A method for pretreatment of magnesium slag
By combining closed-loop dry waste heat recovery cooling with dry density separation and magnetic separation for iron removal, the problems of high-temperature waste heat recovery and impurity separation of hot magnesium slag are solved, realizing efficient pretreatment and resource utilization of magnesium slag.
Patent Information
- Application Number
- CN202611384453.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-08
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies lack a pretreatment method that can concentrate the recovery of high-temperature waste heat from hot magnesium slag, perform low-oxygen controlled cooling, and continuously couple dry physical pre-sorting with magnetic separation for iron removal, while avoiding prolonged natural stacking cooling and direct water quenching. This results in low efficiency of magnesium slag resource utilization.
A closed-loop rotary dry waste heat recovery cooling device is used to perform low-oxygen initial cooling and final cooling on hot magnesium slag. Combined with dry density separation and magnetic separation for iron removal, heavy products and light products are obtained respectively, thus achieving efficient pretreatment of magnesium slag.
Effective recovery of sensible heat from hot magnesium slag reduces oxidation loss and improves the separation efficiency of metals and iron-containing impurities, resulting in pretreated magnesium slag suitable for high-value utilization.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention relates to the field of comprehensive utilization of iron and steel smelting, and in particular to a method for pre-treatment of magnesium slag that involves low-oxygen dry waste heat recovery cooling, dry density pre-sorting, and magnetic separation for iron removal from hot magnesium slag discharged from the silicothermic magnesium smelting process. Background Technology
[0002] Magnesium reduction slag is a solid byproduct produced during the silicothermic magnesium smelting process. It is discharged at a relatively high temperature and mainly consists of CaO, SiO2, MgO, and corresponding silicate phases, while also carrying a certain amount of metallic iron, residual ferrosilicon particles, and ferromagnesian magnetic inclusions. The Ca, Si, and Mg components in the magnesium reduction slag have a certain degree of compatibility with the basic composition of inorganic materials such as continuous casting protective slag and calcium-magnesium silicate materials. If the content of metallic and ferromagnesian impurities can be reduced and its batch composition stabilized, it can be used as a valuable secondary inorganic raw material.
[0003] Current methods for cooling magnesium reduction slag mainly employ natural stack cooling or water quenching. Natural stack cooling has low equipment requirements, but it takes a long time to cool, makes it difficult to recover high-temperature sensible heat, and can cause hot slag to occupy the site for a long time. Water quenching can quickly cool down and refine particles, but it introduces more moisture into the material, requiring subsequent dehydration and drying. Furthermore, the high-temperature sensible heat is mainly carried away by the cooling water, which is not conducive to directly forming a continuous dry pretreatment process.
[0004] In existing magnesium reduction slag resource utilization routes, a magnetic separation iron removal step is usually included. Simple magnetic separation can separate some strongly magnetic metallic iron and iron-containing particles, but the residual ferrosilicon and high-density iron-containing inclusions in magnesium slag have differences in particle size and encapsulation state. When all materials are directly fed into the magnetic separation equipment, the processing load of the magnetic separation equipment is large, and the mixing of some high-density particles with silicate-based particles will affect the fine iron removal effect.
[0005] Furthermore, residual metallic iron and ferrosilicon in hot magnesium slag are easily further oxidized in high-temperature air environments. If exposed to oxygen-rich gas for extended periods at high temperatures, a surface oxide layer may form or secondary bonding with surrounding silicates may occur, weakening the original density and magnetic differences and hindering subsequent separation using a combined "density pre-sorting—magnetic separation for iron removal" method. Therefore, it is necessary to control the oxygen content and cooling rate during the hot cooling stage.
[0006] Therefore, existing technologies lack a pretreatment method that can concentrate the high-temperature waste heat recovery, low-oxygen controlled cooling, and continuously couple dry physical pre-sorting with magnetic separation and iron removal of hot magnesium slag, while avoiding prolonged natural stacking cooling and direct water quenching. Summary of the Invention
[0007] To address the issues of heat loss due to natural stacking and cooling of hot magnesium slag, the introduction of large amounts of moisture through direct water quenching, and the insufficient effectiveness of single-stage magnetic separation in separating complex iron-containing particles, this invention provides a magnesium slag pretreatment method. This method sequentially couples hot residual heat recovery, low-oxygen controlled cooling, dry density pre-sorting, and magnetic separation for iron removal. While avoiding natural stacking and cooling and direct water quenching, it fully utilizes the density and magnetic differences between residual metallic iron and ferrosilicon and calcium magnesium silicate-based particles to obtain pretreated magnesium slag suitable for subsequent high-value utilization.
[0008] To achieve the above objectives, the present invention provides the following solution: This invention provides a method for pretreatment of magnesium slag, comprising the following steps: Step 1: The hot magnesium slag discharged from the magnesium smelting process is directly fed into a closed rotary dry waste heat recovery and cooling device, so that the hot magnesium slag is cooled in sequence through a low-oxygen primary cooling zone and a final cooling zone. Step 2: The cooled magnesium slag is crushed and classified by particle size to obtain magnesium slag particles to be sorted. Step 3: Dry density separation is performed on the magnesium slag particles to be separated to obtain heavy products and light products respectively. Step 4: Perform magnetic separation to remove iron from the light product to obtain pretreated magnesium slag.
[0009] This invention directly feeds the hot magnesium slag discharged from the magnesium smelting process into a closed rotary dry waste heat recovery and cooling device, eliminating the need for natural cooling and storage or direct water quenching.
[0010] The purpose of dry density separation of the magnesium slag particles to be separated is to separate particles rich in metallic iron, ferrosilicon residues and high-density iron-containing inclusions from calcium magnesium silicate-based particles.
[0011] The purpose of magnetic separation to remove iron from the light product is to remove residual metallic iron, ferrosilicon particles, and ferromagnetic inclusions.
[0012] Preferably, in step 1, the hot magnesium slag is the reducing slag discharged from the silicothermic magnesium smelting process, and the temperature of the hot magnesium slag when it enters the closed rotary dry waste heat recovery cooling device is 1000-1150 ℃.
[0013] Preferably, in step 1, the closed rotary dry waste heat recovery and cooling device includes, in sequence along the material conveying direction, a slag inlet section, a low-oxygen primary cooling zone, a final cooling zone, and a slag outlet section; the low-oxygen primary cooling zone is equipped with a low-oxygen circulating cooling gas inlet, a waste heat gas outlet, a frequency converter, a material turning component, and a temperature detection device.
[0014] Preferably, in step 1, the low-oxygen initial cooling zone uses a low-oxygen circulating cooling gas with an oxygen volume fraction of no more than 5%, so that the hot magnesium slag is cooled from the temperature when it enters the low-oxygen initial cooling zone to 500-800 ℃; the average cooling rate of the low-oxygen initial cooling zone is 10-40 ℃ / min.
[0015] Preferably, in step 1, the low-oxygen initial cooling process is controlled by adjusting one or more of the following: the low-oxygen circulating cooling gas flow rate, the low-oxygen circulating cooling gas inlet temperature, the rotary drum speed, the magnesia slag feed rate, and the residence time of the magnesia slag in the low-oxygen initial cooling zone; wherein the low-oxygen circulating cooling gas flow rate is 1500–5000 Nm³. 3 / h; the inlet temperature of the low-oxygen circulating cooling gas is 20-80 ℃; the rotation speed of the rotary drum is 0.5-3.0 r / min; the feed rate of magnesium slag is 0.5-2.0 t / h; the average residence time of magnesium slag in the low-oxygen primary cooling zone is 10-25 min.
[0016] Preferably, in step 1, the final cooling zone uses direct heat exchange with cooling gas, indirect heat exchange with circulating water, or a combination of both to reduce the temperature of the magnesium slag to below 250 ℃; when indirect heat exchange with circulating water is used, the circulating water flows in the jacket of the rotary cylinder, the heat exchange tube bundle, or the heat exchange wall, and remains physically isolated from the magnesium slag.
[0017] Preferably, in step 2, the moisture content of the cooled magnesium slag is not higher than 1.5%; the particle size of the magnesium slag particles to be sorted is 0.5 to 8 mm.
[0018] Preferably, in step 3, the dry density separation adopts one or more of air jigging, airflow reseparation, and vibrating airflow separation.
[0019] The purpose of dry density separation is to use vibration and pulsating airflow to cause the magnesium slag particles to be separated to form stratified layers according to their density differences, thereby collecting heavy products and light products separately.
[0020] Preferably, in step 4, the magnetic induction intensity of the magnetic separation and iron removal is 0.6 to 1.0 T.
[0021] In this invention, the heavy products are collected separately as iron-rich byproducts; the pretreated magnesium slag has CaO, SiO2 and MgO as the main available oxide components.
[0022] Preferably, the obtained pretreated magnesium slag, after chemical composition testing and homogenization, is compounded with one or more of bauxite, wollastonite, quartz sand, alumina, carbonates and melting regulators, and used as a calcium-, silicon-, and magnesium-containing basic raw material for continuous casting protective slag.
[0023] Compared with the prior art, the present invention has the following beneficial effects: (1) Hot magnesium slag does not undergo long-term natural cooling and direct water quenching, but directly enters a closed rotary dry waste heat recovery device, which can concentrate and recover the sensible heat released in the high-temperature stage in the form of hot gas or heat exchange medium, thereby reducing waste heat loss.
[0024] (2) Low oxygen initial cooling reduces the further oxidation of metallic iron and ferrosilicon residues in the high temperature stage, which is conducive to maintaining the density and magnetic difference between iron-containing particles and calcium magnesium silicate-based particles, providing a more stable sorting basis for subsequent dry density separation and magnetic separation to remove iron.
[0025] (3) First, dry density separation is used to pre-enrich high-density metals and iron-containing particles, and then magnetic separation is used to remove iron from light products. This can reduce the amount of material directly entering the magnetic separation equipment and improve the targeting of iron removal.
[0026] (4) In the final cooling process, direct gas heat exchange or indirect circulating water heat exchange is used. The cooling water and magnesium slag can be physically isolated, so that the material is kept in a dry processing state and the subsequent deep drying load is reduced.
[0027] (5) The pretreated magnesium slag retains the main usable components such as CaO, SiO2 and MgO. The heavy products can be collected separately as iron-rich by-products, which is conducive to the separate utilization of silicate components and iron-containing components in magnesium slag. Detailed Implementation
[0028] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation on the scope of protection of the present invention, but should be understood as a further explanation of the technical concept, process steps and preferred parameters of the present invention.
[0029] It should be understood that the upper limit, lower limit and intermediate value of the numerical range used in this invention can be used in combination without departing from the technical purpose of this invention; unless the context clearly defines otherwise, the range also includes endpoint values.
[0030] Unless otherwise stated, the technical and scientific terms used herein have the meanings commonly understood by those skilled in the art. For feeding, conveying, heat exchange, crushing, screening, and testing equipment not specifically defined in this specification, conventional industrial equipment capable of achieving the same purpose may be used.
[0031] The terms “comprising,” “including,” “having,” and “containing” used in this document are all open-ended terms, indicating that they include, but are not limited to, the listed technical features.
[0032] Unless otherwise specified, "%" in this invention refers to mass percentage; the oxygen content in the cooling gas is expressed as volume fraction.
[0033] Unless otherwise specified, the technical solutions described in this invention are all conventional solutions in the field.
[0034] This invention provides a method for pretreatment of magnesium slag, including the following steps: low-oxygen dry waste heat recovery cooling of hot magnesium slag, final cooling, drying and crushing and particle size classification, dry density separation and magnetic separation for iron removal.
[0035] During the hot cooling stage, the hot magnesia slag discharged from the magnesia smelting process at 1000–1150 °C is directly fed into a closed rotary dry waste heat recovery cooling device. It undergoes initial cooling in a low-oxygen circulating cooling gas with an oxygen volume fraction of no more than 5%, reducing the slag temperature to 500–800 °C. Then, in the final cooling zone, the slag is further cooled to below 250 °C. During the low-oxygen initial cooling stage, the average cooling rate is maintained at 10–40 °C / min through the coordinated control of circulating gas flow rate, inlet temperature, rotary drum speed, feed rate, and residence time.
[0036] In the dry separation stage, the final cooled magnesium slag is crushed and classified into 0.5-8 mm particles. First, air jigging, airflow gravity separation or vibrating airflow separation is used for density pre-separation to enrich metallic iron, ferrosilicon residues and high-density iron-containing inclusions into the heavy products. Then, the light products are subjected to magnetic separation to remove residual magnetic iron-containing components, and pretreated magnesium slag is obtained.
[0037] The pretreated magnesium slag obtained by the method of this invention, after component detection and homogenization, can be used as one of the sources of CaO, SiO2 and MgO, and can be compounded with other conditioning raw materials for continuous casting protective slag or other calcium magnesium silicate materials.
[0038] The magnesium slag referred to in this invention is preferably the reduction slag discharged after high-temperature reduction in the silicothermic magnesium smelting process. Typical magnesium slag mainly consists of CaO, SiO2, and MgO as oxides, and contains small amounts of Al2O3, iron oxides, as well as metallic iron, ferrosilicon residues, and other inclusions. Since different raw material ratios and reduction regimes can lead to fluctuations in the composition of magnesium slag, it is preferable to test the content of CaO, SiO2, MgO, Al2O3, and total iron on a batch-by-batch basis during industrial implementation.
[0039] In a preferred embodiment of the present invention, the temperature of the hot magnesia slag entering the closed rotary dry waste heat recovery cooling device is controlled at 1000–1150 °C. If the temperature is too low, the high-grade sensible heat has already been lost during transfer or storage, which is detrimental to centralized waste heat recovery; if the temperature is too high, the requirements for the temperature resistance of the feed seal, the cylinder refractory material, and the heat exchange components are significantly increased. Therefore, the present invention preferably involves the magnesia slag being transferred in a closed system and directly introduced into the rotary cooling device as soon as possible after discharge.
[0040] The closed-loop rotary dry waste heat recovery cooling device is sequentially configured along the material conveying direction as a slag inlet section, a low-oxygen primary cooling zone, a final cooling zone, and a slag outlet section. The low-oxygen primary cooling zone includes a low-oxygen circulating cooling gas inlet, a waste heat gas outlet, a variable frequency air supply device, a temperature detection device, and lifting plates, tipping plates, or other material agitation components. During the rotation of the rotary drum, the magnesium slag continuously agitates and renews the heat exchange surface to improve the uniformity of solid-gas heat exchange.
[0041] In a preferred embodiment of the invention, the oxygen volume fraction of the low-oxygen circulating cooling gas is no more than 5%. The low-oxygen gas can be circulating flue gas, a mixture of nitrogen and circulating gas, or other gases that meet the low-oxygen requirements. The reason for controlling the oxygen content is that residual metallic iron and ferrosilicon in the hot magnesium slag are easily oxidized further in a high-temperature, oxygen-rich environment, forming a thicker oxide layer or undergoing secondary bonding with the silicate matrix, thereby weakening the density and magnetic differences between them and the silicate particles. Using low-oxygen initial cooling is beneficial for recovering waste heat while preserving the differences required for subsequent physical sorting.
[0042] In a preferred embodiment of the invention, low-oxygen initial cooling reduces the magnesium slag temperature from the feed temperature to 500–800 °C, with a temperature drop controlled at 250–500 °C and an average cooling rate of 10–40 °C / min. When the average cooling rate is below 10 °C / min, the equipment size and residence time increase, leading to a decrease in continuous processing efficiency; when the average cooling rate is too high, the temperature gradient between the material and the equipment increases, easily increasing fine powder generation and thermal stress on the equipment. Therefore, the circulating gas flow rate, gas inlet temperature, rotary drum speed, feed rate, and residence time are synergistically controlled.
[0043] Preferably, the rotational speed of the rotary drum is 0.5–3.0 r / min, the average residence time of the magnesium slag in the low-oxygen primary cooling zone is 10–25 min, and the inlet temperature of the circulating cooling gas is 20–80 °C. After being discharged from the low-oxygen primary cooling zone, the waste heat gas can be used for heat utilization in a waste heat boiler, hot air heat exchanger, or raw material drying system.
[0044] Finally, it turned cold: After initial cooling in a low-oxygen environment, the magnesium slag enters the final cooling zone and is further cooled to below 250 °C. Final cooling can be achieved through direct heat exchange with cooling gas, indirect heat exchange with circulating water, or a combination of both.
[0045] When indirect heat exchange using circulating water, the circulating water flows within the jacket, heat exchange tube bundle, or heat exchange wall of the cylinder, maintaining physical isolation from the magnesia slag. The purpose of this setup is to continue utilizing the high heat exchange capacity of water to complete the final cooling process, but without allowing liquid water to directly enter the magnesia slag, thereby maintaining the dry material conditions required for subsequent crushing and sorting. For magnesia slag whose moisture content meets the requirements after final cooling, a separate deep drying step is not necessary.
[0046] In a preferred embodiment of the present invention, the magnesium slag after final cooling is dried as necessary according to its actual moisture content, so that the moisture content of the particles to be sorted is not higher than 1.5%. When the moisture content is too high, the fine particles are prone to sticking together, which will affect the looseness and stratification of the material layer during the airflow separation process; controlling it below 1.5% is beneficial to maintaining the stability of dry density separation.
[0047] In a preferred embodiment of the present invention, magnesium slag is crushed and sieved into particles of 0.5–8 mm to be separated. If the particle size is too small, the particles are easily entrained by the airflow, weakening the effect of density difference on settling and stratification; if the particle size is too large, metallic iron, ferrosilicon, and iron-containing inclusions may not be fully dissociated, affecting the separation selectivity. Therefore, the present invention first improves the stability of dry density separation through crushing and dissociation, and then through particle size classification.
[0048] In a preferred embodiment of the present invention, dry density separation employs one or more of air jigging, airflow gravity separation, and vibrating airflow separation. During separation, the granular material layer is kept loose by pulsating airflow and vibration, and stratification occurs according to the particle density difference; particles rich in metallic iron, ferrosilicon residues, and high-density iron-containing inclusions are enriched in the heavy product, while calcium magnesium silicate-based particles mainly enter the light product.
[0049] This invention places density separation before magnetic separation for iron removal. Its function is not to replace magnetic separation, but rather to pre-enrich and discharge high-density iron-containing particles using density differences, allowing the magnetic separator to primarily process lighter products. This reduces the amount of material entering the magnetic separator and avoids relying solely on magnetic differences to process all complex iron-containing particles.
[0050] The separation airflow velocity, vibration frequency, bed thickness, and feed rate can be adjusted according to the particle size and the occurrence state of iron-containing particles in the raw material, with the principle of forming stable stratification and reducing the entry of calcium magnesium silicate particles into the heavy product. The heavy product can be collected separately for further metal recovery or utilized as an iron-rich by-product.
[0051] The light products after dry density separation are further subjected to magnetic separation for iron removal. The magnetic separation equipment can be a dry drum magnetic separator, belt magnetic separator, or roller magnetic separator, and one or more stages of magnetic separation can be used depending on the content of residual magnetic particles.
[0052] The main purpose of magnetic separation for iron removal is to remove residual metallic iron, ferrosilicon particles, and ferromagnetic inclusions that remain in the light products after density separation. Ideally, the magnetic field strength and feed layer thickness should be controlled according to the actual conditions of the raw materials to further reduce the total iron content in the pretreated magnesium slag, while minimizing the loss of CaO, SiO2, and MgO-based silicate particles.
[0053] The obtained pretreated magnesium slag should be tested for chemical composition and particle size on a batch-by-batch basis. Total iron content can be determined by chemical analysis, X-ray fluorescence analysis combined with metallic phase detection, or equivalent methods; CaO, SiO2, MgO, and Al2O3 can be determined by X-ray fluorescence spectroscopy or wet chemical analysis. The yield of light products is calculated as the ratio of the dry weight of the pretreated magnesium slag after magnetic separation and iron removal to the dry weight of the original magnesium slag to be separated.
[0054] The effectiveness of waste heat utilization during the low-oxygen initial cooling stage can be calculated through heat balance based on the inlet and outlet temperatures, flow rates, and heat capacities of the circulating gas, or by calculating the actual heat recovered by the waste heat boiler and heat exchanger. In formal industrial implementation, the heat recovery rate can be evaluated in relation to the feed temperature, discharge temperature, and throughput.
[0055] After chemical composition analysis and homogenization, the pretreated magnesium slag can be compounded with one or more of bauxite, wollastonite, quartz sand, alumina, carbonates, and melting regulators to serve as a calcium-, silicon-, and magnesium-containing basic raw material for continuous casting protective slag. Subsequent batching should be based on material balance calculations using the measured effective oxide content of the pretreated magnesium slag, taking into account the basicity, melting temperature, viscosity, and crystallization properties of the target protective slag.
[0056] The following examples use the same representative batch of silicothermic magnesium reduction slag to avoid interference from batch differences in raw materials in comparing process parameters. The main oxide composition of this magnesium slag, by mass percentage, is: CaO 59.3%, SiO2 27.7%, MgO 6.0%, Al2O3 2.0%, Fe2O3 2.6%; it also contains small amounts of separable metallic iron, ferrosilicon residues, and iron-containing inclusions. The process parameters for Examples 1-3 are shown in Table 1.
[0057] Table 1 Process parameters for Examples 1-3
[0058] Example 1 Hot magnesia slag at approximately 1050 °C is directly fed into a rotary dry waste heat recovery cooling unit via a closed feeding device. The oxygen volume fraction in the low-oxygen initial cooling zone is controlled at 3%, and the gas flow rate is 2800 Nm³. 3 The feed rate is 1.0 t / h, the inlet temperature is about 40 ℃, the rotation speed of the rotary drum is 1.5 r / min, the feed rate of magnesium slag is 1.0 t / h, and the average residence time is 18 min, which reduces the temperature of magnesium slag to about 650℃.
[0059] Subsequently, a circulating water jacket indirect heat exchange was used for final cooling, reducing the temperature of the magnesium slag to approximately 180 °C, with a final cooling time of 12 minutes. After final cooling, the slag was crushed and screened to obtain particles of 1–6 mm with a moisture content of 0.7%. Dry density separation was performed using air jigging to collect heavy and light products; the light product was further refined by 0.8 T dry magnetic separation to remove iron, yielding pretreated magnesium slag.
[0060] After processing, the light product yield was 86.5%, the total iron mass fraction of the pretreated magnesia slag was 0.72% (calculated as Fe), and the total iron mass fraction of the heavy product was 18.6%. The usable sensible heat recovered during the low-oxygen initial cooling stage was converted to approximately 68.4% of the theoretical sensible heat of the hot magnesia slag.
[0061] Example 2 The only difference from Example 1 is that the hot magnesium slag feed temperature is about 1100 ℃, the oxygen volume fraction in the low oxygen initial cooling zone is controlled at 2%, the circulating gas inlet temperature is about 60 ℃, the rotary drum speed is 1.0 r / min, and the average residence time is 22 min, so that the magnesium slag is cooled to about 700 ℃.
[0062] The final cooling zone employs a combination of direct heat exchange with circulating flue gas containing no more than 5% oxygen by volume and indirect heat exchange with circulating water. The inlet temperature of the circulating flue gas is approximately 40 ℃, the inlet temperature of the circulating water is approximately 25 ℃, and the outlet temperature is approximately 45 ℃, reducing the discharge temperature to approximately 160 ℃. The final cooling time is 10 minutes. After crushing and screening, particles of 0.5–5 mm with a moisture content of 0.6% are obtained. Density pre-sorting is performed using vibrating airflow separation, and the lighter products are further refined by a 1.0 T dry magnetic separator to remove iron.
[0063] After processing, the yield of light products was 84.9%, the total iron mass fraction of the pretreated magnesium slag was 0.58% (calculated as Fe), the total iron mass fraction of the heavy products was 20.1%, and the recoverable sensible heat was approximately 71.2%.
[0064] Example 3 The only difference from Example 1 is that the hot magnesium slag feed temperature is about 1020 ℃, the oxygen volume fraction in the low oxygen primary cooling zone is controlled at 5%, the circulating gas inlet temperature is about 30 ℃, the rotary drum speed is 2.5 r / min, and the average residence time is 12 min, which reduces the magnesium slag temperature to about 560 ℃.
[0065] The final cooling zone uses direct heat exchange with cooling gas to lower the magnesium slag temperature to approximately 200 °C, with a final cooling time of 15 minutes. Crushing and screening yields particles of 0.5–8 mm with a moisture content of 0.9%. Density pre-sorting is performed using airflow gravity separation, and the lighter products are further refined by 0.6 T dry magnetic separation to remove iron.
[0066] After processing, the yield of light products was 88.1%, the total iron mass fraction of the pretreated magnesium slag was 0.93% (calculated as Fe), the total iron mass fraction of the heavy products was 16.9%, and the recoverable sensible heat was approximately 63.5%.
[0067] Comparative Example 1 The only difference from Example 1 is that the hot magnesium slag at approximately 1050 °C is first naturally cooled to below 250 °C and does not enter the low-oxygen rotary dry waste heat recovery cooling device; the other crushing, particle size classification, air jigging and magnetic separation parameters are the same as in Example 1.
[0068] The comparative sample could not recover the high-temperature sensible heat in the pretreatment stage. After natural stacking cooling for 24 hours, the temperature of the magnesium slag dropped to below 250 °C. The total iron mass fraction of the pretreated magnesium slag was 0.78% based on Fe, and the light product yield was 85.8%.
[0069] Comparative Example 2 The only difference from Example 1 is that air is used as the cooling gas in the low-oxygen initial cooling zone, with an oxygen volume fraction of approximately 21%. The remaining cooling, final cooling, crushing, density separation, and magnetic separation parameters are the same as in Example 1.
[0070] After being cooled at high temperature in air, some of the metallic iron and ferrosilicon particles showed obvious oxidation, and the enrichment of heavy products decreased. The total iron mass fraction of the pretreated magnesium slag was 1.26% based on Fe, and the total iron mass fraction of the heavy products was 13.4%, which was significantly lower than the corresponding sorting effect in Example 1.
[0071] Comparative Example 3 The only difference from Example 1 is that air jigging density pre-sorting is not performed. All magnesium slag to be sorted from 1 to 6 mm is directly subjected to 0.8 T dry magnetic separation. The remaining steps are the same as in Example 1.
[0072] Since all the materials to be sorted directly enter the magnetic separation equipment, the magnetic separation load increases, and the total iron mass fraction of the pretreated magnesium slag is 1.18% based on Fe, which is higher than that in Example 1; at the same time, the iron-containing particles do not form heavy product pre-enrichment at the front end.
[0073] Comparative Example 4 The only difference from Example 1 is that the hot magnesium slag is cooled to below 100 ℃ by direct water quenching, and then subjected to pressure filtration dewatering (pressure filtration pressure is 0.4 to 0.8 MPa, and the moisture content of the material after dewatering is not higher than 10%), drying, crushing, air jigging and magnetic separation. The remaining separation parameters are the same as those in Example 1.
[0074] After water quenching, the material needs to undergo dehydration and deep drying processes. The high-temperature sensible heat of the hot magnesium slag mainly enters the cooling water, which is difficult to recover through low-oxygen circulating hot gas. The total iron mass fraction of the pretreated magnesium slag obtained after subsequent sorting is 0.76% based on Fe.
[0075] The treatment effects of Examples 1-3 and Comparative Examples 1-4 are shown in Table 2.
[0076] Table 2 Treatment effects of Examples 1-3 and Comparative Examples 1-4
[0077] As can be seen from Examples 1-3 and Comparative Examples 1-4, using low-oxygen rotary dry waste heat recovery cooling before the hot magnesia slag enters the sorting process, and setting up dry density pre-sorting before magnetic separation, can reduce the residual iron content in the pretreated magnesia slag while maintaining a high yield of light products. Compared with high-temperature air cooling, low-oxygen initial cooling is beneficial for maintaining the density and magnetic differences of iron-rich particles; compared with canceling density pre-sorting, the sequential treatment of "density pre-sorting - magnetic separation for fine iron removal" can reduce the magnetic separation load and improve the fine iron removal effect.
[0078] The above-described embodiments are only for illustrating preferred embodiments of the present invention. For those skilled in the art, without departing from the technical concept of the present invention, the gas flow rate, rotation speed, residence time, particle size range, and magnetic separation stages can be adaptively adjusted according to the actual slag discharge temperature, raw material particle size, iron content, and equipment processing capacity. All such equivalent adjustments should be understood as falling within the scope of the technical concept of the present invention.
Claims
1. A method for pretreatment of magnesium slag, characterized in that, Includes the following steps: Step 1: The hot magnesium slag discharged from the magnesium smelting process is directly fed into a closed rotary dry waste heat recovery and cooling device, so that the hot magnesium slag is cooled in sequence through a low-oxygen primary cooling zone and a final cooling zone. Step 2: The cooled magnesium slag is crushed and classified by particle size to obtain magnesium slag particles to be sorted. Step 3: Dry density separation is performed on the magnesium slag particles to be separated to obtain heavy products and light products respectively. Step 4: Perform magnetic separation to remove iron from the light product to obtain pretreated magnesium slag.
2. The magnesium slag pretreatment method according to claim 1, characterized in that, In step 1, the hot magnesium slag is the reduction slag discharged from the silicothermic magnesium smelting process, and the temperature of the hot magnesium slag when it enters the closed rotary dry waste heat recovery cooling device is 1000-1150 ℃.
3. The magnesium slag pretreatment method according to claim 1, characterized in that, In step 1, the closed rotary dry waste heat recovery and cooling device includes, in sequence along the material conveying direction, a slag inlet section, a low-oxygen primary cooling zone, a final cooling zone, and a slag outlet section; the low-oxygen primary cooling zone is equipped with a low-oxygen circulating cooling gas inlet, a waste heat gas outlet, a frequency converter, a material turning component, and a temperature detection device.
4. The magnesium slag pretreatment method according to claim 1, characterized in that, In step 1, the low-oxygen primary cooling zone uses a low-oxygen circulating cooling gas with an oxygen volume fraction of no more than 5% to cool the hot magnesium slag from its temperature when it enters the low-oxygen primary cooling zone to 500-800 ℃; the average cooling rate of the low-oxygen primary cooling zone is 10-40 ℃ / min.
5. The magnesium slag pretreatment method according to claim 4, characterized in that, In step 1, the low-oxygen primary cooling process is controlled by adjusting one or more of the following: the low-oxygen circulating cooling gas flow rate, the low-oxygen circulating cooling gas inlet temperature, the rotary drum speed, the magnesia slag feed rate, and the residence time of the magnesia slag in the low-oxygen primary cooling zone; wherein, the low-oxygen circulating cooling gas flow rate is 1500–5000 Nm³. 3 / h; the inlet temperature of the low-oxygen circulating cooling gas is 20-80 ℃; the rotation speed of the rotary drum is 0.5-3.0 r / min; the feed rate of magnesium slag is 0.5-2.0 t / h; the average residence time of magnesium slag in the low-oxygen primary cooling zone is 10-25 min.
6. The magnesium slag pretreatment method according to claim 1, characterized in that, In step 1, the final cooling zone uses direct heat exchange with cooling gas, indirect heat exchange with circulating water, or a combination of both to reduce the temperature of the magnesium slag to below 250 ℃. When indirect heat exchange with circulating water is used, the circulating water flows in the jacket of the rotary cylinder, the heat exchange tube bundle, or the heat exchange wall, and remains physically isolated from the magnesium slag.
7. The magnesium slag pretreatment method according to claim 1, characterized in that, In step 2, the moisture content of the cooled magnesium slag is not higher than 1.5%; the particle size of the magnesium slag particles to be sorted is 0.5 to 8 mm.
8. The magnesium slag pretreatment method according to claim 1, characterized in that, In step 3, the dry density separation adopts one or more of the following: air jigging, airflow gravity separation, and vibrating airflow separation.
9. The magnesium slag pretreatment method according to claim 1, characterized in that, In step 4, the magnetic induction intensity of the magnetic separation and iron removal is 0.6 to 1.0 T.
10. The magnesium slag pretreatment method according to any one of claims 1 to 9, characterized in that, After chemical composition analysis and homogenization, the pretreated magnesium slag is compounded with one or more of bauxite, wollastonite, quartz sand, alumina, carbonates and melting regulators to be used as a calcium-, silicon-, and magnesium-containing basic raw material for continuous casting protective slag.