A material preparation method for efficient rubidium recovery

By optimizing the extractant and processing steps, KST, a material for the efficient recovery of rubidium, was prepared, solving the problem of selective enrichment of rubidium from complex solid waste. This enabled the efficient recovery and recycling of rubidium, improving the recovery rate and resource utilization rate.

CN123108315APending Publication Date: 2026-11-17YUNNAN FRONTIER WATER ENVIRONMENT IND RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611408751.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-11
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The lack of low-cost, efficient, and environmentally friendly methods to selectively enrich and recover rubidium from complex rubidium-containing solid waste means that existing technologies cannot meet the needs for sustainable recycling and reuse of rubidium resources.

Method used

KST, a material for efficient rubidium recovery, is prepared by treating silicon-based solid waste with a specific combination of extractants, dopants, and molding agents through a process of settling, stirring, filtering, and drying. This includes the use of acidic and alkaline solvents and solid reagents of specific elements, as well as optimization of solid-liquid ratio and temperature conditions.

Benefits of technology

It increased the rubidium recovery rate by about 20%-30%, significantly improved the utilization rate of waste resources, reduced the rubidium content in wastewater, and achieved efficient rubidium recovery and environmentally friendly resource recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to the field of materials science and engineering, and proposes a method for preparing materials for efficient rubidium recovery. The steps include: adding extractant A to silicon-containing solid waste at a solid-liquid ratio, allowing it to stand for 20-180 minutes, and then filtering to obtain extract Y; adding dopant B to extract Y, stirring, and allowing it to stand to obtain precursor Q; adding forming agent C to precursor Q, stirring at a constant temperature, and then filtering, washing, and drying to obtain material KST for efficient rubidium recovery. This invention achieves efficient rubidium separation by optimizing the selection of the extractant and the solid-liquid ratio during the extraction process. Experimental data show that, under the same conditions, the rubidium recovery rate is increased by approximately 20%-30% compared to traditional methods. In wastewater using the KST series materials prepared according to this invention, the rubidium content is reduced from 300-500 mg / L to 5-8 mg / L.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the fields of materials science and engineering, and more specifically, to a method for preparing materials for the efficient recovery of rubidium. Background Technology

[0002] Rubidium has low abundance in the Earth's crust and is mainly derived from the mining and extraction of lithium ore. Due to the environmental impact and economic costs of traditional mining methods, direct extraction of rubidium from ore is not a sustainable solution. Rubidium has important applications in many high-tech industries, such as in the manufacture of atomic clocks, optoelectronic devices, medical imaging equipment, and certain types of batteries. With technological advancements, the applications of rubidium are expanding, leading to a growing demand for its recycling and reuse. As environmental awareness increases, resource recycling and reuse have become a global focus. Efficient rubidium recycling technologies can not only reduce dependence on natural resources but also lower production costs and reduce waste emissions, thus having a positive impact on environmental protection.

[0003] Currently, there is still a lack of a low-cost, high-efficiency, and environmentally friendly method for the selective enrichment and recovery of rubidium from complex rubidium-containing solid waste, which would provide new research ideas for the recycling of rubidium resources and the sustainable development of the industry. Summary of the Invention

[0004] In view of this, the present invention proposes a material preparation method for efficient recycling of rubidium, in order to overcome the shortcomings of existing technologies in terms of resource utilization, cost control and environmental impact, thereby achieving sustainable recycling and reuse of rubidium.

[0005] To achieve the above objectives, this invention proposes a material preparation method for efficient rubidium recovery, comprising: (1) Extractant A is added to solid waste containing silicon according to the solid-liquid ratio, and after standing for 20-180 minutes, the extract is filtered to obtain extract Y; (2) Add dopant B to the extract Y, stir and let stand to obtain precursor Q; (3) Add molding agent C to the precursor Q, stir at a constant temperature, and after filtration, washing and drying, obtain material KST for efficient rubidium recovery.

[0006] 2. The method according to claim 1, wherein the solid waste is silicon-based waste containing one or more elements selected from phosphorus, magnesium, calcium, fluorine, nitrogen, sulfur, antimony, iodine, and aluminum.

[0007] 3. The method according to claim 1, wherein the extractant A is an acidic solvent selected from one or more of hydrochloric acid, nitric acid, hydrofluoric acid, sulfuric acid, acetic acid, phosphomolybdic acid, and citric acid.

[0008] 4. The method according to claim 1, wherein the dopant B is a solid reagent containing one or more elements selected from fluorine, chlorine, bromine, iodine, beryllium, lithium, sodium, aluminum, platinum, and molybdenum.

[0009] 5. The method according to claim 1, wherein the molding agent C is an alkaline reagent selected from one or more of potassium hydroxide, nickel hydroxide, sodium hydroxide, magnesium hydroxide, calcium oxide, sodium carbonate, and sodium bicarbonate.

[0010] 6. The method according to claim 1, wherein the solid-liquid ratio in step (1) is 1:6 to 1:15.

[0011] 7. The method according to claim 1, wherein the stirring time in step (2) is 20 minutes and the standing time is 15-30 minutes.

[0012] 8. The method according to claim 1, wherein the constant temperature in step (3) is 30°C to 65°C.

[0013] 9. The method according to any one of claims 1 to 8, wherein the material KST for efficient rubidium recovery is used to selectively adsorb or recover rubidium from rubidium-containing waste liquid or solid waste.

[0014] Compared with the prior art, the beneficial effects of the present invention are as follows: By optimizing the selection of the extractant and the solid-liquid ratio, this invention achieves highly efficient separation of rubidium during the extraction process. Experimental data show that, under the same conditions, the recovery rate of rubidium is increased by approximately 20%-30% compared to traditional methods.

[0015] This invention utilizes silicon-based waste containing multiple elements such as phosphorus, magnesium, and calcium as raw materials, increasing the resource utilization rate of waste by more than 50%, significantly reducing the environmental burden of solid waste, and embodying the concept of green chemistry.

[0016] In wastewater containing the KST series materials prepared using this invention, the rubidium content is reduced from 300-500 mg / L to 5-8 mg / L. Detailed Implementation

[0017] Exemplary embodiments of this disclosure will now be described in detail. However, it should be understood that this disclosure may be implemented in various forms and should not be limited to the embodiments set forth herein. Rather, these embodiments are provided to enable a more thorough understanding of this disclosure and to fully convey its scope to those skilled in the art. It should be noted that, unless otherwise specified, the embodiments and features described herein can be combined with each other. The invention will now be described in detail with reference to the embodiments.

[0018] This invention proposes a material preparation method for efficient rubidium recovery, comprising the following steps: (1) Add extractant A to solid waste at a certain solid-liquid ratio, let stand for 20-180 minutes, and then filter to obtain extract Y; (2) Add dopant B to the extract Y obtained in step (1), stir thoroughly and let stand for a certain time to obtain precursor Q.

[0019] (3) Add molding agent C to the precursor Q obtained in step (2), stir at a constant liquid temperature, and then obtain material KST for efficient recovery of element rubidium by means of filtration, drying, washing and drying.

[0020] As a preferred embodiment, the solid waste in step (1) is silicon-based waste containing one or more of the following elements: phosphorus, magnesium, calcium, fluorine, nitrogen, sulfur, antimony, iodine, and aluminum.

[0021] As a preferred embodiment, the extractant A in step (1) comprises one or more acidic solvents such as hydrochloric acid, nitric acid, hydrofluoric acid, sulfuric acid, acetic acid, phosphomolybdic acid, and citric acid. As a preferred embodiment, the dopant B in step (2) is a solid reagent containing one or more of fluorine, chlorine, bromine, iodine, beryllium, lithium, sodium, aluminum, platinum, and molybdenum; As a preferred embodiment, the molding agent C in step (3) is an alkaline reagent containing one or more of the following: potassium hydroxide, nickel hydroxide, sodium hydroxide, magnesium hydroxide, calcium oxide, sodium carbonate, and sodium bicarbonate.

[0022] Example 1 (1): Extractant A (15% hydrochloric acid: 20% nitric acid = 1:2) was added to silicon-containing solid waste at a solid-liquid ratio of 1:10. After standing for 30 minutes, extract Y was obtained.

[0023] (2): Add dopant B (sodium fluoride: calcium fluoride: magnesium fluoride = 1:3::2) to the extract Y, stir at a constant speed for 20 minutes, and let stand for 30 minutes to obtain precursor Q.

[0024] (3): Add molding agent C (potassium hydroxide: calcium hydroxide: aluminum hydroxide = 2:3:2) to precursor Q, stir at a constant liquid temperature of 65℃, and after filtration, drying, washing and drying, obtain material KST-1 for efficient recovery of element rubidium.

[0025] Example 2 (1): Extractant A (15% hydrochloric acid: 10% sulfuric acid = 1:3) was added to silicon-based solid waste containing magnesium and aluminum at a solid-liquid ratio of 1:6. After standing for 45 minutes, extract Y was obtained.

[0026] (2): Add dopant B (lithium chloride: calcium chloride: potassium chloride = 2:1:3) to the extract Y, stir at a constant speed for 20 minutes, and let stand for 15 minutes to obtain precursor Q.

[0027] (3): Add molding agent C (sodium carbonate: sodium bicarbonate: calcium carbonate: aluminum hydroxide = 6:8:5:1) to precursor Q, stir at a constant liquid temperature of 30°C, and after filtration, drying, washing and drying, obtain material KST-2 for efficient recovery of element rubidium.

[0028] Example 3 (1): Extractant A (hydrochloric acid: acetic acid: citric acid = 1:5:5) was added to silicon-containing solid waste with sulfur and nitrogen at a solid-liquid ratio of 1:15. After standing for 120 minutes, extract Y was obtained.

[0029] (2): Add dopant B (sodium bromide:sodium iodide:aluminum chloride = 1:1:5) to the extract Y, stir at a constant speed for 20 minutes, and let stand for 25 minutes to obtain precursor Q.

[0030] (3): Add molding agent C (magnesium hydroxide) to precursor Q, stir at a constant liquid temperature of 45°C, filter, dry, wash and dry to obtain material KST-3 for efficient recovery of element rubidium.

[0031] Comparative Example (1) Take silicon-containing solid waste containing phosphorus and calcium from the same source and with the same composition as in Example 1 as raw material, and add 20% hydrochloric acid to the solid waste at a solid-liquid ratio of 1:5; (2) After standing at room temperature for 60 minutes, filter to obtain the comparative extract Y' (3) The above extract Y' is heated to evaporate the water and obtain precursor slurry Q'.

[0032] (4) Add sodium hydroxide solution to the concentrated precursor slurry Q' until the pH of the mixture is adjusted to neutral.

[0033] (5) Stir at room temperature for 30 minutes, then filter, wash with deionized water, and dry at 80°C for 12 hours to obtain material CST.

[0034] The CST prepared in the comparative example and the KST-1, KST-2 and KST-3 prepared in Examples 1-3 were used to treat simulated wastewater with the same initial rubidium concentration of 400 mg / L. The material dosage was 1 g / L, the adsorption time was 60 minutes, the temperature was 25℃, and the rubidium recovery rate was determined. Meanwhile, using rubidium-silicon-containing solid waste of the same composition as raw materials, after each complete process, the mass percentage of the target component in the solid waste converted into a stable material matrix is ​​calculated, and the raw material resource utilization rate is determined. Meanwhile, CST prepared in the comparative example and KST-1, KST-2 and KST-3 prepared in Examples 1-3 were used to treat simulated wastewater with an initial rubidium concentration of 400 mg / L, respectively. The material dosage was 2 g / L. After adsorption equilibrium, the concentration of the supernatant was measured, and the residual rubidium concentration in the wastewater was measured.

[0035] The statistical results are shown in Table 1 below.

[0036] Table 1

[0037] As shown in Table 1, the KST series materials prepared using the method of this invention, compared with the CST comparative material prepared by the traditional process, achieve a rubidium recovery rate of 89% to 92% under the same treatment conditions, which is more than 20 percentage points higher than the approximately 68% of the traditional method, representing a relative improvement of more than 30%. Simultaneously, this method significantly increases the resource utilization rate of rubidium-containing silicon solid waste from approximately 32% of the traditional process to over 80%, achieving high-value transformation of waste. After deep treatment with KST materials, the residual concentration of rubidium in the wastewater can be stably reduced to an ultra-low level of 5-8 mg / L, with the purification effect improved by an order of magnitude compared to the traditional method. Furthermore, the optimization of the extractant combination, dopant introduction, and molding agent control in this invention achieves a significant improvement in recovery efficiency, economic cost, and environmental performance.

[0038] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit it. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that modifications or equivalent substitutions can still be made to the specific implementation of the present invention. Any modifications or equivalent substitutions that do not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing materials for efficient rubidium recovery, characterized in that, Includes the following steps: (1) Extractant A is added to solid waste containing silicon according to the solid-liquid ratio, and after standing for 20-180 minutes, the extract is filtered to obtain extract Y; (2) Add dopant B to the extract Y, stir and let stand to obtain precursor Q; (3) Add molding agent C to the precursor Q, stir at a constant temperature, and after filtration, washing and drying, obtain material KST for efficient rubidium recovery.

2. The method according to claim 1, characterized in that, The solid waste is silicon-based waste containing one or more elements selected from phosphorus, magnesium, calcium, fluorine, nitrogen, sulfur, antimony, iodine, and aluminum.

3. The method according to claim 1, characterized in that, The extractant A is an acidic solvent selected from one or more of hydrochloric acid, nitric acid, hydrofluoric acid, sulfuric acid, acetic acid, phosphomolybdic acid, and citric acid.

4. The method according to claim 1, characterized in that, The dopant B is a solid reagent containing one or more elements selected from fluorine, chlorine, bromine, iodine, beryllium, lithium, sodium, aluminum, platinum, and molybdenum.

5. The method according to claim 1, characterized in that, The molding agent C is an alkaline reagent selected from one or more of potassium hydroxide, nickel hydroxide, sodium hydroxide, magnesium hydroxide, calcium oxide, sodium carbonate, and sodium bicarbonate.

6. The method according to claim 1, characterized in that, The solid-liquid ratio in step (1) is 1:6 to 1:

15.

7. The method according to claim 1, characterized in that, The stirring time in step (2) is 20 minutes, and the standing time is 15-30 minutes.

8. The method according to claim 1, characterized in that, The constant temperature in step (3) is 30°C to 65°C.

9. The method according to any one of claims 1 to 8, characterized in that, The material KST for efficient rubidium recovery is used to selectively adsorb or recover rubidium from rubidium-containing liquid or solid waste.