A method for recovering rare earth metals from water
By using photocatalytic reaction and nitric acid immersion, the problems of low rare earth metal recovery efficiency and poor environmental compatibility in existing technologies have been solved, achieving efficient and environmentally friendly rare earth metal recovery. It has good pH adaptability and resistance to anion and cation interference, and is suitable for continuous treatment of rare earth-containing wastewater.
Patent Information
- Application Number
- CN202610311874.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-03-13
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies are inefficient and have poor environmental compatibility when recovering rare earth metals from water, especially when the concentration of rare earth metals is low. They also rely on chemical reagents and consume a lot of energy.
A photocatalytic reaction is carried out using a photoelectric device consisting of a photoanode and a cathode. Photogenerated electron-hole pairs drive electrons to migrate to the cathode, and rare earth ions adsorbed on the cathode surface are recovered by nitric acid immersion, thus achieving efficient recovery of rare earth metals.
It achieves efficient and environmentally friendly rare earth metal recovery, has good pH adaptability and resistance to anion and cation interference, and is suitable for continuous treatment of rare earth-containing wastewater while generating electricity simultaneously.
Smart Images

Figure CN123108296A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of rare earth wastewater resource utilization technology, specifically relating to a method for recovering rare earth metals from water. Background Technology
[0002] The mining and processing of rare earth elements generate high-concentration rare earth wastewater, which not only leads to the loss of precious resources but also poses a risk of environmental pollution. Therefore, the development of efficient and environmentally friendly rare earth recycling technologies is urgently needed.
[0003] Currently, the main technologies for recovering rare earth metals from aqueous solutions include adsorption, precipitation, solvent extraction, ion exchange, and electrochemical methods. However, most of these methods rely on chemical reagents and / or have high energy consumption, resulting in high costs and significant environmental impacts, especially when the concentration of rare earth metals is low. Summary of the Invention
[0004] The purpose of this invention is to provide a method for recovering rare earth metals from water. The method provided by this invention enables efficient and environmentally friendly recovery of rare earth metals.
[0005] To achieve the objectives of this invention, the following technical solutions are provided: A method for recovering rare earth metals from water includes the following steps: The photoanode and cathode, connected by an external circuit, are placed in a mixed solution of electrolyte solution and rare earth metal solution. The photoanode is then irradiated with a light source to carry out a photocatalytic reaction. The cathode after the photocatalytic reaction is immersed in nitric acid to recover rare earth ions adsorbed on the cathode surface.
[0006] Preferably, the photoanode comprises a conductive glass-based semiconductor thin film and a photovoltaic cell.
[0007] Preferably, the conductive glass-based semiconductor thin film is a titanium dioxide thin film; the photovoltaic cell includes a silicon solar cell.
[0008] Preferably, the cathode includes an electrode substrate and an organometallic framework material loaded on the surface of the electrode substrate.
[0009] Preferably, the electrode substrate comprises carbon felt; the organometallic framework material is ZIF-67; and the loading of the ZIF-67 material is 7~10 mg·cm³. -2 .
[0010] Preferably, the electrolyte solution includes a sodium sulfate solution, and the concentration of the electrolyte solution in the mixed solution is 0.005~0.5M.
[0011] Preferably, the rare earth metal solution is a wastewater solution containing rare earth ions, wherein the rare earth ions include Eu. 3+ Er 3 + Tm 3+ and Y 3+ One or more of the following: the concentration of rare earth ions in the rare earth metal solution is 5~15 mg / L; the volume ratio of electrolyte solution to rare earth metal solution in the mixed solution is 1~2:1~2.
[0012] Preferably, the light source includes simulated sunlight, xenon lamp light source, ultraviolet light source, LED light source, or natural light; the luminous intensity of the light source is 50~150mW·cm. -2 .
[0013] Preferably, the photocatalytic reaction takes 1 to 30 minutes.
[0014] Preferably, the concentration of the nitric acid is 0.1~0.2M; and the soaking time is 20~30min.
[0015] This invention provides a method for recovering rare earth metals from water, comprising the following steps: placing a photoanode and a cathode connected by an external circuit in a mixed solution of an electrolyte solution and a rare earth metal solution; irradiating the photoanode with a light source to perform a photocatalytic reaction; and immersing the cathode after the photocatalytic reaction with nitric acid to recover rare earth ions adsorbed on the cathode surface. In this method, when the photoanode is irradiated by the light source, photogenerated electron-hole pairs are generated. Driven by an internal electric field, the photogenerated electrons migrate to the cathode via an external circuit, generating electricity. Furthermore, the migration of photogenerated electrons to the cathode helps to excite active sites on the cathode, thereby promoting the coordination and fixation of rare earth ions between the cathode and rare earth ions, enhancing the adsorption and recovery of rare earth ions by the cathode under catalysis. This method relies on light energy to recover rare earth metals from water, simultaneously generating electricity during the recovery process. It exhibits good pH adaptability, resistance to anion and cation interference, and system stability, making it suitable for continuous treatment of rare earth-containing wastewater. The method for recovering rare earth metals from water provided by this invention effectively solves the problems of low efficiency and poor environmental compatibility of existing recovery technologies, achieving efficient and environmentally friendly rare earth resource recovery. Compared with existing technologies, the present invention shows significant advantages in rare earth recovery efficiency, energy consumption control and environmental compatibility. Attached Figure Description
[0016] Figure 1 This is a schematic diagram of the apparatus for recovering rare earth metals from water according to the present invention; Figure 2 Example 1 of the present invention is in the presence of Eu 3+ Er 3+ Tm 3+and Y 3+ A graph showing the rare earth recovery efficiency in a simulated rare earth solution. Figure 3 To recover Eu from the cathode ZIF-67 / CF composite material in Example 1 of this invention 3+ Er 3+ Tm 3+ and Y 3+ The subsequent SEM image; Figure 4 To recover Eu from the cathode ZIF-67 / CF composite material in Example 1 of this invention 3+ Er 3+ Tm 3+ and Y 3+ XPS spectra afterward; Figure 5 The cathode ZIF-67 / CF composite material in Example 1 of this invention was used to simulate Eu in rare earth solutions under different pH conditions. 3+ Er 3+ Tm 3+ and Y 3+ Characterization diagram of removal rate and apparent rate constant; Figure 6 The cathode ZIF-67 / CF composite material in Example 1 of this invention is used to simulate rare earth solutions containing Eu under different electrolyte concentrations. 3+ Er 3+ Tm 3+ and Y 3+ Characterization diagram of removal rate and apparent rate constant; Figure 7 The cathode ZIF-67 / CF composite material in Example 1 of this invention is used to simulate Eu in rare earth solutions under different coexistence conditions of anions and cations. 3+ Er 3+ Tm 3+ and Y 3+ Characterization diagram of removal rate and apparent rate constant; Figure 8 This invention, in Example 1, demonstrates the effect of the ZIF-67 / CF composite cathode material on Eu in simulated rare earth solutions under different concentrations of organic matter. 3+ Er 3+ Tm 3+ and Y 3+ Characterization diagram of removal rate and apparent rate constant; Figure 9 The cathode ZIF-67 / CF composite material in Example 1 of this invention is used to simulate Eu in rare earth solution. 3+ Er 3+ Tm 3+ and Y 3+ The characterization diagram of the repeated recycling performance. Detailed Implementation
[0017] This invention provides a method for recovering rare earth metals from water, comprising the following steps: The photoanode and cathode, connected by an external circuit, are placed in a mixed solution of electrolyte solution and rare earth metal solution. The photoanode is then irradiated with a light source to carry out a photocatalytic reaction. The cathode after the photocatalytic reaction is immersed in nitric acid to recover rare earth ions adsorbed on the cathode surface.
[0018] In this invention, unless otherwise specified, all raw materials used in the preparation are preferably commercially available products well known to those skilled in the art.
[0019] This invention places a photoanode and cathode, connected by an external circuit, in a mixed solution of electrolyte and rare earth metal solutions. A light source is used to irradiate the photoanode to perform a photocatalytic reaction. In one embodiment, the photoanode comprises a conductive glass-based semiconductor film and a photovoltaic cell; the conductive glass-based semiconductor film is a titanium dioxide film, which possesses photoresponsive characteristics; the titanium dioxide film can have dimensions of 2cm × 5cm and a volume resistivity of 7Ω·cm. -1 The photovoltaic cell includes a silicon solar cell, with four silicon solar cells connected in series, and the functional area size is 2×4cm. 2 The photoanode is composed of a conductive glass-based semiconductor thin film and a photovoltaic cell laminate bonded together. The present invention does not have any special limitations on the bonding method or the reagents used, and any method known to those skilled in the art can be used.
[0020] This invention uses a titanium dioxide thin film with photoresponsive properties and a photovoltaic cell as a photoanode, so that the photoanode generates and transfers electrons under illumination by relying on light energy, thereby realizing the recovery of rare earth metals in water.
[0021] As one embodiment of the present invention, the method for preparing the conductive glass-based semiconductor thin film includes the following steps: A mixed solution of tributyltin and ethanol was coated onto the surface of FTO conductive glass and subjected to a first annealing treatment to obtain an FTO conductive glass substrate with a titanium dioxide seed layer. The FTO conductive glass substrate with the titanium dioxide seed layer is placed face down in a hydrothermal reaction solution to carry out a hydrothermal reaction, thereby obtaining an intermediate film. The intermediate film was subjected to a second annealing treatment to obtain a titanium dioxide film.
[0022] This invention involves coating a mixed solution of tributyltin and ethanol onto the surface of FTO conductive glass and then performing a first annealing treatment to obtain an FTO conductive glass substrate coated with a titanium dioxide seed layer. In one embodiment of this invention, the volume ratio of tributyltin to ethanol can be 1:90~110, specifically 1:100; the coating is spin-coating, the spin-coating time can be 15~25s, specifically 20s, and the rotation speed can be 2000rpm; the temperature of the first annealing treatment can be 400~500℃, specifically 450℃; the holding time can be 1~3h, specifically 2h; and the heating rate from room temperature to the temperature of the first annealing treatment can be 1~3℃·min. -1 Specifically, it can be 2℃·min -1 .
[0023] After obtaining an FTO conductive glass substrate coated with a titanium dioxide seed layer, the present invention places the FTO conductive glass substrate coated with the titanium dioxide seed layer downwards in a hydrothermal reaction solution for hydrothermal reaction to obtain an intermediate film. In one embodiment of the present invention, the hydrothermal reaction solution is a mixture of tributyltin, hydrochloric acid, and deionized water, wherein the mass concentration of the hydrochloric acid is 37%; the volume ratio of the tributyltin, hydrochloric acid, and deionized water can be 0.7~0.8:25~35:25~35, specifically 0.72:30:30; the hydrothermal reaction solution is a colorless and transparent solution; the hydrothermal reaction is carried out in a sealed stainless steel reactor lined with polytetrafluoroethylene, the temperature of the hydrothermal reaction can be 160~180℃, specifically 170℃, and the time can be 5~7 hours, specifically 6 hours.
[0024] After obtaining the intermediate film, the present invention performs a second annealing treatment on the intermediate film to obtain a titanium dioxide film. In one embodiment of the present invention, the second annealing treatment is performed in a muffle furnace, and the temperature of the second annealing treatment can be 400~600℃, specifically 500℃; the holding time can be 1~3h, specifically 2h; and the heating rate to the temperature of the second annealing treatment can be 1~3℃·min. -1 Specifically, it can be 2℃·min -1 .
[0025] In one embodiment of the present invention, the cathode includes an electrode substrate and an organometallic framework material loaded on the surface of the electrode substrate; the electrode substrate includes a carbon felt; the organometallic framework material is ZIF-67 material; and the loading amount of ZIF-67 material is 7~10 mg·cm³. -2 .
[0026] In one embodiment of the present invention, the cathode is a ZIF-67 / carbon felt (ZIF-67 / CF) composite material, and the preparation method of the ZIF-67 / CF composite material includes the following steps: The electrode substrate was immersed in an aqueous solution of cobalt nitrate hexahydrate, and an aqueous solution of 2-methylimidazole was added to carry out the reaction, thus obtaining the ZIF-67 / CF composite material.
[0027] In one embodiment of the present invention, the concentration of the cobalt nitrate hexahydrate aqueous solution can be 0.01~0.06 mmol / mL, specifically 0.04 mmol / mL; the concentration of the 2-methylimidazole aqueous solution can be 0.1~0.6 mmol / mL, specifically 0.4 mmol / mL; the volume ratio of the cobalt nitrate hexahydrate aqueous solution to the 2-methylimidazole aqueous solution can be 1~2:1~2, specifically 1:1; the reaction is carried out under static conditions, the reaction temperature is room temperature, and the reaction time can be 3~5 h, specifically 4 h; the electrode substrate is immersed in the cobalt nitrate hexahydrate aqueous solution for 2 min. In another embodiment of the present invention, before immersing the electrode substrate in the cobalt nitrate hexahydrate aqueous solution, it further includes cleaning and drying. The cleaning is carried out sequentially with ethanol and deionized water under ultrasonic conditions. The present invention does not have specific limitations on the ultrasonication and drying. After obtaining the ZIF-67 / CF composite material, the present invention cleans and dries the ZIF-67 / CF composite material. The cleaning uses deionized water, and the drying temperature is 60°C for 8~20 h. In the reaction process described in this invention, ZIF-67 is grown on the surface of carbon felt to ultimately obtain ZIF-67 / CF composite material.
[0028] The cathode ZIF-67 / CF composite material provided by this invention has a catalytic effect. The electrons transferred by the photoanode can activate the active sites, promote the coordination and fixation of rare earth ions between the ZIF-67 / CF composite material and rare earth ions, and enhance the adsorption and recovery of rare earth ions by the cathode ZIF-67 / CF composite material.
[0029] In one embodiment of the present invention, the electrolyte solution includes a sodium sulfate solution, and the concentration of the electrolyte solution in the mixed solution can be 0.005~0.5M, specifically 0.005M, 0.01M, 0.02M, 0.05M, 0.1M or 0.5M.
[0030] In one embodiment of the present invention, the rare earth metal solution is a wastewater solution containing rare earth ions, and the metal ions and organic matter contained in the rare earth metal solution are common components in various rare earth ore extraction waste liquids; specifically, the rare earth ions include Eu. 3+ Er 3+ Tm 3+ and Y3+ One or more of the following; the concentration of rare earth ions in the rare earth metal solution can be independently 5~15 mg / L, specifically 5 mg / L, 6 mg / L, 7 mg / L, 8 mg / L, 9 mg / L, 10 mg / L, 11 mg / L, 12 mg / L, 13 mg / L, 14 mg / L, 15 mg / L.
[0031] In one embodiment of the present invention, the rare earth metal solution further contains interfering substances, including K. + Ca 2+ Mn 2+ Al 2+ Fe 2+ Mg 2+ NH4 + Pb 2+ NO3 - Cl - One or more of EDTA, citric acid, and oxalic acid; the device of the present invention does not affect the removal rate of rare earth ions when performing photocatalytic reactions in rare earth metal solutions containing the aforementioned interfering substances.
[0032] In one embodiment of the present invention, the volume ratio of electrolyte solution to rare earth metal solution in the mixed solution is 1~2:1~2, specifically 1:1; the pH range of the mixed solution is 3~10, specifically 3, 4, 5, 5.4, 6, 7, 8, 9, 10.
[0033] The electrolyte solution serves as a reaction medium and charge transport channel, transferring electrons and forming an internal conductive pathway. The rare earth metal solution is the target for treatment, providing rare earth metal ions. However, the conductivity of the rare earth metal solution is low. Therefore, this invention balances the conductivity and rare earth ion strength of the mixed solution by controlling the volume ratio of the electrolyte solution to the rare earth metal solution, ensuring both the electron transport efficiency and rare earth ion removal efficiency of the photocatalytic reaction. This invention limits the pH value of the mixed solution to 3-10 to ensure excellent removal efficiency for different rare earth elements in the rare earth metal solution.
[0034] In one embodiment of the present invention, the light source includes simulated sunlight, xenon lamp light source, ultraviolet light source, LED light source, or natural light; the light intensity of the light source can be 50~150mW·cm. -2 Specifically, it can be 100mW·cm -2 .
[0035] When the light source of the present invention irradiates the photoanode, it excites the generation of photogenerated electron-hole pairs. The photogenerated electrons migrate to the cathode through the external circuit under the drive of the internal electric field, thereby realizing external power generation.
[0036] In one embodiment of the present invention, the photocatalytic reaction time can be 1-30 min, or more specifically 1-15 min; the photocatalytic reaction temperature is room temperature.
[0037] Figure 1 This is a schematic diagram of the apparatus for recovering rare earth metals from water according to the present invention. The present invention is based on... Figure 1 A device for recovering rare earth metals from water is set up. The photoanode and cathode, made of ZIF-67 / CF composite material, are connected via an external circuit and placed in wastewater containing rare earth elements. When the photoanode is illuminated by a light source, it generates photogenerated electron-hole pairs. The electrons, driven by internal forces, migrate through the external circuit to the cathode to generate electricity. Simultaneously, the cathode catalyzes and adsorbs and recovers rare earth metals from the water. This system can recover rare earth metals from water under purely light-driven conditions, while simultaneously generating electricity. It is adaptable to different pH environments, performs well under varying anion and cation coexistence conditions, and exhibits good stability, allowing for continuous treatment of rare earth wastewater. It possesses significant application potential and value.
[0038] This invention limits the temperature and time of the photocatalytic reaction, allowing the reaction to proceed under mild conditions, thus ensuring the stability of the device for recovering rare earth metals from water, suppressing hydrogen evolution side reactions, and improving the recovery rate of rare earth metals.
[0039] Following the photocatalytic reaction, this invention employs nitric acid to immerse the cathode after the photocatalytic reaction, recovering the rare earth ions adsorbed on the cathode surface. In one embodiment of this invention, the concentration of the nitric acid can be 0.1~0.2M, specifically 0.1M; the immersion time can be 20~30 min, typically 30 min. By limiting the type, concentration, and immersion time of the recovery solution, this invention enables the elution and recovery of rare earth ions adsorbed on the cathode surface, thereby improving the recovery rate of rare earth ions.
[0040] To further illustrate the present invention, the technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments thereof. Obviously, the described embodiments are merely some embodiments of the present invention, and not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0041] Example 1 0.1 mL of tributyltin was mixed with 10 mL of ethanol to obtain a mixed solution. The mixed solution was spin-coated onto the surface of FTO conductive glass at 2000 rpm for 20 s, and the temperature was increased at a rate of 2 °C / min. -1The temperature was raised from room temperature to 450℃, and annealed in air at 450℃ for 2 hours to obtain a TiO2 seed layer; 30 mL of deionized water, 30 mL of 37% hydrochloric acid, and 0.72 mL of tributyltin were mixed and stirred at 500 r·min. -1 The mixture was stirred continuously at a constant stirring rate until the solution became colorless and transparent, yielding a hydrothermal reaction solution. This hydrothermal reaction solution was transferred to a 100 mL stainless steel reactor lined with polytetrafluoroethylene (PTFE), and an FTO substrate coated with a TiO2 seed layer (seed layer facing down) was placed inside. The reactor was sealed and reacted at 170 °C for 6 hours. The resulting film was then placed in a muffle furnace and heated at a rate of 2 °C / min. -1 The TiO2 film is obtained by heating from room temperature to 500°C and annealing in air at 500°C for 2 hours. The TiO2 film is then laminated with a photovoltaic cell to obtain a photoanode.
[0042] The carbon felt was ultrasonically cleaned sequentially with ethanol and deionized water, and then dried for later use. 2 mmol of Co(NO3)2·6H2O was dissolved in 50 mL of deionized water and stirred until homogeneous to obtain solution A. 20 mmol of 2-methylimidazole was dissolved in 50 mL of deionized water and stirred until homogeneous to obtain solution B. The dried carbon felt was immersed in solution A for 2 min, and then solution B was poured into the resulting system. The system was allowed to stand at room temperature for 4 h, during which ZIF-67 grew on the surface of the carbon felt. After the reaction, a ZIF-67 / CF composite material was obtained, thoroughly cleaned with deionized water, and dried overnight at 60 °C. The obtained ZIF-67 / CF composite material was used as the cathode.
[0043] Using Eu 3+ Er 3+ Tm 3+ Or Y 3+ A rare earth metal wastewater solution was used as a simulated rare earth solution, wherein the concentration of each rare earth ion was 10 mg / L. A 20 mg / L simulated rare earth solution was mixed with a 0.1 M Na₂SO₄ electrolyte solution at a volume ratio of 1:1 to form a 35 mL mixed solution. The Na₂SO₄ electrolyte solution concentration in the mixed solution was 0.05 M, and the pH value was 5.4. The photoanode and cathode were then... Figure 1 The circuit shown is connected via an external circuit and placed in the mixed solution, using simulated sunlight (light intensity 100 mW·cm²). -2 A device for recovering rare earth metals from water was constructed by irradiating a photoanode and performing a photocatalytic reaction to recover rare earth metals from the water. After 15 minutes of reaction, the removal rate of rare earth ions in the simulated rare earth solution was measured as follows: Figure 2 As shown. Figure 2 Example 1 of the present invention is in the presence of Eu 3+ Er 3+ Tm3+ and Y 3+ The rare earth recovery efficiency curve in the simulated rare earth solution. Based on... Figure 2 It can be seen that after 15 minutes of reaction, Eu 3+ Er 3+ Tm 3+ and Y 3+ The removal rates all reached over 99%, indicating that the present invention exhibits excellent removal performance in the process of treating mixed rare earth solutions.
[0044] Figure 3 To recover Eu from the cathode ZIF-67 / CF composite material in Example 1 of this invention 3+ Er 3+ Tm 3+ and Y 3+ The subsequent SEM image; based on Figure 3 It can be seen that particulate matter is attached to the surface of the cathode ZIF-67 / CF composite sheet. Figure 4 To recover Eu from the cathode ZIF-67 / CF composite material in Example 1 of this invention 3+ Er 3+ Tm 3+ and Y 3+ The subsequent XPS spectra showed that characteristic signals of rare earth elements such as C, N, O, Co, Er, Eu, Tm, and Y could be detected, indicating that rare earth ions were effectively adsorbed and fixed on the surface of the ZIF-67 / CF composite material.
[0045] The cathode after the photocatalytic reaction was immersed in 0.1M nitric acid for 30 minutes to recover rare earth ions adsorbed on the cathode surface. Analysis of the solution after immersion showed that the recovery rate of rare earth ions after nitric acid immersion was 99.87%.
[0046] Example 2 The apparatus is basically the same as that in Example 1, and also uses a device containing Eu. 3+ Er 3+ Tm 3+ Or Y 3+ A rare earth metal wastewater solution was added to an electrolyte solution as a simulated rare earth solution to form a mixed solution, in which the concentration of each rare earth ion was 10 mg / L; the difference was that the pH values were limited to 3, 4, 5, 6, 7, 8, 9, and 10, and the results were as follows. Figure 5 As shown.
[0047] Comparative Example 1 The apparatus is basically the same as that in Example 1, and also uses a device containing Eu. 3+ Er 3+ Tm 3+ Or Y 3+A rare earth metal wastewater solution was added to an electrolyte solution as a simulated rare earth solution to form a mixed solution, in which the concentration of each rare earth ion was 10 mg / L; the difference was that the pH value was limited to 2, and the results were as follows. Figure 5 As shown.
[0048] Figure 5 The cathode ZIF-67 / CF composite material in Example 1 of this invention was used to simulate Eu in rare earth solutions under different pH conditions. 3+ Er 3+ Tm 3+ and Y 3+ The removal rate and apparent rate constant characterization diagram. Based on... Figure 5 It can be seen that when the pH value is 2, the removal rate of each rare earth ion in the simulated rare earth solution is less than 40%, indicating that the pH value of 2 will significantly affect the removal effect of rare earth ions in the simulated rare earth solution; when the pH value is 3~10, the removal rate of each rare earth ion in the simulated rare earth solution is about 100%, indicating that when the pH value is 3~10, the device of the present invention maintains excellent removal effect on different rare earth elements in the simulated rare earth solution.
[0049] in addition, Figure 5 It also shows the apparent rate constants of each rare earth ion in the simulated rare earth solution under standard solar spectral conditions and dark conditions, based on Figure 5 It can be seen that, under different pH conditions, the apparent rate constants of each rare earth ion in the simulated rare earth solution under standard solar spectrum conditions are higher than those under dark conditions, indicating that the recovery rate of the device of the present invention is higher under light conditions than under dark conditions.
[0050] Example 3 The apparatus is basically the same as that in Example 1, and also uses a device containing Eu. 3+ Er 3+ Tm 3+ Or Y 3+ A rare earth metal wastewater solution was used as a simulated rare earth solution and added to an electrolyte solution to form a mixed solution, in which the concentration of each rare earth ion was 10 mg / L. The difference was that the concentrations of the electrolyte solutions were limited to 0 M, 0.005 M, 0.01 M, 0.02 M, 0.1 M, and 0.5 M, respectively. The results are as follows: Figure 6 As shown.
[0051] Figure 6 The cathode ZIF-67 / CF composite material in Example 1 of this invention is used to simulate rare earth solutions containing Eu under different electrolyte concentrations. 3+ Er 3+ Tm 3+ and Y 3+ The removal rate and apparent rate constant characterization diagram. Based on... Figure 6It is known that the device of the present invention exhibits varying recovery effects on rare earth ions at different sodium sulfate electrolyte concentrations; the recovery effect of rare earth ions increases synchronously with the increase of electrolyte solution concentration. However, the promoting effect of electrolyte solution concentration has an upper limit; excessively high electrolyte concentrations will inhibit the recovery of different rare earth ions by the device to some extent, thereby reducing the removal rate of rare earth ions.
[0052] In addition, according to Figure 6 It can be seen that the recovery rate of different rare earth ions first increases and then decreases with the increase of electrolyte solution concentration.
[0053] Test Example 1 K was added to the simulated rare earth solution respectively + Ca 2+ Mn 2+ Al 2+ Fe 2+ Mg 2+ NH4 + Pb 2+ NO3 - Cl - Soluble salts of the ions (all concentrations 10 ppm). The apparatus constructed in Example 1 of this invention was used to test the recovery of rare earth elements from water under the influence of different ions, and the results are as follows. Figure 7 As shown. Figure 7 The cathode ZIF-67 / CF composite material in Example 1 of this invention is used to simulate Eu in rare earth solutions under different coexistence conditions of anions and cations. 3+ Er 3+ Tm 3+ and Y 3+ The removal rate and apparent rate constant characterization diagram. Based on... Figure 7 It can be seen that the device of the present invention still has good removal performance for each rare earth ion in the simulated rare earth solution under the condition that most cations are present, among which Pb 2+ With Ca 2+ It has a certain inhibitory effect on the removal process, but the removal rate of each rare earth ion can still be maintained above 75% after 15 min of photocatalytic reaction; different anions have no significant effect on the removal rate of each rare earth ion in the simulated rare earth solution.
[0054] Test Example 2 The device constructed in Example 1 of this invention was further investigated to examine the effects of different concentration gradients of EDTA, citric acid (CA), and oxalic acid (OA) on the removal efficiency of various rare earth ions. Figure 8 As shown. Figure 8 This invention, in Example 1, demonstrates the effect of the ZIF-67 / CF composite cathode material on Eu in simulated rare earth solutions under different concentrations of organic matter. 3+ Er 3+ Tm3+ and Y 3+ The removal rate and apparent rate constant characterization diagram. Based on... Figure 8 It is known that high concentrations of organic extractants can inhibit the recovery of different rare earth elements. However, through comparison, it can be seen that the recovery efficiency of the device of the present invention for different rare earth elements is significantly better than that of simple adsorption recovery under dark conditions in organic matter with different concentration gradients. Moreover, it can maintain a removal efficiency of more than 80% for organic matter with different concentration gradients.
[0055] Test Example 3 Further investigation was conducted into the repeatability of the device constructed in Example 1 of this invention for rare earth recovery in water, and the results are as follows: Figure 9 As shown. Figure 9 The cathode ZIF-67 / CF composite material in Example 1 of this invention is used to simulate Eu in rare earth solution. 3+ Er 3+ Tm 3+ and Y 3+ The characterization diagram of repeated recycling performance. Based on... Figure 9 It is known that, without elution, after the cathode is continuously operated 10 times, the device of the present invention can still maintain a removal efficiency of more than 90% for different rare earth elements.
[0056] This document uses specific examples to illustrate the principles and implementation methods of the present invention. The descriptions of the above embodiments are only for the purpose of helping to understand the method and core ideas of the present invention. Furthermore, those skilled in the art will recognize that, based on the ideas of the present invention, there will be changes in the specific implementation methods and application scope. Therefore, the content of this specification should not be construed as a limitation of the present invention.
Claims
1. A method for recovering rare earth metals from water, comprising the following steps: The photoanode and cathode, connected by an external circuit, are placed in a mixed solution of electrolyte solution and rare earth metal solution. The photoanode is then irradiated with a light source to carry out a photocatalytic reaction. The cathode after the photocatalytic reaction is immersed in nitric acid to recover rare earth ions adsorbed on the cathode surface.
2. The method according to claim 1, characterized in that, The photoanode includes a conductive glass-based semiconductor thin film and a photovoltaic cell.
3. The method according to claim 2, characterized in that, The conductive glass-based semiconductor thin film is a titanium dioxide thin film; the photovoltaic cell includes a silicon solar cell.
4. The method according to claim 1, characterized in that, The cathode includes an electrode substrate and an organometallic framework material loaded on the surface of the electrode substrate.
5. The method according to claim 4, characterized in that, The electrode substrate comprises carbon felt; the organometallic framework material is ZIF-67; and the loading of the ZIF-67 material is 7~10 mg·cm³. -2 .
6. The method according to claim 1, characterized in that, The electrolyte solution includes a sodium sulfate solution, and the concentration of the electrolyte solution in the mixed solution is 0.005~0.5M.
7. The method according to claim 1, characterized in that, The rare earth metal solution is a wastewater solution containing rare earth ions, including Eu. 3+ Er 3+ Tm 3+ and Y 3+ One or more of the following: the concentration of rare earth ions in the rare earth metal solution is 5~15 mg / L; the volume ratio of electrolyte solution to rare earth metal solution in the mixed solution is 1~2:1~2.
8. The method according to claim 1, characterized in that, The light source includes simulated sunlight, xenon lamp light source, ultraviolet light source, LED light source, or natural light; the light intensity of the light source is 50~150mW·cm. -2 .
9. The method according to claim 1, characterized in that, The photocatalytic reaction takes 1 to 30 minutes.
10. The method according to claim 1, characterized in that, The concentration of the nitric acid is 0.1~0.2M; the soaking time is 20~30min.