A magnetized roasting method based on the regulation of autogenous carbon dioxide internal circulation in siderite.

By regulating the magnetized roasting of siderite through the internal circulation of self-generated CO2, the problem of unutilized CO2 from the decomposition of siderite was solved, achieving efficient conversion and resource utilization of FeO to Fe3O4, reducing the consumption of exogenous CO2, and improving the magnetic properties and iron recovery rate of the roasting products.

CN123108286APending Publication Date: 2026-11-17NORTHEASTERN UNIV CHINA
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611240955.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-17
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the existing siderite magnetization roasting technology, the CO2 generated by the decomposition of siderite is not effectively recovered and utilized, resulting in the incomplete conversion of FeO into Fe3O4. The proportion of FeO in the roasting product is too high, which affects the subsequent magnetic separation effect. In addition, the cost of additional CO2 gas consumption and atmosphere control is high.

Method used

By collecting, purifying, regulating the temperature, and utilizing the CO2 generated by the thermal decomposition of siderite, a self-generated CO2 internal circulation is formed, which regulates the CO2 partial pressure in the roasting atmosphere, promotes the conversion of FeO to Fe3O4, and reduces dependence on exogenous CO2.

Benefits of technology

This method enables the resource utilization of self-generated CO2, reduces the cost of atmosphere control and external CO2 consumption in the roasting process, improves the stability of the FeO/TFe ratio and magnetic response in the roasted products, enhances the magnetism of the roasted products, and increases the iron recovery rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108286A_ABST
    Figure CN123108286A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of mineral processing technology, specifically relating to a magnetized roasting method based on the internal circulation regulation of self-generated carbon dioxide in siderite. The method includes the following steps: (1) material pretreatment; (2) neutral atmosphere pre-decomposition roasting; (3) self-generated CO2 collection and regulation: the CO2-containing tail gas generated in the pre-decomposition roasting stage is led out through the tail gas outlet, and after passing through gas-solid separation, dust removal, buffering, temperature adjustment and flow regulation in sequence, it is reintroduced into the magnetized roasting reaction zone as self-generated CO2 regulating gas; (4) self-generated CO2 feedback roasting; (5) cooling and subsequent sorting to obtain a magnetized roasting product with magnetite as the main magnetic iron mineral. This invention collects the CO2 released by the thermal decomposition of siderite, transforming it from exhaust gas into an atmosphere regulating component participating in the reaction, thereby reducing dependence on exogenous CO2 and obtaining a roasting product with magnetite as the main magnetic iron mineral.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of mineral processing technology, specifically relating to a magnetization roasting method based on the regulation of self-generated carbon dioxide internal circulation in siderite. Background Technology

[0002] Siderite is an important type of low-grade carbonate iron ore resource, with siderite (FeCO3) as its main iron-bearing mineral. The theoretical iron grade of siderite is approximately 48.2%, lower than common iron minerals such as magnetite and hematite. During natural mineralization, due to the influence of Ca²⁺… + Mg² + Mn² + Equal impurity ion radius and Fe² + Similar to other minerals, iron ions readily enter the siderite lattice via isomorphous processes, replacing some iron ions and further reducing the actual iron grade of natural siderite ore. Furthermore, siderite itself is a weakly magnetic mineral and often occurs in close association with gangue minerals such as quartz, dolomite, calcite, mica, and clay minerals. Directly employing conventional physical beneficiation methods such as gravity separation, magnetic separation, or flotation makes it difficult to obtain ideal iron concentrate grades and iron recovery rates. Therefore, roasting-magnetic separation has become one of the important technical routes for the efficient utilization of siderite resources.

[0003] The basic principle of siderite roasting-magnetic separation is as follows: under certain temperature and atmosphere conditions, weakly magnetic siderite undergoes thermal decomposition and phase transformation to generate strongly magnetic magnetite. Then, weak magnetic separation is used to separate the iron minerals from the gangue minerals. Unlike hematite, limonite, and other iron oxide minerals, siderite crystals contain carbonate ions. During heating, it first undergoes a self-decomposition reaction, generating ferrous oxide and carbon dioxide. The FeO generated during decomposition is an important intermediate phase in the magnetized roasting process of siderite. If the CO2 partial pressure in the roasting system is suitable, FeO can further react with CO2 to form magnetite (Fe3O4): FeCO3 → FeO + CO2, 3FeO + CO2 → Fe3O4 + CO. Therefore, the magnetized roasting of siderite is not simply a process dependent on the addition of reducing or oxidizing gas, but involves multiple coupled reactions simultaneously, including siderite self-decomposition, CO2 release, the formation of the FeO intermediate phase, and the conversion of FeO to Fe3O4. Ideally, the iron in the roasting product should be present in the form of magnetite to enhance the product's magnetism and improve the subsequent weak magnetic separation recovery effect.

[0004] In the prior art, Chinese patent CN108504855B discloses a method for producing iron concentrate using siderite as a reducing agent through suspension magnetization roasting. The core concept of this method is to utilize the CO generated from the decomposition of siderite to reduce weakly magnetic iron minerals such as hematite and limonite to magnetite, followed by two stages of weak magnetic separation to obtain high-grade iron concentrate. Chinese patent CN118957250A discloses a mixed roasting and iron beneficiation process using hematite tailings and siderite. This patent obtains hematite rough concentrate through strong magnetic pre-selection, mixes it with fine siderite powder, adds sodium carbonate and a carbonaceous reducing agent, and performs reduction roasting to magnetize the surface of the mineral particles. After cooling and weak magnetic separation, iron concentrate is obtained. Existing siderite magnetization roasting technologies mostly employ reducing atmosphere, neutral atmosphere, CO2-controlled atmosphere, or a combination of multiple atmospheres for roasting. Among these, neutral atmosphere roasting has advantages such as simple atmosphere composition, high safety, and avoidance of external reducing gas consumption. However, during roasting in neutral atmospheres such as N2 or Ar, the CO2 generated from the decomposition of siderite is usually discharged directly from the roasting system with the carrier gas and is not recovered as an effective atmospheric component. Due to insufficient CO2 partial pressure in the system, the FeO generated by decomposition is difficult to be fully converted into Fe3O4, resulting in a high proportion of FeO in the roasted product and a phase composition that deviates from ideal magnetite.

[0005] Taking roasting in a simple N2 atmosphere as an example, the total iron (TFe) content of the siderite roasting product can reach 65.32%, but the FeO content is as high as 43.31%, with an FeO / TFe ratio of 66.30%, significantly higher than the theoretical FeO / TFe ratio of magnetite Fe3O4. This result indicates that although roasting in a simple neutral atmosphere can promote the decomposition of siderite and increase the iron grade of the product, the insufficient further magnetization of FeO means that the roasted product does not achieve the ideal magnetite composition, which is detrimental to obtaining stable magnetic response and subsequent magnetic separation indicators.

[0006] To promote the conversion of FeO to Fe3O4, existing processes can adjust the atmosphere composition of the roasting system by adding an external CO2 atmosphere. For example, during roasting under a certain concentration of CO2, CO2 can participate in the conversion reaction of FeO to Fe3O4, making the FeO / TFe ratio of the roasted product closer to the theoretical composition of magnetite. However, this type of method usually requires the continuous introduction of external CO2 gas, increasing gas consumption, atmosphere control costs, and the burden of tail gas recycling. At the same time, the external CO2 method does not fully utilize the CO2 released by the thermal decomposition of siderite itself, resulting in insufficient utilization of self-generated CO2 resources. In addition, while directly reducing the concentration of external CO2 is beneficial to reducing gas consumption, it can easily lead to a decline in the indicators of roasted products; while relying solely on self-decomposition under a neutral atmosphere can easily result in an excessively high FeO content. Therefore, the key to the magnetized roasting process of siderite is not only whether to introduce CO2, but also how to establish a suitable and controllable CO2 partial pressure in the roasting system so that the FeO generated by decomposition can selectively convert to Fe3O4, while reducing the consumption of external CO2.

[0007] In existing technologies, the CO2 released from the decomposition of siderite is mostly treated as tail gas and directly discharged, lacking process design for collecting, purifying, temperature-regulating, pressure-stabilizing, and feedback-utilizing this self-generated CO2. There is also a lack of methods to regulate the roasting atmosphere through self-generated CO2 reflux, promote the conversion of FeO to Fe3O4, and bring the FeO / TFe composition of the product closer to the theoretical magnetite composition. Especially in continuous or semi-continuous roasting processes, there is still a lack of effective methods for feeding back the CO2-containing tail gas generated during the pre-decomposition stage of siderite to the magnetized roasting zone to achieve a closed-loop or semi-closed-loop process of "siderite decomposition - self-generated CO2 recovery - atmosphere feedback regulation - FeO magnetite mineralization conversion."

[0008] Therefore, it is necessary to develop a magnetization roasting method based on the internal circulation regulation of siderite's self-generated carbon dioxide. Summary of the Invention

[0009] The purpose of this invention is to provide a magnetized roasting method based on the internal circulation regulation of self-generated carbon dioxide from siderite. By collecting, purifying, temperature-regulating, flow-regulating, and feedback-utilizing the CO2 released from the thermal decomposition of siderite, it transforms the exhaust gas into an atmosphere-regulating component participating in the reaction, forming a controllable CO2 partial pressure within the roasting system, promoting the conversion of FeO to Fe3O4, thereby reducing dependence on exogenous CO2 and obtaining roasting products with magnetite as the main magnetic iron mineral.

[0010] To achieve the above objectives, the present invention provides the following technical solution: A magnetization roasting method based on the regulation of autogenous carbon dioxide internal circulation in siderite includes the following steps: (1) Material pretreatment: Take a siderite sample, crush and screen it to obtain the material to be roasted; (2) Neutral atmosphere pre-decomposition roasting: The material to be roasted is pre-decomposition roasted in a neutral gas atmosphere, so that the siderite undergoes thermal decomposition to generate pre-decomposition products containing FeO and tail gas containing CO2.

[0011] (3) Self-generated CO2 collection and regulation: The CO2-containing tail gas generated in the pre-decomposition roasting stage is led out through the tail gas outlet, and after passing through gas-solid separation, dust removal, buffering, temperature adjustment and flow regulation in sequence, it is reintroduced into the magnetized roasting reaction zone as self-generated CO2 regulation gas. (4) Self-generated CO2 feedback roasting: The self-generated carbon dioxide control gas from step (3) is reintroduced into the magnetized roasting reaction zone and roasting continues under the self-generated CO2 feedback atmosphere; (5) Cooling and subsequent sorting: After roasting, the product is cooled under a nitrogen atmosphere to obtain a magnetized roasted product with magnetite as the main magnetic iron mineral.

[0012] Preferably, a siderite sample is taken, crushed, and sieved into three particle size products: 100 mesh ≤ coarse particle size < 50 mesh; 200 mesh ≤ medium particle size < 100 mesh; and fine particle size < 200 mesh.

[0013] Preferably, the mass ratio of fine particle size to medium particle size to coarse particle size is (1-2):5:(3-4).

[0014] Preferably, the neutral atmosphere pre-decomposition roasting specifically includes the following steps: placing the material to be roasted in a roasting reactor, and pre-decomposing it at 600~850℃ for 3~15 minutes under N2 atmosphere, so that the siderite undergoes thermal decomposition to generate pre-decomposition products containing FeO and tail gas containing CO2.

[0015] Preferably, during the roasting process in step (4), an online CO2 analyzer is used to detect the CO2 volume fraction in the feedback gas, and the CO2 volume fraction in the magnetized roasting zone is maintained at 5%~30% by adjusting the ratio of reflux gas to N2.

[0016] Preferably, in step (4), the roasting continues at 600~850℃ for 10-30 minutes under a self-generated CO2 feedback atmosphere.

[0017] Preferably, at least 50% of the CO2 in the self-generated carbon dioxide control gas in step (4) originates from the self-generated CO2 control gas in step (3).

[0018] Preferably, in step (4), exogenous CO2 can be supplemented during the roasting start-up stage or when the concentration of self-generated CO2 is insufficient.

[0019] Preferably, the neutral gas in step (2) is N2, Ar, or a mixture of the two.

[0020] Preferably, the FeO / Tfe ratio in the obtained roasted product is ≤0.484.

[0021] Preferably, the siderite-containing material in step (1) is at least one of siderite ore, siderite concentrate, mixed iron ore containing siderite, or difficult-to-process iron ore of the siderite type.

[0022] Preferably, the neutral atmosphere pre-decomposition roasting temperature in step (2) is 650~750℃.

[0023] Preferably, the CO2 volume fraction in the calcination system described in step (4) is 10%~25%, more preferably 12%~18%.

[0024] Preferably, the roasting reactor is a fixed bed reactor, a tubular furnace, a vertical furnace, a rotary kiln, a fluidized bed reactor, a suspended roasting reactor, or a multi-stage fluidized bed reactor.

[0025] Preferably, the roasting method includes two or more reaction zones, wherein the first reaction zone is used for the pre-decomposition of siderite in a neutral atmosphere and the generation of CO2-containing tail gas, and the second reaction zone is used for introducing the self-generated carbon dioxide control gas and promoting the conversion of FeO to Fe3O4.

[0026] Existing processes typically roast crushed siderite directly in its entirety in the furnace. This results in a mixture of coarse and fine particles in the roasted material. Coarse particles have slow heat transfer and incomplete decomposition, while fine particles are prone to over-burning or short-circuiting and loss with the airflow, leading to uneven roasting products. This invention blends three specific siderite particles of different sizes in a gradient mass ratio, creating a synergistic reaction micro-ecosystem during roasting, which increases the total iron content in the product. The coarse particles construct airflow channels, improving bed permeability and ensuring uniform CO2 feedback airflow penetration; the medium particles act as the main conversion agent, undertaking the primary magnetization reaction; and the fine particles rapidly decompose to replenish CO2. The synergistic effect of these three particles ensures uniform reaction across all particle sizes, preventing over-burning loss of fine powder and under-burning residue of coarse particles, thus improving total iron recovery.

[0027] This invention further combines the above three particle sizes to reduce the FeO content. Analysis shows that the fine particle size rapidly releases CO2 in the early stages of calcination, providing a timely gas source for FeO magnetization and preventing FeO from remaining in a neutral atmosphere for extended periods and undergoing lattice aging; the medium particle size is fully magnetized in a sufficient CO2 atmosphere; and the coarse particle size ensures uniform gas flow, allowing all FeO particles to participate in the reaction with CO2. This spatiotemporal synergy of the three particle sizes significantly reduces FeO residue in the product.

[0028] Simultaneously, the synergistic effect of particle size and mass ratio in this invention can improve batch consistency in magnetization and roasting methods. Analysis shows that when all particle sizes are fed into the furnace, the particle size distribution of the material varies with the fluctuations in the raw ore, leading to significant batch-to-batch differences in roasting effects. This invention fixes the particle size distribution with three particle sizes and precise ratios, resulting in high stability of specific surface area, heat transfer characteristics, and airflow resistance for each batch of material, a uniform and stable roasting atmosphere, and significantly reduced fluctuations in the FeO / TFe ratio of the product.

[0029] Compared with the prior art, the advantages and beneficial effects of the present invention are as follows: 1. This invention transforms the CO2 generated from the thermal decomposition of siderite into a roasting atmosphere control medium instead of traditional tail gas, thus realizing the resource utilization of self-generated CO2.

[0030] 2. This invention can overcome the problem of excessive FeO content during roasting in a simple N2 atmosphere, and significantly reduce the FeO / TFe ratio of the roasted product compared to roasting in a simple neutral atmosphere, and bring it closer to the FeO / TFe ratio of theoretical magnetite Fe3O4.

[0031] 3. This invention reduces the amount of external CO2 gas used, thereby lowering the cost of atmosphere control and exhaust gas treatment during the roasting process.

[0032] 4. The roasting method of the present invention has high batch stability. Attached Figure Description

[0033] Figure 1 This is a schematic diagram of the magnetization roasting process based on the internal circulation regulation of siderite-generated carbon dioxide.

[0034] Figure 2 This is a schematic diagram of the reaction mechanism of the neutral atmosphere pre-decomposition of siderite and the self-generated CO2 feedback regulation of the conversion of FeO to Fe3O4 in this invention.

[0035] Figure 3 This is a comparison chart of the FeO / TFe ratios of the products obtained in Example 1 and Comparative Examples 1-4.

[0036] Figure 4 The X-ray diffraction patterns are of the products obtained in Example 1 and Comparative Examples 1-4.

[0037] Figure 5 Hysteresis loop diagrams of the products obtained in Example 1 and Comparative Examples 1-4. Detailed Implementation

[0038] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0039] Example 1 like Figure 1-2 As shown, this embodiment provides a magnetization roasting method based on the internal circulation regulation of siderite's self-generated carbon dioxide, including the following steps: (1) Material pretreatment Siderite samples were coarsely crushed to less than 2 mm using a jaw crusher, and then further crushed to less than 0.5 mm using a double-roll crusher. The crushed material was then precisely sieved into three particle sizes using a standard vibrating screen and a double-screen sieve: 100 mesh ≤ coarse particle size < 50 mesh; 200 mesh ≤ medium particle size < 100 mesh; and fine particle size < 200 mesh. The mass ratio of fine particle size to medium particle size to coarse particle size was 2:5:3. Samples of each particle size were weighed and thoroughly mixed in a V-type mixer for 10 minutes to obtain the material to be roasted. (2) Neutral atmosphere pre-decomposition roasting The material to be roasted was placed in a tubular roasting reactor. N2 was introduced into the reactor to purge air, and the temperature was raised to 675°C at a N2 flow rate of 200 mL / min. The sample was pre-decomposed and roasted for 5 min under N2 atmosphere to cause thermal decomposition of siderite, generating pre-decomposition products containing FeO and tail gas containing CO2.

[0040] (3) Self-generated CO2 collection and regulation The CO2-containing tail gas generated during the pre-decomposition roasting stage is led out through the tail gas outlet and first passed through a high-temperature resistant gas-solid separator located at the tail gas outlet to separate solid particles with a diameter greater than 10μm entrained in the tail gas. Then, it is passed through a high-temperature resistant filter with a filtration accuracy of 5μm for secondary dust removal. The CO2-containing tail gas after dust removal is passed into a 1L airtight buffer tank, and the pressure inside the buffer tank is maintained at a slight positive pressure of 2kPa. Subsequently, the tail gas temperature is adjusted to 25℃ by a gas cooler, and the return flow rate is adjusted by a mass flow controller. The return gas is mixed with supplementary N2 to maintain the total flow rate of the mixed gas at 200mL / min. The flow ratio of return gas to N2 is adjusted in real time according to the detection value of the CO2 online analyzer to stabilize the CO2 volume fraction in the mixed gas at 15%. The mixed gas is preheated to 150℃ through a preheating tube and then sent to the inlet end of the reactor at 675℃ as a self-generated CO2 control gas to be reintroduced into the magnetized roasting reaction zone. During the roasting process, an online CO2 analyzer was used to detect the CO2 volume fraction in the feedback gas, and the CO2 volume fraction in the magnetized roasting zone was maintained at 15% by adjusting the ratio of reflux gas to N2.

[0041] (4) Self-generated CO2 feedback roasting The self-generated carbon dioxide control gas from step (3) is reintroduced into the magnetized roasting reaction zone, and roasted at 675°C for 20 min under the self-generated CO2 feedback atmosphere to control the conversion of FeO to Fe3O4.

[0042] (5) Cooling and subsequent sorting After roasting, the product is cooled under a nitrogen atmosphere to obtain a magnetized roasted product with magnetite as the main magnetic iron mineral. Analysis shows that the obtained roasted product contains 62.46% TFe, 30.12% FeO, and an FeO / TFe ratio of 0.482. Depending on the requirements, the roasted product can be ground and subjected to weak magnetic separation to obtain iron concentrate and tailings. Compared to the FeO / TFe ratio of 0.66 obtained from roasting in a simple N2 atmosphere, the FeO / TFe ratio of the product obtained in this embodiment is reduced by 0.183, indicating that the self-generated CO2 feedback can effectively promote the conversion of FeO in the neutral atmosphere pre-decomposition product towards magnetite. Compared to roasting in a continuously added 25% CO2 atmosphere, this embodiment does not require the continuous introduction of high-concentration exogenous CO2, but instead recovers and feeds back the CO2 generated by the decomposition of siderite itself, realizing the resource utilization of self-generated CO2 and the internal control of the roasting atmosphere.

[0043] In this embodiment, the main reactions in the siderite pre-decomposition stage are: FeCO3→FeO+CO2; From this reaction, we know that 1 mol of FeCO3 theoretically produces 1 mol of CO2 upon decomposition. The molar mass of FeCO3 is 115.86 g / mol. Therefore, based on 5 g of siderite-containing material, if the mass fraction of FeCO3 is η, the theoretical CO2 release is: Theoretically, nCO2 = 5 × η / 115.86 × 1000 = 43.15ηmmol; Where η is the mass fraction of FeCO3 in the siderite-containing material. When η=1, that is, based on 5g of pure FeCO3, the theoretical CO2 release is 43.15mmol.

[0044] During the roasting process, an online CO2 analyzer was used to detect the CO2 volume fraction in the reflux gas, and the actual amount of CO2 utilized by the reflux was calculated by combining the total reflux gas flow rate and reflux time.

[0045] The reflux utilization rate Z is calculated using the following formula: Z = Y / theoretical nCO2 × 100%; The above calculations determine the source and utilization ratio of CO2 in the feedback control gas. In this embodiment, the CO2 volume fraction in the magnetized roasting zone is maintained at 10%~18%, and the CO2 from the decomposition of siderite accounts for more than 80% of the total reflux CO2, indicating that the CO2 released from the decomposition of siderite itself can participate in the conversion of FeO to Fe3O4 as an effective atmosphere control medium.

[0046] Example 2 This embodiment provides a magnetization roasting method based on the internal circulation regulation of siderite's self-generated carbon dioxide, including the following steps: (1) Material pretreatment Siderite samples were coarsely crushed to less than 2 mm using a jaw crusher, and then further crushed to less than 0.5 mm using a double-roll crusher. The crushed material was then precisely sieved into three particle sizes using a standard vibrating screen and a double-screen sieve: 100 mesh ≤ coarse particle size < 50 mesh; 200 mesh ≤ medium particle size < 100 mesh; and fine particle size < 200 mesh. The mass ratio of fine particle size to medium particle size to coarse particle size was 1:5:3. Samples of each particle size were weighed and thoroughly mixed in a V-type mixer for 10 minutes to obtain the material to be roasted. (2) Neutral atmosphere pre-decomposition roasting The material to be roasted was placed in a tubular roasting reactor. N2 was introduced into the reactor to purge air, and the temperature was raised to 700°C at a N2 flow rate of 200 mL / min. The sample was pre-decomposed and roasted for 3 min under N2 atmosphere to cause thermal decomposition of siderite, generating pre-decomposition products containing FeO and tail gas containing CO2.

[0047] (3) Self-generated CO2 collection and regulation The CO2-containing tail gas generated during the pre-decomposition roasting stage is led out through the tail gas outlet and first passed through a high-temperature resistant gas-solid separator located at the tail gas outlet to separate solid particles with a diameter greater than 10μm entrained in the tail gas. Then, it is passed through a high-temperature resistant filter with a filtration accuracy of 5μm for secondary dust removal. The CO2-containing tail gas after dust removal is passed into a 1L airtight buffer tank, and the pressure inside the buffer tank is maintained at a slight positive pressure of 2kPa. Subsequently, the tail gas temperature is adjusted to 25℃ by a gas cooler, and the return flow rate is adjusted by a mass flow controller. The return gas is mixed with supplementary N2 to maintain the total flow rate of the mixed gas at 200mL / min. The flow ratio of return gas to N2 is adjusted in real time according to the detection value of the CO2 online analyzer to stabilize the CO2 volume fraction in the mixed gas at 15%. The mixed gas is preheated to 150℃ through a preheating tube and then sent to the inlet end of the reactor at 675℃ as a self-generated CO2 control gas to be reintroduced into the magnetized roasting reaction zone. During the roasting process, an online CO2 analyzer was used to detect the CO2 volume fraction in the feedback gas, and the CO2 volume fraction in the magnetized roasting zone was maintained at 15% by adjusting the ratio of reflux gas to N2.

[0048] (4) Self-generated CO2 feedback roasting The self-generated carbon dioxide control gas from step (3) is reintroduced into the magnetized roasting reaction zone, and roasted at 700°C for 18 min under the self-generated CO2 feedback atmosphere to control the conversion of FeO to Fe3O4.

[0049] (5) Cooling and subsequent sorting After roasting, the product was cooled under a nitrogen atmosphere to obtain a magnetized roasted product with magnetite as the main magnetic iron mineral. The product was tested and found to contain 62.81% TFe, 30.15% FeO, and a FeO / TFe ratio of 0.480.

[0050] Example 3: Locally generated CO2 + small amount of exogenous CO2 compensation The difference between this embodiment and Embodiment 1 is that: the CO2-containing tail gas generated in step (3) of the pre-decomposition roasting stage is led out through the tail gas outlet and successively passes through gas-solid separation, dust removal, buffering, temperature adjustment, and flow regulation before being reintroduced into the magnetized roasting reaction zone as a self-generated CO2 control gas. In the early stage of roasting, since the CO2 released by the decomposition of siderite has not yet reached a stable concentration, a small amount of external CO2 is added to the return gas flow to maintain the CO2 volume fraction in the roasting reaction zone at 15%. As the siderite decomposition reaction proceeds, the self-generated CO2 concentration increases, and the amount of external CO2 added is gradually reduced, with self-generated CO2 serving as the main control gas.

[0051] This implementation method is suitable for the start-up stage of roasting or continuous operation process with large fluctuations in the self-generated CO2 concentration, and can be used to maintain the stability of CO2 concentration in the magnetized roasting zone.

[0052] Example 4: Dual Reaction Zone The difference between this embodiment and Embodiment 1 is that the roasting apparatus is configured as a first reaction zone and a second reaction zone. The first reaction zone is used for the pre-decomposition of siderite under N2 atmosphere to generate FeO and CO2-containing tail gas; the second reaction zone is used to introduce the CO2-containing tail gas generated in the first reaction zone and promote the conversion of FeO to Fe3O4.

[0053] Specifically, the siderite-containing material is fed into the first reaction zone and heated to 675°C under a nitrogen atmosphere, causing the siderite to thermally decompose and release CO2. The CO2-containing tail gas generated in the first reaction zone is then separated into gas and solid components and purged of dust before being introduced into the second reaction zone. Simultaneously, the pre-decomposed solid material from the first reaction zone is also fed into the second reaction zone. In the second reaction zone, the return gas flow rate is adjusted to maintain the CO2 volume fraction at 15%, thereby promoting the conversion of the pre-decomposed FeO to Fe3O4.

[0054] This implementation method is applicable to multi-stage fluidized beds, suspension roasting furnaces, vertical shaft furnaces or other continuous roasting equipment, and can be implemented in continuous or semi-continuous equipment.

[0055] Example 5 The difference between this embodiment and Embodiment 1 is that: a siderite sample is taken, crushed, and the material to be roasted is obtained. The particle size of the material to be roasted is less than 0.5 mm, of which 65% is less than 0.074 mm.

[0056] Example 6 The difference between this embodiment and Embodiment 1 is as follows: Siderite samples are first coarsely crushed to less than 2mm using a jaw crusher, and then further crushed to less than 0.5mm using a double-roll crusher. The crushed material is then precisely sieved into two narrow particle sizes using a standard vibrating screen and a double-roll screen: 100 mesh ≤ coarse particle size < 50 mesh; fine particle size < 200 mesh. The mass ratio of fine particle size to coarse particle size is 2:3. Samples of each particle size are weighed and thoroughly mixed in a V-type mixer for 10 minutes to obtain the material to be roasted.

[0057] Example 7 The difference between this embodiment and Embodiment 1 is as follows: Siderite samples are first coarsely crushed to less than 2mm using a jaw crusher, and then further crushed to less than 0.5mm using a double-roll crusher. The crushed material is then precisely sieved into three particle sizes using a standard vibrating screen and a double-roll screen: 100 mesh ≤ coarse particle size < 50 mesh; 200 mesh ≤ medium particle size < 100 mesh; and fine particle size < 200 mesh. The mass ratio of fine particle size to medium particle size to coarse particle size is 1:1:1. Samples of each particle size are weighed and thoroughly mixed in a V-type mixer for 10 minutes to obtain the material to be roasted.

[0058] Example 8 The difference between this embodiment and Embodiment 1 is as follows: Siderite samples are first coarsely crushed to less than 2mm using a jaw crusher, and then further crushed to less than 0.5mm using a double-roll crusher. The crushed material is then precisely sieved into three particle sizes using a standard vibrating screen and a double-roll screen: 100 mesh ≤ coarse particle size < 50 mesh; 200 mesh ≤ medium particle size < 100 mesh; and fine particle size < 200 mesh. The mass ratio of fine particle size to medium particle size to coarse particle size is 3:4:2. Samples of each particle size are weighed and thoroughly mixed in a V-type mixer for 10 minutes to obtain the material to be roasted.

[0059] Example 9 The difference between this embodiment and Embodiment 1 is as follows: Siderite samples are first coarsely crushed to less than 2mm using a jaw crusher, and then further crushed to less than 0.5mm using a double-roll crusher. The crushed material is then precisely sieved into three particle sizes using a standard vibrating screen and a double-roll screen: 80 mesh ≤ coarse particle size < 35 mesh; 100 mesh ≤ medium particle size < 80 mesh; and fine particle size < 100 mesh. The mass ratio of fine particle size to medium particle size to coarse particle size is 2:5:3. Samples of each particle size are weighed and thoroughly mixed in a V-type mixer for 10 minutes to obtain the material to be roasted.

[0060] Comparative Example 1: Calcination in a simple N2 atmosphere The difference between this comparative example and Example 1 is that in step (3), the pre-decomposition product containing FeO is roasted in N2 atmosphere. During the roasting process, the CO2 released by the decomposition of siderite is not recovered or fed back, and the tail gas is directly discharged from the system.

[0061] After roasting, the obtained roasted product was tested and found to contain 65.32% TFe and 43.31% FeO, with an FeO / TFe ratio of 0.663. This ratio is significantly higher than the theoretical FeO / TFe ratio of 42.88% for magnetite Fe3O4, indicating that under pure N2 atmosphere roasting conditions, the FeO generated from the decomposition of siderite was not fully converted into Fe3O4, resulting in an excessively high FeO proportion in the product and insufficient magnetite mineralization control.

[0062] Comparative Example 2: Calcination under an atmosphere of 25% CO2 The difference between this comparative example and Example 1 is that in step (3), the pre-decomposition product containing FeO is directly roasted in a mixed atmosphere of 25% CO2 and 75% N2 for 20 minutes at 675°C.

[0063] After roasting, the obtained roasted product was found to have a TFe content of 63.15% and an FeO content of 27.44%, with an FeO / TFe ratio of 0.435, which is close to the theoretical FeO / TFe ratio of magnetite Fe3O4. This result indicates that a suitable CO2 partial pressure can promote the conversion of FeO to Fe3O4, but this method requires the addition of a relatively high concentration of CO2 gas.

[0064] Comparative Example 3: Calcination under an atmosphere of 15% CO2 Instead of performing the N2 pre-decomposition tail gas feedback control in step (2), the material to be roasted in step (1) is directly roasted in a mixed atmosphere of 15% CO2 and 85% N2 for 20 minutes at 675°C.

[0065] After roasting, the obtained roasted product was tested and found to have a TFe content of 61.17% and an FeO content of 27.23%. The FeO / TFe ratio was 0.445. Compared with roasting under an external 25% CO2 atmosphere, directly reducing the CO2 concentration led to a decrease in the TFe content of the roasted product, indicating that direct roasting under a low CO2 atmosphere is difficult to fully achieve the product indicators of roasting under a high CO2 atmosphere.

[0066] Comparative Example 4: Pre-roasted with N2 followed by roasting in an atmosphere of 15% CO2 The difference between this comparative example and Example 1 is that the material to be roasted was first pre-roasted at 675°C for 5 minutes in a N2 atmosphere, and then roasted at 675°C for 20 minutes in a mixed atmosphere of 15% CO2 and 85% N2.

[0067] After roasting, the obtained roasted product was found to have a TFe content of 62.82% and an FeO content of 27.34%. The FeO / TFe ratio was 0.435. Compared with direct 15% CO2 roasting without pre-roasting, N2 pre-roasting followed by 15% CO2 roasting increased the TFe content from 61.17% to 62.82%, indicating that the staged atmosphere route of neutral pre-decomposition-CO2 control helps improve the quality of roasted products under low CO2 conditions. This comparative example used exogenous CO2 as the control gas, while the example involved recovering and reusing the CO2 released from the decomposition of siderite itself to reduce dependence on exogenous CO2.

[0068] Performance testing The same batch of siderite samples were subjected to three magnetization roastings according to the methods of the examples and comparative examples. The roasting products were tested: TFe content: GB / T6730.73-2024 "Determination of Total Iron Content in Iron Ore by EDTA Photometric Titration"; FeO content: GB / T6730.8-1986 "Chemical Analysis Methods for Iron Ore: Determination of Ferrous Content by Potassium Dichromate Titration Method"; FeO / TFe = FeO content ÷ TFe content. The results are shown in Table 1-2.

[0069] Table 1. Test results of the first roasting product

[0070] Table 2. FeO / TFe results after three calcinations

[0071] Through Table 1 and Figure 3-5 It can be seen that Examples 1-2, employing a self-generated CO2 feedback roasting process, exhibited a significantly lower FeO / TFe ratio than Comparative Example 1, which used a simple N2 atmosphere roasting. This indicates that the present invention effectively increases the CO2 partial pressure in the roasting system by recovering and utilizing the CO2 released from the decomposition of siderite, promoting the magnetization conversion of FeO to Fe3O4, and overcoming the technical defect of excessive FeO residue in neutral atmosphere roasting. Furthermore, compared to Comparative Examples 2-4, the present invention fully utilizes the CO2 generated from the decomposition of siderite as an atmosphere control medium, achieving resource utilization of self-generated CO2 and reducing the consumption of external CO2 gas and the burden of tail gas treatment.

[0072] Table 2 shows that the FeO / TFe ratio fluctuation range obtained from the three parallel calcination experiments in Example 1 was small, and the batch-to-batch reproducibility was significantly better than that of Examples 5-9. This indicates that the process conditions adopted in this invention have good stability and can effectively resist the influence of small fluctuations in raw materials or operating conditions on the phase composition of the calcination product. In contrast, Examples 5-9 did not use optimized particle size distribution, and the calcination system was more sensitive to changes in raw materials, resulting in a significant increase in the batch-to-batch fluctuation of the FeO / TFe ratio. The above results show that this invention can not only achieve excellent FeO to Fe3O4 conversion in a single calcination, but also has good process repeatability and operational stability in actual industrial production, which is beneficial to ensuring the consistency of product indicators in continuous production.

[0073] The above description represents the preferred embodiments of the present invention. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A magnetized roasting method based on the internal circulation regulation of self-generated carbon dioxide in siderite, characterized in that, Includes the following steps: (1) Material pretreatment: Take a siderite sample, crush and screen it to obtain the material to be roasted; (2) Neutral atmosphere pre-decomposition roasting: The material to be roasted is pre-decomposition roasted in a neutral gas atmosphere to cause siderite to undergo thermal decomposition, generating pre-decomposition products containing FeO and tail gas containing CO2. (3) Self-generated CO2 collection and regulation: The CO2-containing tail gas generated in the pre-decomposition roasting stage is led out through the tail gas outlet, and after passing through gas-solid separation, dust removal, buffering, temperature adjustment and flow regulation in sequence, it is reintroduced into the magnetized roasting reaction zone as self-generated CO2 regulation gas. (4) Self-generated CO2 feedback roasting: The self-generated carbon dioxide control gas from step (3) is reintroduced into the magnetized roasting reaction zone and roasting continues under the self-generated CO2 feedback atmosphere; (5) Cooling and subsequent sorting: After roasting, the product is cooled under a nitrogen atmosphere to obtain a magnetized roasted product with magnetite as the main magnetic iron mineral.

2. The magnetization roasting method based on the internal circulation regulation of siderite-generated carbon dioxide as described in claim 1, characterized in that, Siderite samples were taken, crushed, and sieved into three particle sizes: 100 mesh ≤ coarse particle size < 50 mesh; 200 mesh ≤ medium particle size < 100 mesh; and fine particle size < 200 mesh.

3. The magnetization roasting method based on the internal circulation regulation of siderite-generated carbon dioxide as described in claim 2, characterized in that, The mass ratio of fine particle size to medium particle size to coarse particle size is (1-2):5:(3-4).

4. The magnetization roasting method based on the internal circulation regulation of siderite-generated carbon dioxide as described in claim 1, characterized in that, The neutral atmosphere pre-decomposition roasting specifically includes the following steps: placing the material to be roasted in a roasting reactor, and pre-decomposing it at 600~850℃ for 3~15 minutes under N2 atmosphere, so that the siderite undergoes thermal decomposition, generating pre-decomposition products containing FeO and tail gas containing CO2.

5. The magnetization roasting method based on the internal circulation regulation of siderite-generated carbon dioxide as described in claim 1, characterized in that, In step (4) during the roasting process, the CO2 volume fraction in the feedback gas is detected by an online CO2 analyzer, and the CO2 volume fraction in the magnetized roasting zone is maintained at 5%~30% by adjusting the ratio of reflux gas to N2.

6. The magnetization roasting method based on the internal circulation regulation of siderite-generated carbon dioxide as described in claim 1, characterized in that, Step (4) Continue roasting at 600~850℃ for 10-30 minutes under a self-generated CO2 feedback atmosphere.

7. The magnetization roasting method based on the internal circulation regulation of siderite-generated carbon dioxide as described in claim 1, characterized in that, At least 50% of the CO2 in the self-generated carbon dioxide control gas in step (4) comes from the self-generated CO2 control gas in step (3).

8. The magnetization roasting method based on the internal circulation regulation of siderite-generated carbon dioxide as described in claim 1, characterized in that, In step (4), external CO2 is added during the roasting start-up stage or when the concentration of self-generated CO2 is insufficient.

9. The magnetization roasting method based on the internal circulation regulation of siderite-generated carbon dioxide as described in claim 1, characterized in that, The neutral gas mentioned in step (2) is N2, Ar, or a mixture of the two.

10. The magnetization roasting method based on the internal circulation regulation of siderite-generated carbon dioxide as described in claim 1, characterized in that, The FeO / TFe ratio in the obtained roasted product is ≤0.484.

Citation Information

Patent Citations

  • A method for producing iron concentrate by suspension magnetization roasting using siderite as a reducing agent.

    CN108504855B

  • Process for separating iron by mixing and roasting hematite tailings and siderite

    CN118957250A