissolution of strengthening phases, related technologies typically involve overall heat treatment of the welded assembly to promote the re-precipitation of these phases. However, such heat treatment methods, if raising the heating temperature to a level sufficient for adequate phase precipitation, can easily lead to significant deformation of the welded assembly, affecting dimensional accuracy. Conversely, if the heating temperature is lowered to avoid such deformation and microstructure coarsening, the thermodynamic driving force for strengthening phase precipitation becomes insufficient, resulting in a difference between the amount of re-precipitated strengthening phase in the weld and the base material, limiting the improvement in the high-temperature tensile properties and elongation of the joint.
[0006] Therefore, how to improve the high-temperature tensile properties of nickel-based powder superalloy inertial friction welded joints has become a technical problem that urgently needs to be solved by those skilled in the art. Summary of the Invention
[0007] The purpose of this application is to disclose a method for improving the high-temperature tensile properties of FGH99 alloy inertial friction welded joints, so as to improve the high-temperature tensile properties of nickel-based powder superalloy inertial friction welded joints.
[0008] Another objective of this application is to disclose a nickel-based powder superalloy inertial friction welding head prepared by the above-described method for improving the high-temperature tensile properties of FGH99 alloy inertial friction welding head.
[0009] A method for improving the high-temperature tensile properties of FGH99 alloy inertial friction welded joints includes the following steps:
[0010] Step S10: Provide two FGH99 nickel-based powder superalloy parts that have undergone solution treatment and aging treatment;
[0011] Step S20: Weld the two parts to be welded using inertial friction welding to form a metallurgical bond on the surfaces to be welded, thus obtaining a welded joint.
[0012] Step S30: Perform a two-stage aging heat treatment on the welded joint after welding. First, heat the welded joint to the first-stage aging temperature and hold it at that temperature. After holding, cool it down to the second-stage aging temperature and hold it at that temperature. After holding, cool it to room temperature. The first-stage aging temperature is 800℃ to 820℃ and the holding time is 1 hour to 4 hours. The second-stage aging temperature is 760℃ to 780℃ and the holding time is 1 hour to 4 hours. Both the first-stage aging temperature and the second-stage aging temperature are lower than the solution temperature of the workpiece to be welded.
[0013] In one possible implementation, the first aging temperature is 800°C, the second aging temperature is 760°C, and the holding time for both the first and second aging temperatures is 2 hours.
[0014] In one possible implementation, in step S30, the heating rate to the first aging temperature is 100°C / hour to 300°C / hour; the cooling method after the second aging and heat preservation is air cooling.
[0015] In one possible implementation, the volume fraction of the γ′ phase in the FGH99 nickel-based powder superalloy is not less than 40%, the solution temperature of the FGH99 nickel-based powder superalloy is 1150°C, and the aging temperature of the base material is 760°C.
[0016] In one possible implementation, step S10 includes the following steps:
[0017] Step S11: The workpiece to be welded, which has undergone solution treatment and aging treatment, is machined into a hollow cylindrical part. After machining, the wall thickness of the welding part of the workpiece to be welded is 6mm to 12mm.
[0018] Step S12: Grind the surface of the workpiece to be welded to remove oxide scale and oil stains;
[0019] Step S13: Clean the polished workpiece with anhydrous ethanol and then dry it.
[0020] In one possible implementation, when the incoming workpiece is in a solution-treated state, the solution-treated workpiece is subjected to an aging heat treatment at 760°C for at least 4 hours in step S10.
[0021] In one possible implementation, in step S20, the process parameters for inertial friction welding are: a moment of inertia of 20 kg·m. 2 Up to 45 kg·m 2 The rotation speed is 1000 r / min to 1400 r / min, and the welding pressure is 8 MPa to 12 MPa.
[0022] In one possible implementation, in step S20, the shortening of the welded joint after welding is greater than 2 mm and does not exceed 5 mm.
[0023] In one possible implementation, after step S30, at least one of the following tests is performed on the heat-treated welded joint:
[0024] Perform metallographic dissection examination;
[0025] Perform non-destructive testing, wherein the non-destructive testing is one or more of fluorescence detection, ultrasonic detection and X-ray detection;
[0026] High-temperature tensile property test at 650℃, tensile rate of 1mm / min, test indexes include one or more of tensile strength, yield strength, elongation after fracture and reduction of area.
[0027] Microscopic tissue characterization is performed, wherein the microscopic tissue characterization is one or more of scanning electron microscopy characterization, electron backscatter diffraction characterization, and transmission electron microscopy characterization.
[0028] Compared to related technologies, the method disclosed in this application for improving the high-temperature tensile properties of FGH99 alloy friction fusion welded joints employs a two-stage aging heat treatment after welding. Both the first and second stage aging temperatures are lower than the solution temperature of the nickel-based powder superalloy, thus eliminating the need for solution treatment on components already close to their precision-machined dimensions. This helps avoid significant deformation caused by solution treatment and maintains the dimensional accuracy of the components. The two-stage aging creates a gradient heat treatment near the aging temperature of the base material, increasing the thermodynamic driving force for the recrystallization of the γ′ phase. This promotes the full precipitation of the γ′ phase decomposed during welding in the weld region, enhancing the strengthening effect of the weld area. Simultaneously, it helps reduce residual stress in the joint and decreases the risk of heat treatment cracks. The nickel-based powder superalloy friction fusion welded joints prepared by this method exhibit improved high-temperature tensile strength, yield strength, elongation after fracture, and reduction of area at 650°C, while also helping to maintain a fine-grained weld structure, resulting in a better balance between strength and plasticity.
[0029] A nickel-based powder superalloy inertial friction welding head is prepared by a method for improving the high-temperature tensile properties of an FGH99 alloy inertial friction welding head as described in any of the above possible embodiments; the nickel-based powder superalloy inertial friction welding head includes a weld zone and a base material zone located outside the weld zone;
[0030] The volume fraction of the γ′ phase in the weld zone is not less than 40%; the grain size of the weld zone is smaller than the grain size of the base material zone, and the grain orientation of the weld zone is randomly distributed; the tensile strength of the nickel-based powder superalloy inertial friction welded joint at 650℃ is not less than 1400MPa.
[0031] The nickel-based powder superalloy inertial friction welding head provided in this application is made by the above-mentioned method for improving the high-temperature tensile properties of the FGH99 alloy inertial friction welding head, and therefore has all the technical effects of the above method, which will not be repeated here. Attached Figure Description
[0032] To more clearly illustrate the technical solutions in the embodiments or related technologies of this application, the accompanying drawings used in the description of the embodiments or related technologies will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0033] Figure 1This is a flowchart of a method for improving the high-temperature tensile properties of FGH99 alloy inertial friction welded joints, as disclosed in an embodiment of this application.
[0034] Figure 2 This is a flowchart of step S10 in the method for improving the high-temperature tensile properties of FGH99 alloy inertial friction welded joints disclosed in the embodiments of this application;
[0035] Figure 3 The image shows a scanning electron microscope (SEM) image of the welded joint disclosed in the embodiments of this application.
[0036] Figure 4 The image shows a scanning electron microscope tissue image of the connector obtained as a comparative example disclosed in this application. Detailed Implementation
[0037] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0038] In related technologies, nickel-based powder superalloys are used in key components such as high-pressure compressor disks and turbine disks of aero-engines due to their uniform microstructure, small macroscopic segregation, high alloying degree, high yield strength, and excellent fatigue resistance. Third-generation high-alloy nickel-based powder superalloys, represented by FGH99, use the γ phase as the matrix and the γ′ phase as the main strengthening phase, with the γ′ phase volume fraction reaching over 40%. After inertial friction welding, the γ′ phase in this type of alloy undergoes significant decomposition in the weld region, leading to a decrease in the high-temperature tensile strength and elongation of the joint. While post-weld heat treatment using the solution treatment and aging temperature combination of the base metal can promote the recrystallization of the γ′ phase, the welded components are already close to their precision-machined dimensions, and solution treatment at these temperatures can easily cause significant deformation, affecting the dimensional accuracy of the components. Single-stage aging using only the base metal aging temperature provides limited improvement in the high-temperature tensile strength and elongation of the joint.
[0039] Based on this, this application provides a method for improving the high-temperature tensile properties of FGH99 alloy inertial friction welded joints. The method involves first performing inertial friction welding on nickel-based powder superalloy parts that have undergone solution treatment and aging treatment to form a metallurgical bond on the weld surfaces. Subsequently, a two-stage aging heat treatment is performed: the first stage aging temperature is 800℃ to 820℃ with a holding time of 1 to 4 hours, and the second stage aging temperature is 760℃ to 780℃ with a holding time of 1 to 4 hours. Both aging temperatures are lower than the solution temperature of the nickel-based powder superalloy. Through this method, without resorting to solution treatment or affecting the dimensional accuracy of the parts, the dissolved γ′ phase in the weld is induced to reprecipitate, while preserving the fine-grained structure of the weld, thereby improving the high-temperature tensile strength and elongation of the joint.
[0040] The basic embodiments of this application will now be described with reference to the accompanying drawings.
[0041] See Figure 1 The method for improving the high-temperature tensile properties of FGH99 alloy inertial friction welded joints provided in this application includes steps S10, S20 and S30.
[0042] In step S10, two nickel-based powder superalloy parts to be welded are provided after solution treatment and aging treatment. Solution treatment refers to heating the alloy to the solution temperature and holding it at that temperature to dissolve the strengthening phase into the matrix, followed by cooling to obtain a supersaturated solid solution. Aging treatment refers to heating the alloy to a certain temperature and holding it at that temperature after solution treatment to precipitate the strengthening phase. After solution treatment and aging treatment, the microstructure of the parts to be welded is a state in which precipitated γ′ phases are distributed on a γ matrix. Nickel-based powder superalloys refer to nickel-based powder metallurgy superalloys with γ phase as the matrix and γ′ phase as the main strengthening phase. For example, this type of alloy can be the third-generation high-alloy nickel-based powder superalloy FGH99, which has a high volume fraction of γ′ phase.
[0043] In step S20, inertial friction welding is used to weld two workpieces to form a metallurgical bond between their surfaces, resulting in a welded joint. During welding, the two workpieces are clamped at the rotating end and the sliding end of the inertial friction welding equipment, respectively. The rotating end is connected to a flywheel, which accelerates to a set speed and then disengages from the motor. The workpiece at the sliding end contacts the workpiece at the rotating end under welding pressure. The welding interface rapidly heats up under frictional heat, causing plastic softening of the interface metal. The thermoplastic metal is extruded under axial pressure and torsional shear coupling, forming flash. Oxides at the original welding interface are discharged with the flash, achieving self-cleaning. When the speed of the flywheel and the workpiece at the rotating end drops to zero, the pressure is maintained for a period of time, and the welding interface achieves metallurgical bonding, completing the welding. Throughout the welding process, the metal does not melt, and the joint does not exhibit solidification defects common in fusion welding processes, such as hot cracking, porosity, and component segregation. Therefore, it is suitable for joining nickel-based powder superalloys with high γ′ phase volume fractions and sensitivity to hot cracking.
[0044] In step S30, the welded joint undergoes a two-stage post-weld aging heat treatment. First, the welded joint is heated to the first-stage aging temperature and held at that temperature. After holding, it is cooled to the second-stage aging temperature and held at that temperature. After holding, it is cooled to room temperature. The first-stage aging temperature is 800℃ to 820℃, and the holding time is 1 hour to 4 hours. The second-stage aging temperature is 760℃ to 780℃, and the holding time is 1 hour to 4 hours. Both the first and second-stage aging temperatures are lower than the solution temperature of the nickel-based powder superalloy. The two-stage aging creates a gradient heat treatment near the aging temperature of the base material, resulting in a significant thermodynamic driving force for the precipitation of the γ′ phase. The γ′ phase dissolved in the weld is fully precipitated during the heat treatment process. After the two-stage aging, the volume fraction of the γ′ phase in the weld zone is not less than 40%, essentially reaching a level comparable to that of the base material. Moreover, since both the first and second-stage aging temperatures are lower than the solution temperature, the post-weld heat treatment will not cause overall solution treatment or significant deformation of the part. The formed dynamic recrystallized fine-grained structure does not undergo grain growth or static recrystallization coarsening, allowing the weld to maintain a grain size smaller than that of the base metal and a random grain orientation, thus preserving the fine-grain strengthening effect.
[0045] In one specific embodiment, the nickel-based powder superalloy is the third-generation high-alloyed nickel-based powder superalloy FGH99, with a γ′ phase volume fraction of not less than 40%, a solution temperature of 1150℃, and a base metal aging temperature of 760℃. The matrix of FGH99 is the γ phase, and the strengthening phase is mainly γ′(Ni3(Al,Ti)). In the two-stage aging heat treatment of this application, the first-stage aging temperature is higher than the base metal aging temperature, and the second-stage aging temperature is similar to the base metal aging temperature, both of which are lower than the solution temperature. Due to the high γ′ phase volume fraction of FGH99, the γ′ phase decomposes significantly after inertial friction welding. The two-stage aging heat treatment of this application can promote the re-precipitation of the γ′ phase under conditions lower than the solution temperature.
[0046] Furthermore, the first-stage aging temperature is 800℃, and the second-stage aging temperature is 760℃, with a holding time of 2 hours for both stages. Under these values, the first-stage aging temperature is approximately 40℃ higher than the base metal aging temperature, while the second-stage aging temperature is the same as the base metal aging temperature. The total holding time for both stages is 4 hours, achieving a better balance between γ′ phase precipitation and weld grain stability.
[0047] In one specific implementation, the heating rate in step S30 to the first-stage aging temperature can be between 100°C / hour and 300°C / hour, for example, 200°C / hour. When the heating rate is within this range, the temperature distribution of the component tends to be uniform during the heating process, reducing the risk of cracking. The cooling method after the second-stage aging and holding is air cooling. Air cooling can avoid excessive thermal stress that may be caused by water cooling or oil cooling, thereby reducing the risk of heat treatment cracks. It should be noted that the heating rate and cooling method can be adjusted according to the joint size and the conditions of the heat treatment furnace, as long as the two-stage aging temperature can be achieved and significant cracking is avoided.
[0048] See Figure 2 Step S10 may include steps S11, S12 and S13.
[0049] In step S11, the workpiece to be welded, after solution treatment and aging, is machined into a hollow cylindrical part. After machining, the wall thickness of the welding area of the workpiece is 6mm to 12mm, exemplarily 9mm. If the wall thickness of the welding area is too small, the weld interface is prone to instability under axial pressure, and the amount of thermoplastic metal extruded is insufficient, resulting in inadequate interface self-cleaning. If the wall thickness of the welding area is too large, the temperature gradient along the wall thickness direction increases, requiring a larger moment of inertia and axial pressure to complete interface softening at the set rotational speed. For tubular samples using FGH99, with an outer diameter of 47mm, the wall thickness of the welding area can be correspondingly 9mm. Under this set of dimensions, the joint shortening and flash formation are relatively stable.
[0050] In step S12, the surface of the workpiece to be welded is polished to remove oxide scale and oil. For example, polishing can be performed by using sandpaper to treat the surface.
[0051] In step S13, the polished workpiece is cleaned with anhydrous ethanol and then dried. For example, the polished workpiece can be immersed in anhydrous ethanol for ultrasonic cleaning, then removed and dried for later use. Step S12 polishes to remove oxide scale, and step S13 further removes embedded grinding debris and residual oil, both of which together reduce the possibility of oxide inclusions at the welding interface. A clean surface for welding helps reduce the adverse effects of oxides and oil at the welding interface on metallurgical bonding.
[0052] In some embodiments, when the incoming workpiece is in a solution-treated state, the solution-treated workpiece is subjected to an aging heat treatment at 760°C for at least 4 hours in step S10. For example, this aging heat treatment is performed at 760°C for 8 hours. This aging heat treatment transforms the solution-treated incoming workpiece into a solution-treated and aged state, thereby obtaining a base material microstructure with a γ′ strengthening phase before welding. This aging heat treatment can be performed before or after step S11, as long as the workpiece has been aged before welding.
[0053] The process parameters for inertial friction welding in step S20 can be: a moment of inertia of 20 kg·m. 2 Up to 45 kg·m 2 The rotational speed is 1000 r / min to 1400 r / min, and the welding pressure is 8 MPa to 12 MPa. For example, the moment of inertia is 25 kg·m. 2 The rotational speed is 1000 r / min, and the welding pressure is 10 MPa. The moment of inertia and rotational speed together determine the rotational kinetic energy stored in the flywheel, which in turn determines the interfacial frictional heat power and welding heat input. The welding pressure determines the extrusion rate of the interfacial thermoplastic metal and the upsetting effect. Insufficient heat input results in inadequate softening of the interfacial metal, making it difficult for the interfacial oxide film to be fully removed with the flash. Excessive heat input leads to excessive flash, excessive joint shortening, and a tendency for weld grain coarsening. The above parameter range aims to control the heat input within a reasonable range while ensuring sufficient interfacial softening and self-cleaning.
[0054] In one specific embodiment, the shrinkage of the weld joint after welding in step S20 is greater than 2 mm and does not exceed 5 mm, exemplarily 2.1 mm. The shrinkage is a direct measure of the amount of thermoplastic metal extruded from the interface. A shrinkage greater than 2 mm helps to ensure that all the original thermoplastic metal at the weld interface is extruded to form flash, promoting thorough self-cleaning of weld oxides. A shrinkage not exceeding 5 mm avoids excessive material extrusion and excessive welding energy input, which is beneficial for controlling joint formation and microstructure.
[0055] After step S30, at least one of the following tests can be performed on the heat-treated welded joint. The first test is to perform a metallographic dissection examination. After preparing a cross-section containing the weld area, the sample is directly observed under an optical microscope to determine the presence, morphology, length, and location of cracks.
[0056] The second item is non-destructive testing (NDT), used to determine whether heat treatment cracks have occurred in the weld zone after two stages of aging. NDT can be one or more of fluorescence detection, ultrasonic testing, and X-ray testing. Fluorescence detection is based on the capillary penetration principle; a penetrant is applied to the joint surface, allowing it to penetrate surface-opening defects. After cleaning and development, the defect traces are displayed under specific wavelength light, primarily used to detect surface-opening heat treatment cracks. Ultrasonic testing is based on reflection caused by differences in acoustic impedance. When ultrasonic waves propagate inside the joint, they are reflected at the crack interface. The depth and size of the defect are determined by the echo position and amplitude, and it can be used to detect internal weld cracks. X-ray testing images based on the difference in attenuation of radiation between the defect and the substrate, suitable for detecting areas with relatively small thicknesses.
[0057] The third item is the high-temperature tensile property test. For example, the test temperature is 650℃, the tensile rate is 1mm / min, and the test indicators include one or more of the following: tensile strength, yield strength, elongation after fracture, and reduction of area.
[0058] The fourth item is microstructural characterization, which includes at least one of the following: grain size, grain orientation, and the size and distribution of the γ′ phase in the weld zone. Microstructural characterization can be one or more of scanning electron microscopy (SEM), electron backscatter diffraction (ESD), and transmission electron microscopy (TEM). SEM is used to observe the morphology, size, and distribution density of the γ′ phase. Figure 3 The scanning electron microscope (SEM) image of the weld zone of the joint obtained in this application is shown. Electron backscatter diffraction characterization is used to obtain information on grain size and grain orientation, which can be used to determine whether the weld still retains the fine-grained characteristics of post-weld dynamic recrystallization. Transmission electron microscopy characterization is used to observe the interface relationship between the γ′ phase and the matrix at a finer scale. The above testing items are independent of each other and can be implemented individually or in combination according to quality control requirements.
[0059] This application also provides a nickel-based powder superalloy inertial friction welding joint, which is prepared by the method in any of the possible embodiments described above. The joint includes a weld zone and a base metal zone located outside the weld zone. The weld zone refers to the area where plastic deformation, dynamic recrystallization, and γ′ phase dissolution occur during welding, followed by γ′ phase reprecipitation, and its near-weld influence zone. The base metal zone refers to the area in the joint located outside the weld zone, whose microstructure retains the original state of the base metal. The boundary between the two can be determined based on differences in grain size, grain orientation, or γ′ phase morphology. The volume fraction of the γ′ phase in the weld zone is not less than 40%. The grain size in the weld zone is smaller than the grain size in the base metal zone, and the grain orientation in the weld zone is randomly distributed. Random grain orientation means that the grain orientation in the weld zone does not have a distinct preferred orientation, retaining the typical characteristics of dynamically recrystallized grains.
[0060] The joint has a tensile strength of not less than 1400 MPa, a yield strength of not less than 1100 MPa, an elongation after fracture of not less than 15%, and a reduction of area of not less than 9% at 650℃. The joint has a tensile strength of 1464.33 MPa, a yield strength of 1104 MPa, an elongation after fracture of 17.23%, and a reduction of area of 9.13% at 650℃. This nickel-based powder superalloy inertial friction welded joint can be used in components such as FGH99 alloy rotor assemblies for aero-engines.
[0061] The following describes the complete working process of the method for improving the high-temperature tensile properties of FGH99 alloy inertial friction welded joints, using an FGH99 nickel-based powder superalloy workpiece as an example.
[0062] Initially, the incoming parts to be welded are either in a solution-treated and aged state, or in a solution-treated state. If the incoming part is determined to be in a solution-treated state, it undergoes an aging heat treatment at 760℃ for 8 hours to transform it into a solution-treated and aged state. If the incoming part is already in a solution-treated and aged state, it can proceed directly to the next steps. Subsequently, the parts to be welded are machined into hollow cylindrical parts with a wall thickness of 9mm at the welding area. The surfaces to be welded are ground to remove oxide scale and oil. After cleaning with anhydrous ethanol, they are dried. At this point, the parts to be welded are ready for welding, with clean surfaces and consistent dimensions.
[0063] Two workpieces to be welded are clamped on the rotating and sliding ends of the inertial friction welding equipment, respectively, and their concentricity is corrected and adjusted. The equipment is started, and the motor drives the flywheel and the workpieces on the rotating end to accelerate to the set speed of 1000 r / min. When the flywheel reaches the set speed, it disengages from the motor, and continues to rotate, carrying the workpieces on the rotating end. At this time, the workpieces on the sliding end move towards the workpieces on the rotating end under the welding pressure of 10 MPa. The surfaces of the two workpieces come into contact and rub against each other. Under the action of frictional heat, the temperature of the welding interface rises rapidly, and the interface metal undergoes plastic softening. Under the coupled action of axial pressure and torsional shear, the thermoplastic metal at the interface is extruded to form flash, and the oxides at the original welding interface are discharged with the flash, achieving self-cleaning. As the kinetic energy of the flywheel is consumed, the speed gradually decreases until it drops to zero. At this time, the axial pressure is maintained for a period of time to allow the welding interface to complete dynamic recrystallization and diffusion, forming a metallurgical bond. After welding, the joint shortening is 2.1 mm. After welding, a welded joint is obtained.
[0064] Subsequently, the welded joint underwent a two-stage post-weld aging heat treatment. The joint was placed in a heat treatment furnace and heated to the first-stage aging temperature of 800℃ at a rate of 200℃ / hour, holding for 2 hours. After holding, the temperature was lowered to the second-stage aging temperature of 760℃ and held for 2 hours. After the second-stage aging holding, the joint was air-cooled to room temperature. Since both the first and second-stage aging temperatures are lower than the solution temperature of FGH99 (1150℃), this heat treatment process did not cause overall solution treatment or significant deformation. Simultaneously, the two-stage aging caused the dissolved γ′ phase in the weld to re-precipitate, ensuring that the volume fraction of the γ′ phase in the weld zone was not less than 40%, and that the grain size in the weld zone was smaller than that in the base metal zone and exhibited random orientation.
[0065] After heat treatment, the joint can be subjected to metallographic dissection or non-destructive testing as needed to check for heat treatment cracks. A high-temperature tensile test at 650℃ and a tensile rate of 1 mm / min can also be performed to test tensile strength, yield strength, elongation after fracture, and reduction of area. Scanning electron microscopy, electron backscatter diffraction, or transmission electron microscopy can also be used to characterize the weld microstructure. Ultimately, a well-formed nickel-based powder superalloy inertial friction welded joint with no welding defects and a tensile strength of not less than 1400 MPa at 650℃ is obtained.
[0066] A comparative example under specific test conditions is provided below to demonstrate the difference in effectiveness between two-stage aging and single-stage aging at the base material aging temperature. In this comparative example, all conditions were kept consistent except for the post-weld heat treatment regime, which was a single-stage aging process at 760℃ for 4 hours. A high-temperature tensile test was conducted at 650℃ and a tensile rate of 1 mm / min. The test results show that, compared to the comparative example, the tensile strength of the nickel-based powder superalloy inertial friction welded joint of this application increased from 1385.33 MPa to 1464.33 MPa, the yield strength increased from 1074.33 MPa to 1104 MPa, the elongation after fracture increased from 11.7% to 17.23%, and the reduction of area increased from 7.93% to 9.13%. The microstructure observation results correspond to the above performance differences. Figure 3 The following is a scanning electron microscope image of the microstructure of the nickel-based powder superalloy inertial friction welded joint of this application. Figure 4 A comparative scanning electron microscope (SEM) tissue image of the joint is shown. Figure 3 and Figure 4 It can be seen that the volume fraction of fine and dispersed γ′ phase in the weld of the joint treated with the two-stage aging process of this application is significantly higher than that in the joint treated with the single-stage aging process, and the weld grains still maintain a relatively small size.
[0067] The terms "first" and "second," etc., used in this application are used to distinguish different objects, not to describe a specific order, and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. Furthermore, the terms "comprising" and "having," and any variations thereof, are intended to cover non-exclusive inclusion. For example, a process, method, system, product, or apparatus that includes a series of steps or units may include steps or units not listed, but rather steps or units not listed.
[0068] In the description of this application, it should be understood that the terms "height," "thickness," "upper," "lower," "top," "bottom," "inner," and "outer," etc., indicating orientation or positional relationships based on the orientation or positional relationships shown in the accompanying drawings, are used only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this application. In the description of this application, "a plurality of" means two or more, and "at least one" can mean one, two, or more, unless otherwise expressly specified.
[0069] The above description of the disclosed embodiments enables those skilled in the art to make or use this application. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of this application. Specific technical means in some embodiments may be incorporated, in whole or in part, into another embodiment unless explicitly excluded by another embodiment. Therefore, this application is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method of improving high temperature tensile properties of FGH99 alloy inertia friction welded joints, characterized by, Includes the following steps: Step S10: Provide two FGH99 nickel-based powder superalloy parts that have undergone solution treatment and aging treatment; Step S20: Weld the two parts to be welded using inertial friction welding to form a metallurgical bond on the surfaces to be welded, thus obtaining a welded joint. Step S30: Perform a two-stage aging heat treatment on the welded joint after welding. First, heat the welded joint to the first-stage aging temperature and hold it at that temperature. After holding, cool it down to the second-stage aging temperature and hold it at that temperature. After holding, cool it to room temperature. The first-stage aging temperature is 800℃ to 820℃ and the holding time is 1 hour to 4 hours. The second-stage aging temperature is 760℃ to 780℃ and the holding time is 1 hour to 4 hours. Both the first-stage aging temperature and the second-stage aging temperature are lower than the solution temperature of the workpiece to be welded.
2. The method of improving high temperature tensile properties of a FGH99 alloy inertia friction welded joint according to claim 1, wherein, The first-stage aging temperature is 800℃, the second-stage aging temperature is 760℃, and the holding time for both the first-stage and second-stage aging temperatures is 2 hours.
3. The method of improving high temperature tensile properties of a FGH99 alloy inertia friction welded joint according to Claim 1 wherein, In step S30, the heating rate to the first aging temperature is 100℃ / hour to 300℃ / hour; the cooling method after the second aging and heat preservation is air cooling.
4. The method for improving the high-temperature tensile properties of FGH99 alloy inertial friction welded joints as described in claim 1, characterized in that, The volume fraction of the γ′ phase in the FGH99 nickel-based powder superalloy is not less than 40%, the solution temperature of the FGH99 nickel-based powder superalloy is 1150℃, and the aging temperature of the base material is 760℃.
5. The method for improving the high-temperature tensile properties of FGH99 alloy inertial friction welded joints as described in claim 1, characterized in that, Step S10 includes the following steps: Step S11: The workpiece to be welded, which has undergone solution treatment and aging treatment, is machined into a hollow cylindrical part. After machining, the wall thickness of the welding part of the workpiece to be welded is 6mm to 12mm. Step S12: Grind the surface of the workpiece to be welded to remove oxide scale and oil stains; Step S13: Clean the polished workpiece with anhydrous ethanol and then dry it.
6. The method for improving the high-temperature tensile properties of FGH99 alloy inertial friction welded joints as described in claim 1, characterized in that, When the incoming workpiece is in a solution-treated state, the workpiece in the solution-treated state is subjected to an aging heat treatment at 760°C for at least 4 hours in step S10.
7. The method for improving the high-temperature tensile properties of FGH99 alloy inertial friction welded joints as described in claim 1, characterized in that, In the step S20, the process parameters of the inertia friction welding are: the moment of inertia is 20 kg·m 2 to 45 kg·m 2 , the rotating speed is 1000 r / min to 1400 r / min, and the welding pressure is 8 MPa to 12 MPa.
8. The method for improving the high-temperature tensile properties of FGH99 alloy inertial friction welded joints as described in claim 1, characterized in that, In step S20, the shortening of the welded joint after welding is greater than 2 mm and does not exceed 5 mm.
9. The method for improving the high-temperature tensile properties of FGH99 alloy inertial friction welded joints as described in claim 1, characterized in that, Following step S30, at least one of the following tests is performed on the heat-treated welded joint: Perform metallographic dissection examination; Perform non-destructive testing, wherein the non-destructive testing is one or more of fluorescence detection, ultrasonic detection and X-ray detection; High-temperature tensile property test at 650℃, tensile rate of 1mm / min, test indexes include one or more of tensile strength, yield strength, elongation after fracture and reduction of area. Microscopic tissue characterization is performed, wherein the microscopic tissue characterization is one or more of scanning electron microscopy characterization, electron backscatter diffraction characterization, and transmission electron microscopy characterization.
10. A nickel-based powder superalloy inertial friction welding head, characterized in that, The method for improving the high-temperature tensile properties of FGH99 alloy inertial friction welding joint as described in any one of claims 1 to 9 is used; the nickel-based powder high-temperature alloy inertial friction welding joint includes a weld zone and a base material zone located outside the weld zone; The volume fraction of the γ′ phase in the weld zone is not less than 40%; the grain size of the weld zone is smaller than the grain size of the base material zone, and the grain orientation of the weld zone is randomly distributed; the tensile strength of the nickel-based powder superalloy inertial friction welded joint at 650℃ is not less than 1400MPa.