A Zr-Nb-Ti-Ag amplitude-modulated medium-entropy alloy for orthopedic implants, its preparation method and application

By preparing a Zr-Nb-Ti-Ag alloy, wrapping Ag ingots with Ti foil, and combining annealing, cold rolling, and aging treatment to form an amplitude-modulated microstructure, the shortcomings of existing alloys in terms of plasticity, modulus, and antibacterial properties are solved, and the stability and anti-infection ability of orthopedic implants are achieved.

CN123108336APending Publication Date: 2026-11-17南方医科大学第五附属医院
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611302997.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-26
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing medical alloys cannot simultaneously achieve good plasticity, low elastic modulus, high yield strength, and good antibacterial properties, resulting in problems such as loosening and failure, infection risk, and abnormal mechanical conduction in orthopedic implants during clinical applications.

Method used

The Zr-Nb-Ti-Ag alloy preparation method involves wrapping Ag ingots with Ti foil of a specific thickness, precisely controlling the melting current, and combining annealing, cold rolling, and aging treatment to form an alternating light and dark amplitude microstructure, thereby optimizing the alloy's microstructure and properties.

Benefits of technology

The alloy exhibits excellent plasticity, low elastic modulus, and high yield strength, along with good antibacterial properties, meeting the requirements for clinical use and industrial production of orthopedic implants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108336A_ABST
    Figure CN123108336A_ABST
Patent Text Reader

Abstract

This invention relates to the field of orthopedic implant metal materials technology, specifically to a Zr-Nb-Ti-Ag amplitude-modulated medium-entropy alloy for orthopedic implants, its preparation method, and its application. The invention provides a method for preparing a Zr-Nb-Ti-Ag alloy, comprising the following steps: Under a specific ratio, Ag metal ingots coated with Ti foil, Ti metal ingots, Zr metal ingots, and Nb metal ingots are stacked sequentially from bottom to top. First, Zr and Nb are melted under a specific current to form a liquid phase and coat solid Ti and Ag. Then, the current is reduced to melt Ti and Ag. After tumbling and melting, the mixture is cooled and then vacuum-cast to obtain an alloy sheet. The alloy sheet is then subjected to annealing, cold rolling, and aging treatments to obtain the Zr-Nb-Ti-Ag alloy. This alloy possesses excellent plasticity, low elastic modulus, high yield strength, and good antibacterial properties, meeting the requirements of clinical use and industrial production of modern implantable devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of orthopedic implant metal materials technology, and in particular to a Zr-Nb-Ti-Ag amplitude-modulated medium-entropy alloy for orthopedic implants, its preparation method and application. Background Technology

[0002] The development of novel orthopedic implantable metal materials is crucial for driving the clinical iteration and upgrading of orthopedic implants. With the deepening aging of China's population, the incidence of orthopedic diseases such as osteoporosis, osteoarthritis, and traumatic fractures is rising year by year. Clinical practice is placing higher demands on the biomechanical compatibility, infection resistance, and osseointegration performance of hard tissue implantable metal materials. Currently, medical titanium and titanium alloys, with their excellent mechanical properties, corrosion resistance, and biocompatibility, have become the most widely used matrix materials in the field of orthopedic hard tissue implants. However, their inherent defects continue to limit long-term clinical efficacy: On the one hand, the elastic modulus of traditional titanium alloys is generally higher than 80 GPa, significantly different from the 10-30 GPa modulus level of human cortical bone. Excessively high elastic modulus can easily trigger a stress shielding effect, causing poor osseointegration of the surrounding bone tissue, ultimately leading to implant loosening and failure. Simultaneously, yield strength is also a key weakness restricting the service safety of titanium alloy implants. If the yield strength is insufficient, the implant is prone to irreversible plastic deformation during service, leading to fixation failure and abnormal force transmission. On the other hand, the high incidence of bacterial infection at the implantation interface can also lead to bone destruction and implantation failure. These two defects coupled together create a vicious cycle, severely affecting the long-term service stability of the implant. Therefore, developing structural-functional integrated medical metallic materials that combine low elastic modulus, high yield strength, and antibacterial properties has become a core research direction in this field.

[0003] To overcome the technical challenge of modulus mismatch in titanium-based alloys, zirconium-based alloys, with their inherently low elastic modulus, low magnetic susceptibility, excellent corrosion resistance, and good biocompatibility, have become the preferred matrix material to replace traditional titanium alloys. Based on optimizing the alloy's mechanical compatibility, doping with broad-spectrum antibacterial metal elements such as silver, copper, and zinc is a mainstream modification technique for achieving the antibacterial properties of metal implant materials. Among these, silver (Ag) combines the advantages of strong broad-spectrum antibacterial ability with no bacterial resistance, making it the optimal additive for antibacterial modification of orthopedic alloys. According to the generally accepted performance evaluation standards for medical implant alloys in this field: low-modulus alloys must meet the following requirements: elastic modulus ≤ 80 GPa to effectively alleviate stress shielding; antibacterial performance must achieve an antibacterial rate of ≥ 90% against common pathogens (such as Staphylococcus aureus) to meet clinical anti-infection needs (GB / T 4789.2-2010); plasticity must achieve an elongation at room temperature ≥ 10% to meet the requirements of plastic processing and clinical service safety (GB / T 13810-2017); and yield strength must be ≥ 870 MPa to ensure that the implant does not undergo plastic deformation under complex stress conditions (GB / T 13810-2017). Although existing research has explored many aspects of these performance goals, it has not yet been able to overcome the technical bottleneck of synergistic improvement of multiple properties. For example, Chinese patent application CN109022853A discloses a Ti-Nb-Zr-Ag cast antibacterial alloy, which achieves a low elastic modulus of 39.7~55.6 GPa, high compressive strength and antibacterial rate of 82%~99%, and has made some progress in modulus adaptation and antibacterial modification. However, this alloy, prepared using a casting process, has the following drawbacks: First, its room temperature elongation at break is only 2.2%, far below the requirement of at least 10% for Ti-Nb alloys in GB / T 13810-2017 "Titanium and Titanium Alloy Processed Materials for Surgical Implants." This indicates a significant lack of tensile plasticity. This severe lack of plasticity not only prevents the alloy from being processed into complex orthopedic devices such as bone plates, intramedullary nails, and porous implant scaffolds using conventional processes like rolling and forging, but also leads to problems such as easy cracking during processing, low yield, and poor industrial adaptability, making it difficult to meet the mass production needs of multi-specification and irregularly shaped orthopedic implants in clinical practice. Second, its antibacterial rate fluctuates widely, with the lower limit failing to meet the industry standard for stable antibacterial properties, resulting in insufficient reliability in application. Third, it does not address the yield strength property, making it impossible to determine whether its resistance to plastic deformation in high-load-bearing areas meets clinical requirements.

[0004] Therefore, there is an urgent need to develop a medical alloy that combines good plasticity (elongation at break ≥10%), low elastic modulus (≤80 GPa), high yield strength (≥870 MPa) and good antibacterial properties (antibacterial rate ≥90%) to meet the clinical application and industrial manufacturing requirements of modern orthopedic implants. Summary of the Invention

[0005] The technical problem to be solved by the present invention is to overcome the defects and shortcomings of existing medical alloys that cannot simultaneously achieve good plasticity, low elastic modulus, high yield strength and good antibacterial properties, and to provide a method for preparing Zr-Nb-Ti-Ag alloy.

[0006] Another object of the present invention is to provide a Zr-Nb-Ti-Ag alloy prepared by the above preparation method.

[0007] Another object of the present invention is to provide the application of the above-mentioned Zr-Nb-Ti-Ag alloy in the preparation of medical implant materials.

[0008] Another object of the present invention is to provide a medical implant material.

[0009] The above-mentioned objective of this invention is achieved through the following technical solution: This invention protects a method for preparing a Zr-Nb-Ti-Ag alloy, comprising the following steps: S1. Under a protective gas atmosphere, Ag metal ingots, Ti metal ingots, Zr metal ingots and Nb metal ingots coated with Ti foil are stacked sequentially from bottom to top. At 250~280 A, Zr and Nb are melted to form a liquid phase and coat solid Ti and Ag. The current is then reduced to 180~220 A to completely melt Ti and Ag. After tumbling and melting, the alloy plate is obtained by suction casting after cooling. S2. Anneal the alloy sheet obtained in step S1 at 1100~1300 ℃, cool, cold roll until the deformation of the sheet is 80%~85%, and then age the rolled sheet at 600~700 ℃ and cool to obtain Zr-Nb-Ti-Ag alloy. The atomic percentages of Ag, Ti, Zr, and Nb are (1.3%~3.2%): (8%~10%): (52%~54%): (34%~36%). The single-pass reduction during cold rolling is controlled to be 14%~17%; The thickness of the Ti foil is 0.15~0.25 mm.

[0010] To address the issue that existing medical alloys cannot simultaneously achieve good plasticity, low elastic modulus, high yield strength, and good antibacterial properties, this invention achieves a synergistic improvement in alloy microstructure and properties through synergistic optimization of the preparation process and element ratios. Specifically: First, an Ag ingot is wrapped with a Ti foil of a specific thickness. Then, Zr, Nb, and other Ti ingots are placed on top of the Ti foil. By precisely controlling the melting current, the metal dissolution process is controlled, effectively preventing Ag volatilization and ensuring compositional uniformity, resulting in an alloy sheet. Subsequently, the alloy sheet undergoes a specific annealing treatment to eliminate as-cast dendritic segregation and obtain a homogeneous matrix microstructure. Then, a specific rolling process further eliminates residual segregation and refines the grains, solidifying the microstructure foundation for its mechanical properties. Finally, a specific aging treatment eliminates processing stress and induces amplitude-modulated phase transformation in the alloy, significantly improving the material's plastic deformation capacity while ensuring the alloy's strength and hardness. Furthermore, this invention, by rationally controlling the Ag element ratio and combining it with the synergistic effect of the Zr, Nb, and Ti matrix metals, enables the alloy to possess stable antibacterial capabilities.

[0011] The Zr-Nb-Ti-Ag alloy prepared by the above process exhibits a typical alternating light and dark amplitude-modulated microstructure, mainly composed of a soft phase β1 with low elastic modulus and a hard phase β2 with high elastic modulus. During tensile deformation, the soft phase β1 guides the orderly movement of dislocations, improving the overall deformation uniformity and effectively enhancing the alloy's plasticity while maintaining its low elastic modulus. The hard phase β2, as a reinforcing phase, acts as a barrier during dislocation slip, inhibiting continuous dislocation movement and significantly improving the alloy's yield strength. Simultaneously, the heterogeneous interfaces generated by amplitude-modulated decomposition alter the dislocation slip mechanism: transforming planar slip, which easily leads to localized stress concentration, into cross-slip, further optimizing deformation uniformity and enabling the alloy to achieve long-term strain-strengthening effects. Ultimately, the alloy possesses excellent plasticity, low elastic modulus, high yield strength, and antibacterial properties, meeting the requirements for clinical use and industrial production of modern implantable devices.

[0012] Furthermore, the protective gas is argon.

[0013] Furthermore, the purity of the argon gas is ≥99.5%.

[0014] Furthermore, air purging pretreatment is required before introducing the protective gas.

[0015] Furthermore, the pretreatment operation is as follows: the furnace body is evacuated to a vacuum degree ≤1×10⁻⁶. 3 Pa, then fill with argon gas, and repeat the above vacuuming and argon filling operation 2 to 3 times, until the reaction vessel is completely filled with argon gas.

[0016] Furthermore, as a preferred embodiment, the Ag metal ingot is an Ag metal ingot coated with Ti foil.

[0017] Furthermore, the atomic percentages of Ag, Ti, Zr and Nb are (1.5%~3%): (8.8%~9.8%): (52.8%~53.8%): (34.8%~35.8%).

[0018] Furthermore, there are no special limitations on the container for placing the metal ingot.

[0019] Furthermore, as a preferred method, the container used for placement is a water-cooled copper crucible.

[0020] As an optional implementation, the current is introduced by tungsten electrode arc ignition melting, with the arc gun suspended above the container holding the raw materials. During melting, the surface metal (Nb, Zr) is first burned, and the surface metal melts into droplets that drip to the bottom of the material pile. The low-melting-point Ag and Ti are melted by preheating and reducing the current.

[0021] Furthermore, there are no special limitations on the container used for the melting process.

[0022] Furthermore, as a preferred method, the melting vessel is a vacuum electric arc furnace.

[0023] Furthermore, the vacuum degree of the vacuum electric arc furnace is 0.5 × 10⁻⁶. 3 ~1×10 3 Pa.

[0024] Furthermore, the number of times the melting process is flipped is 8 to 10.

[0025] Furthermore, in step S1, the cooling is cooling to room temperature.

[0026] Furthermore, the cooling method is circulating water cooling.

[0027] Furthermore, the container for suction casting is a water-cooled copper mold.

[0028] Furthermore, the wall thickness of the water-cooled copper mold is 23~27 mm.

[0029] Furthermore, the interior of the water-cooled copper mold is circulated with cooling water.

[0030] Preferably, the temperature of the circulating cooling water is 15~25℃.

[0031] More preferably, the flow rate of the circulating cooling water is 2.5~3.5 L / min.

[0032] As an optional implementation, the alloy plate has dimensions of (5~9)×(4~8)×(60~80) mm. 3 .

[0033] Furthermore, the annealing is a homogenization annealing.

[0034] Furthermore, the annealing temperature is 1150~1250 ℃.

[0035] Furthermore, the annealing time is 1 to 5 hours. Within this time range, not only can grain growth be suppressed and overheating defects be eliminated, but dendritic segregation can also be completely eliminated, allowing the alloy structure to reach an ideal uniform state, laying a good microstructure foundation for subsequent rolling, aging and other processes.

[0036] Furthermore, the annealing time is 1.5 to 2.5 hours.

[0037] Furthermore, the annealing heating rate is 5~15 °C / min.

[0038] Furthermore, in step S2, the cooling is cooling to room temperature.

[0039] Furthermore, the cooling method is ice-water quenching. The rapid cooling effect of ice-water quenching can suppress the evolution of the microstructure and the initiation of defects during the cooling process, stably retain the amplitude-modulated decomposition microstructure of the alloy, and thus improve the plastic deformation capacity of the material while ensuring the strength and hardness of the alloy.

[0040] In this invention, the total deformation is controlled within the range of 80% to 85%, which can not only make the grains obtain uniform and appropriate deformation, avoiding grain damage and microcrack defects, but also maximize the deformation strengthening effect and steadily improve the comprehensive mechanical properties of the alloy.

[0041] Furthermore, the aging treatment temperature is 625~675 ℃.

[0042] Furthermore, the aging treatment time is 1-5 hours. Within this time range, it ensures the normal progress of amplitude modulation decomposition while effectively curbing grain coarsening; simultaneously, it avoids excessive precipitation of the α phase and ensures sufficient release of residual internal stress. The alloy not only has stable elastic modulus parameters and sufficient softening, but also possesses good plasticity, providing an ideal microstructure and performance basis for subsequent rolling processing and finished product use.

[0043] Furthermore, the aging process takes 1.5 to 2.5 hours.

[0044] Furthermore, the heating rate of the aging treatment is 5~15 ℃ / min.

[0045] In this invention, the alloy is subjected to aging treatment after cold rolling. This process eliminates residual internal stress and promotes microstructural recovery and amplitude degradation. Rapid water cooling to room temperature then prevents various structural defects and stably preserves the amplitude degradation microstructure. Ultimately, the alloy maintains its original strength and hardness while effectively enhancing its plastic deformation capacity.

[0046] This invention protects the Zr-Nb-Ti-Ag alloy prepared by the above preparation method.

[0047] This invention protects the application of the above-mentioned Zr-Nb-Ti-Ag alloy in the preparation of medical implant materials.

[0048] Furthermore, the medical implant material includes bone implant material and / or dental implant material.

[0049] Furthermore, the medical implant material is a bone implant material.

[0050] This invention protects a medical implant material made from raw materials including the aforementioned Zr-Nb-Ti-Ag alloy.

[0051] Compared with the prior art, the present invention has the following beneficial effects: This invention provides a method for preparing a Zr-Nb-Ti-Ag alloy, comprising the following steps: Under a specific ratio, Ag metal ingots coated with Ti foil, Ti metal ingots, Zr metal ingots, and Nb metal ingots are stacked sequentially from bottom to top. First, Zr and Nb are melted under a specific current to form a liquid phase, which then coats solid Ti and Ag. Subsequently, the current is reduced to melt Ti and Ag. After tumbling and melting, the mixture is cooled and then vacuum-cast to obtain an alloy sheet. The alloy sheet is then subjected to annealing, cold rolling, and aging treatments to obtain the Zr-Nb-Ti-Ag alloy. This alloy possesses excellent plasticity, low elastic modulus, high yield strength, and good antibacterial properties, meeting the requirements for clinical use and industrial production of modern implantable devices. Attached Figure Description

[0052] Figure 1 The XRD patterns of the Zr-Nb-Ti-Ag alloy prepared in Example 1 are shown in the suction casting state and the aging state.

[0053] Figure 2 The image shows a backscattered SEM image of the Zr-Nb-Ti-Ag alloy prepared in Example 1 in the absorbent casting state.

[0054] Figure 3 The image shows the TEM-EDS image of the Zr-Nb-Ti-Ag alloy prepared in Example 1 under aging treatment.

[0055] Figure 4The figures show the tensile stress-strain curves of the Zr-Nb-Ti-Ag alloy prepared in Example 1 in the suction casting state and after aging treatment.

[0056] Figure 5 The tensile stress-strain curve of the Ti-30Nb-5Zr-6Ag alloy prepared in Comparative Example 18 after aging treatment is shown.

[0057] Figure 6 This is a summary diagram of the relative cell activity of Zr-Nb-Ti-Ag alloys prepared in Examples 1-3 and Comparative Examples 1-3 against MC3T3-E1 mouse osteoblasts.

[0058] Figure 7 The bar chart summarizes the antibacterial rates of the Zr-Nb-Ti-Ag alloys prepared in Examples 1-3 and Comparative Examples 1-3 against Staphylococcus aureus. Detailed Implementation

[0059] The present invention will be further described below with reference to the accompanying drawings and specific embodiments, but the embodiments do not limit the present invention in any way. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in this technical field.

[0060] Unless otherwise specified, all reagents and materials used in the following examples are commercially available.

[0061] Ag: 99.5% purity, produced by Beijing Licheng Chuangxin Metal Materials Technology Co., Ltd. Ti: 99.5% purity, produced by Beijing Licheng Chuangxin Metal Materials Technology Co., Ltd. Zr: 99.5% purity, produced by Beijing Licheng Chuangxin Metal Materials Technology Co., Ltd. Nb: 99.5% purity, produced by Beijing Licheng Chuangxin Metal Materials Technology Co., Ltd.

[0062] Figure 3 (a) indicates Figure 3 Figure (a) in the middle, Figure 3 (b) indicates Figure 3 The order of the other figures follows the same pattern as in figure (b).

[0063] Example 1: Preparation of a Zr-Nb-Ti-Ag alloy S1. Evacuate the furnace body of the vacuum electric arc furnace to a vacuum degree ≤1×10⁻⁶. 3The pressure was increased to Pa, and then argon gas (purity ≥99.5%) was introduced. The vacuuming and argon-filling process was repeated three times until the reaction vessel was completely filled with argon. Under argon protection, the raw materials were weighed out according to the atomic percentages of Ag, Ti, Zr, and Nb as 3%:9%:53%:35%, totaling 40 g of raw materials. Ag metal ingots were coated with Ti foil with a thickness of 0.2 mm. The coated Ag metal ingots, the remaining Ti metal ingots, Zr metal ingots, and Nb metal ingots were then stacked sequentially from bottom to top in a water-cooled copper crucible. Tungsten electrode arc melting was used, with the arc gun suspended above the crucible. First, Zr and Nb were melted at a current of 250 A to form a liquid phase and coat the solid Ti and Ag. Then, the current was reduced to 200 A to completely melt Ti and Ag. After repeated melting eight times, the mixture was then cast into a water-cooled copper utensil (25 mm thick, with circulating cooling water at a temperature of 20°C). At a temperature of ℃ and a flow rate of 2.8 L / min, the dimensions were 7×6×70 mm. 3 Alloy sheet metal; S2. The alloy sheet obtained in step S1 is placed in a vacuum tube furnace. After evacuation, nitrogen is introduced as a protective atmosphere. The temperature is raised to 1200℃ at a rate of 10℃ / min and held for 2 hours for homogenization annealing. Then, it is water-quenched and cooled to room temperature. The homogenized sheet is then rolled on a small two-roll mill. The reduction in rolling pressure per pass is 16%. Rolling is stopped when the deformation of the sheet reaches 80%. After five repeated rolling passes, an alloy sheet with a final thickness of about 0.5 mm is obtained. The rolled sheet is then placed back into the vacuum tube furnace and heated to 650℃ at a rate of 10℃ / min under a nitrogen atmosphere. It is held for 2 hours for aging treatment and then water-quenched and cooled to room temperature to obtain the Zr-Nb-Ti-Ag alloy, denoted as ZNTAg. 3.0 alloy.

[0064] Example 2: Preparation of a Zr-Nb-Ti-Ag alloy The difference from Example 1 is that in step S1, the atomic percentages of Ag, Ti, Zr, and Nb are adjusted from 3%:9%:53%:35% to 2%:9.34%:53.33%:35.33%, thus obtaining a Zr-Nb-Ti-Ag alloy, denoted as ZNTAg. 2.0 alloy.

[0065] The other steps and conditions are the same as in Example 1.

[0066] Example 3: Preparation of a Zr-Nb-Ti-Ag alloy The difference from Example 1 is that in step S1, the atomic percentages of Ag, Ti, Zr, and Nb are adjusted from 3%:9%:53%:35% to 1.5%:9.5%:53.5%:35.5%, thus obtaining a Zr-Nb-Ti-Ag alloy, denoted as ZNTAg. 1.5 alloy.

[0067] The other steps and conditions are the same as in Example 1.

[0068] Comparative Example 1: Preparation of a Zr-Nb-Ti-Ag alloy The difference from Example 1 is that in step S1, the atomic percentages of Ag, Ti, Zr, and Nb are adjusted from 3%:9%:53%:35% to 1%:9.66%:53.67%:35.67%, thus obtaining a Zr-Nb-Ti-Ag alloy, denoted as ZNTAg. 1.0 alloy.

[0069] The other steps and conditions are the same as in Example 1.

[0070] Comparative Example 2: Preparation of a Zr-Nb-Ti-Ag alloy The difference from Example 1 is that in step S1, the atomic percentages of Ag, Ti, Zr, and Nb are adjusted from 3%:9%:53%:35% to 0.5%:9.83%:53.83%:35.84%, thus obtaining a Zr-Nb-Ti-Ag alloy, denoted as ZNTAg. 0.5 alloy.

[0071] The other steps and conditions are the same as in Example 1.

[0072] Comparative Example 3: Preparation of a Zr-Nb-Ti-Ag Alloy The difference from Example 1 is that in step S1, Ag is not added, that is, the atomic percentages of Ag, Ti, Zr and Nb are replaced from 3%:9%:53%:35% to 0%:10%:54%:36%, thus obtaining the Zr-Nb-Ti-Ag alloy, denoted as ZNTAg0 alloy.

[0073] The other steps and conditions are the same as in Example 1.

[0074] Comparative Example 4: Preparation of a Zr-Nb-Ti-Ag alloy The difference from Example 1 is that in step S1, the mass ratio of Ag, Ti, Zr, and Nb is adjusted from the atomic percentage of 3% and 9%:53%:35% to 5%:8.33%:52.33%:34.34%, thus obtaining a Zr-Nb-Ti-Ag alloy, denoted as ZNTAg. 5.0 alloy.

[0075] The other steps and conditions are the same as in Example 1.

[0076] Experimental Results: Following step S2, the homogenized sheet was rolled using a small twin-roll mill. When the rolling deformation reached 16%, large-area cracking occurred in the sheet, making further testing impossible.

[0077] Comparative Example 5: Preparation of a Zr-Nb-Ti-Ag Alloy The difference from Example 1 is that, in step S1, Ti foil was not used to coat the Ag metal ingot. The specific operation is as follows: S1. Under argon protection, the raw materials are prepared according to the mass ratio of Ag, Ti, Zr and Nb as atomic percentages of 3%, 9%, 53% and 35%, respectively, and a total of 40 g of raw materials are weighed. Then, Ag metal ingots, Ti metal ingots, Zr metal ingots and Nb metal ingots are stacked in sequence in a water-cooled copper crucible. Melting is carried out by tungsten electrode arc ignition, with the arc gun suspended above the crucible and a current of 250 A applied.

[0078] The specific steps and conditions are consistent with those in Example 1.

[0079] Experimental Results: When Zr and Nb began to melt, a large amount of white smoke was generated in the furnace, and the Ag ingot at the bottom underwent violent volatilization, causing severe contamination of the melting chamber and making it impossible to continue the experiment. After the current was cut off and the furnace was cooled to room temperature, a layer of Ag powder was found adhering to the inner wall of the melting furnace. The reason for this problem is that the melting points of the four metals Zr, Nb, Ti, and Ag are significantly different. During the melting and heating process, when the system temperature reached the boiling point of silver, the Zr and Nb particles were still not completely melted, ultimately leading to the failure of this melting experiment to be completed normally.

[0080] Comparative Example 6: Preparation of a Zr-Nb-Ti-Ag Alloy The difference from Example 1 is that in step S1, the thickness of the Ti foil is replaced by 0.05 mm instead of 0.2 mm.

[0081] The specific steps and conditions are consistent with those in Example 1.

[0082] Experimental results: Due to the excessively thin thickness of the Ti foil, the encapsulated Ag metal ingot melted prematurely and underwent violent volatilization during the smelting process, resulting in severe contamination of the smelting chamber and making it impossible to continue the experiment. After the current was cut off and the furnace was cooled to room temperature, a layer of Ag powder was still adhered to the inner wall of the smelting furnace.

[0083] Comparative Example 7: Preparation of a Zr-Nb-Ti-Ag Alloy The difference from Example 1 is that in step S1, the thickness of the Ti foil is replaced by 0.4 mm instead of 0.2 mm.

[0084] The specific steps and conditions are consistent with those in Example 1.

[0085] Experimental results: Due to the excessive thickness of the Ti foil, it is difficult to achieve plastic deformation and thus it is difficult to completely wrap the Ag ingot. This will still cause the exposed Ag ingot to melt prematurely due to heat and undergo violent volatilization.

[0086] Comparative Example 8: Preparation of a Zr-Nb-Ti-Ag Alloy The difference from Example 1 is that in step S2, the number of rolling cycles is changed from 5 to 6, that is, the deformation of the sheet is adjusted from 80% to 96%.

[0087] The other steps and conditions are the same as in Example 1.

[0088] Experimental results: After more than five rolling passes, the rolling effect rapidly diminished, microcracks appeared on the sample surface, and it became difficult to continue rolling. Simultaneously, due to the large cumulative deformation, the sample thickness decreased significantly, resulting in a size effect, making subsequent experiments impossible.

[0089] Comparative Example 9: Preparation of a Zr-Nb-Ti-Ag Alloy The difference from Example 1 is that in step S2, the single-blade rolling pressure is changed from 16% to 8%.

[0090] The other steps and conditions are the same as in Example 1.

[0091] Experimental results: Insufficient pressure in single-pass rolling leads to insufficient overall plastic deformation of the material, almost no effective plastic deformation in the core, and severe uneven grain breakage along the thickness direction, which in turn causes stratification of mechanical properties in the thickness direction of the alloy, failure of amplitude modulation decomposition microstructure control, and disordered distribution of internal residual stress.

[0092] Comparative Example 10: Preparation of a Zr-Nb-Ti-Ag Alloy The difference from Example 1 is that in step S2, the single-blade rolling pressure is adjusted from 16% to 20%.

[0093] The other steps and conditions are the same as in Example 1.

[0094] Experimental results: The single-blade rolling pressure was too large, and the sample cracked after three rolling passes, making it impossible to continue the subsequent test.

[0095] Comparative Example 11: Preparation of a Zr-Nb-Ti-Ag alloy The difference from Example 1 is that in step S2, the rolling temperature is changed from room temperature to 900 °C.

[0096] The other steps and conditions are the same as in Example 1.

[0097] Experimental results: When the cumulative deformation of the plate reached about 30%, obvious cracks appeared on the surface, and subsequent tests could not be carried out.

[0098] Comparative Example 12: Preparation of a Zr-Nb-Ti-Ag Alloy The difference from Example 1 is that in step S1, the current is adjusted from 250 A to 150 A.

[0099] The other steps and conditions are the same as in Example 1.

[0100] Experimental results: The melting current was too low, failing to allow the Nb and Zr particles to be slowly heated and fully melted. Unmelted Nb and Zr hard particles easily remained in the alloy, resulting in uneven ingot microstructure and composition distribution. If the heating time was extended or the temperature was further increased to melt the high-melting-point components, a large amount of low-boiling-point Ag would volatilize, not only contaminating the furnace cavity but also causing the final alloy composition to deviate significantly from the design value, making it impossible to obtain a qualified ingot.

[0101] Comparative Example 13: Preparation of a Zr-Nb-Ti-Ag Alloy The difference from Example 1 is that in step S1, the current is adjusted from 250 A to 350 A.

[0102] The other steps and conditions are the same as in Example 1.

[0103] Experimental results: Excessive melting current causes simultaneous melting of various metal particles and rapid vaporization and volatilization of Ag components, resulting not only in raw material quality loss but also in the generation of white smoke and contamination of the melting chamber. Due to the loss of Ag components through volatilization, the alloy composition becomes uncontrolled, easily leading to structural defects and compositional inhomogeneity within the ingot. Consequently, the plasticity of the billet deteriorates, making subsequent rolling processes prone to cracking, deformation, and failure, thus hindering the production of alloy plates with intact morphology.

[0104] Comparative Example 14: Preparation of a Zr-Nb-Ti-Ag Alloy The difference from Example 1 is that in step S2, the homogenization temperature is adjusted from 1200 °C to 900 °C.

[0105] The other steps and conditions are the same as in Example 1.

[0106] Experimental results: Insufficient homogenization temperature prevented complete elimination of dendritic segregation, resulting in poor uniformity of the as-cast microstructure. This non-uniform microstructure leads to uneven deformation during rolling, exacerbates localized stress concentration, and easily generates microcracks or even full-blown cracks, hindering the successful completion of the rolling process.

[0107] Comparative Example 15: Preparation of a Zr-Nb-Ti-Ag Alloy The difference from Example 1 is that in step S2, the homogenization temperature is adjusted from 1200 °C to 1400 °C.

[0108] The other steps and conditions are the same as in Example 1.

[0109] Experimental results: A high homogenization temperature can easily lead to abnormal growth of recrystallized grains, and may even cause the alloy to overheat. Such structural defects will severely degrade the cold working properties of the alloy, significantly reduce its deformation capacity, and make it prone to cracking in subsequent rolling processes, making it impossible to process into qualified plates.

[0110] Comparative Example 16: Preparation of a Zr-Nb-Ti-Ag Alloy The difference from Example 1 is that in step S2, the aging treatment temperature is adjusted from 650 °C to 500 °C.

[0111] The other steps and conditions are the same as in Example 1.

[0112] Experimental results: When the aging temperature is too low, the alloy not only precipitates a large amount of α phase, but also retains high residual internal stress, resulting in poor mechanical properties.

[0113] Comparative Example 17: Preparation of a Zr-Nb-Ti-Ag Alloy The difference from Example 1 is that in step S2, the aging treatment temperature is adjusted from 650 °C to 800 °C.

[0114] The other steps and conditions are the same as in Example 1.

[0115] Experimental results: When the aging temperature is too high, the alloy is difficult to undergo amplitude decomposition and may even cause abnormal growth of recrystallized grains. The microstructure loses the fine structure corresponding to amplitude decomposition, and the grain size increases, resulting in poor cold working performance of the alloy. Problems such as cracking and uneven deformation occur during rolling, making it impossible to produce qualified plates.

[0116] Comparative Example 18: Preparation of a Zr-Nb-Ti-Ag Alloy The Ti-30Nb-5Zr-6Ag alloy was prepared according to the steps of Example 4 of Chinese Patent Application CN109022853A. The alloy has an elastic modulus of 49.5 GPa, a compressive strength of 1140 MPa, and an antibacterial rate of 95%. It achieves a good balance between low elastic modulus, excellent antibacterial properties, and excellent mechanical strength, making it the alloy system with the best comprehensive performance in this patent.

[0117] Experimental Example 1: Structural Characterization Test of Zr-Nb-Ti-Ag Alloy Pretreatment: Take the aged Zr-Nb-Ti-Ag alloy sample obtained in Example 1, and polish it with SiC metallographic sandpaper from 400# to 2000# in stages. After cleaning and drying, it is ready for use.

[0118] 1. X-ray diffraction characterization The Zr-Nb-Ti-Ag alloy prepared in Example 1 was characterized by X-ray diffraction (XRD) in both the suction-cast and aged states using a Smart Lab XRD instrument. The test results are as follows: Figure 1 As shown. The alloy matrix phase in both states is the β phase, with the suction-cast ZNTAg... 3.0 The alloy exhibits only a single β-BCC phase diffraction peak, while the aged ZNTAg... 3.0 The appearance of sideband peaks in the alloy diffraction peaks indicates that the alloy underwent amplitude modulation decomposition, with the original β-phase diffraction peaks undergoing significant splitting, ultimately differentiating into a two-phase amplitude modulation heterostructure of β1 and β2. This not only verifies the effectiveness of the microstructure control of the aging process in this invention, but also provides experimental evidence at the phase level for the excellent mechanical properties of the alloy.

[0119] 2. Scanning electron microscopy characterization The Zr-Nb-Ti-Ag absorbent-cast alloy prepared in Example 1 was characterized by expanded backscattered scanning electron microscopy (BSE-SEM) using a TESCAN MIRA 4 SEM instrument. The test results are as follows: Figure 2 As shown, the alloy consists of uniformly sized equiaxed β phases with nanoscale amplitude-modulated compositional fluctuations within the grains. There are no α phases or intermetallic compounds precipitated, the grain boundaries are clear and continuous, and the overall microstructure is highly homogeneous.

[0120] 3. Transmission electron microscopy-energy dispersive spectroscopy characterization The Zr-Nb-Ti-Ag alloy in the aged state of Example 1 was characterized by transmission electron microscopy-energy dispersive spectroscopy (TEM-EDS) using a JEM-2100F field emission TEM instrument. The results are as follows: Figure 3 As shown. By Figure 3 (a) It is evident that a periodically alternating light and dark stripe structure was formed in the alloy matrix, which is a typical morphological feature of amplitude modulation decomposition, confirming that the alloy underwent significant amplitude modulation decomposition after aging; combined with Figure 3 (b) ~ Figure 3 The EDS elemental distribution results in (e) further confirm that the bright contrast region is a β1-BCC phase rich in Zr and Ag, and a β2-BCC phase rich in Nb and Ti.

[0121] The aforementioned X-ray diffraction, scanning electron microscopy, and transmission electron microscopy-energy dispersive spectroscopy characterizations, from phase and morphology to elemental distribution, mutually corroborate each other, jointly confirming that the Zr-Nb-Ti-Ag alloy of this invention exhibits a uniform, single-phase supersaturated β-BCC microstructure without brittle precipitates in its absorbent casting state. After aging, typical amplitude modulation decomposition occurs, forming a nanoscale amplitude modulation heterostructure with periodically alternating Zr and Ag-rich β1 phase and Nb and Ti-rich β2 phase. The low-modulus β1 soft phase guides the ordered movement of dislocations, maintains the alloy's intrinsic low elastic modulus, and improves deformation uniformity. The hard β2 phase, as a reinforcing phase, acts as a barrier during dislocation slip, inhibiting continuous dislocation movement and enhancing the alloy's yield strength. The amplitude modulation heterostructure interface transforms plane slip, which easily induces stress concentration, into cross-slip, further optimizing deformation compatibility. This unique amplitude modulation heterostructure provides the microstructural basis for the alloy to synergistically achieve low elastic modulus, excellent plasticity, and high strength.

[0122] Experimental Example 2: Performance Testing of Zr-Nb-Ti-Ag Alloy 1. Mechanical properties (1) Experimental methods Yield strength (YS) and elastic modulus (E): Uniaxial tensile tests were conducted on the above alloy specimens at room temperature using an AW-1000 universal tensile testing machine. The gauge length of the specimens was 8 mm, the width was 2.5 mm, and the thickness was 0.5 mm. The tensile rate was 0.4 mm / min. The yield strength was taken as the stress value corresponding to 0.2% of the plastic strain. The elastic modulus was determined by the slope of the elastic stage of the tensile stress-strain curve. A higher yield strength indicates better resistance to plastic deformation; a lower elastic modulus indicates that it is closer to the elastic modulus of human bone tissue, and the alloy has better biomechanical compatibility.

[0123] Elongation at break (ε): During the uniaxial tensile test, the tensile elongation at break (ε) of each alloy specimen was measured using a strain gauge (model: BSF120-3AA-T) manufactured by Jinan Sigma Technology Co., Ltd. A higher elongation at break indicates better plasticity of the alloy.

[0124] (2) Experimental results Table 1 Performance data of alloys in each embodiment and comparative example

[0125] As shown in Table 1, the Zr-Nb-Ti-Ag alloys of Examples 1-3 all exhibit yield strengths ≥1051 MPa, elastic moduli ≤66 GPa, and elongation at break ≥14.5%, indicating that the Zr-Nb-Ti-Ag alloys of the present invention possess good plasticity, low elastic modulus, and high yield strength. Furthermore, the tensile stress-strain curves of the Zr-Nb-Ti-Ag alloy prepared in Example 1 in the suction-cast state and after aging treatment are shown below. Figure 4 As shown. ZNTAg of Example 1 3.0 After aging treatment, the yield strength and elastic modulus of the alloy were improved compared with the suction-cast alloy, while the fracture elongation did not change significantly. This indicates that amplitude modulation decomposition can improve the yield strength and elastic modulus, while the fracture elongation did not decrease, thus significantly improving the mechanical compatibility of the alloy.

[0126] In contrast, the yield strength of alloys in Comparative Examples 1-3 is significantly reduced, resulting in insufficient mechanical load-bearing capacity and making it difficult to meet the load-bearing mechanical requirements of orthopedic implants. The fracture elongation of alloy in Comparative Example 16 is significantly reduced, while its elastic modulus is excessively high, making it prone to forming a stress shielding effect with human bone tissue, which is detrimental to postoperative osseointegration and long-term implant stability. The tensile stress-strain curve of Comparative Example 18 is shown below. Figure 5 As shown, although its tensile yield strength is as high as nearly 1110 MPa, it breaks immediately after yielding, with a fracture elongation of only 2%, and has almost no plastic deformation capacity. This characteristic not only greatly increases the difficulty of processing and molding and reduces the adaptability to industrial mass production, but also makes it prone to brittle fracture under load after implantation, which cannot meet the safety standards for clinical orthopedic implants.

[0127] 2. Biocompatibility (1) Experimental methods In accordance with ISO 10993-5 standard, the in vitro cell compatibility of Zr-Nb-Ti-Ag alloys prepared in Examples 1-3 and Comparative Examples 1-3 was systematically evaluated using the direct contact method. Mouse pre-osteoblast cells MC3T3-E1 and human osteosarcoma cells MG-63 were used as cell models in the experiment. The specific steps are as follows: S1. Sample pretreatment: The Zr-Nb-Ti-Ag alloys prepared in Examples 1-3 and Comparative Examples 1-3 were processed into circular samples with a diameter of 8 mm and a thickness of 0.4 mm. They were polished with SiC metallographic sandpaper to 2000#. The surface impurities were removed by ultrasonic cleaning with anhydrous ethanol and 75% medical ethanol in sequence. Then, they were sterilized in an autoclave at 121 ℃ for 20 min. After cooling, they were transferred to the bottom of a 48-well cell culture plate under sterile conditions for later use. S2. Cell Culture and Seeding: Cells were passaged in α-essential medium (α-MEM) supplemented with 10% fetal bovine serum and 1% penicillin-streptomycin antibiotics at a constant temperature of 37 ℃, 95% relative humidity, and 5% CO2. Cells in the logarithmic growth phase were digested with trypsin, resuspended, and the cell density was adjusted to 3 × 10⁶ cells / mL. 4Cells / mL were inoculated into 48-well plates containing alloy samples at a seeding rate of 1 mL per well. Simultaneously, a control group was set up with culture wells containing only an equal amount of cells and no alloy samples, and a zeroing group was set up with cell-free wells containing only complete culture medium. Each group had 3 parallel replicates. S3. Cell viability assay: The culture plates were incubated at 37 ℃, 5% CO2, and saturated humidity for 1 day and 3 days, respectively. After reaching the preset incubation time, the original culture medium in each well was discarded, and each well was gently washed 3 times with phosphate-buffered saline (PBS). 100 μL of fresh complete culture medium containing 10% (v / v) CCK-8 reagent was added to each well, and the plates were returned to the incubator for 2 h in the dark. After incubation, the supernatant from each well was transferred to a 96-well plate, and the absorbance (OD) at 450 nm was measured using a microplate reader (TECAN, model: SPARK10M). 450 ); Relative cell viability calculation: The relative cell viability of each group of samples was calculated using the following formula: Relative cell viability (%) = (experimental group OD) 450 - Zeroing group OD 450 ) / (control group OD 450 - Zeroing group OD 450 ) × 100%.

[0128] (2) Experimental results like Figure 6 As shown, the cell viability on the surface of the alloy samples in the above embodiments and comparative examples is higher than 95%, proving that this series of alloys has no obvious cytotoxicity and has excellent biocompatibility.

[0129] 3. Antibacterial properties (1) Experimental methods Selected Escherichia coli ( E. coli ) and Staphylococcus aureus ( S.aureus The in vitro antibacterial properties of the Zr-Nb-Ti-Ag alloy samples prepared in Examples 1-3 and Comparative Examples 1-3 were systematically evaluated using the plate colony counting method, with the test strain being the test strain.

[0130] Before the experiment, all the above alloy samples were autoclaved at 121 ℃ for 20 min and then placed on sterile agar plates. LB liquid culture medium was then used for activation overnight at 37 ℃, and the concentration was adjusted to 1×10⁻⁶. 5 A bacterial suspension of CFU / mL was prepared, with 50 μL evenly added and spread onto the sample surface. After incubation at 37 ℃ for 20 h, the number of colonies was counted and recorded. A blank agar plate without the sample was simultaneously set up as a control group. Each group had three replicates. The bacterial morphology on the sample surface was observed using scanning electron microscopy (SEM): a bacterial suspension of 1×10⁻⁶ CFU / mL was prepared. 5CFU / mL bacterial suspension was added dropwise to the surface of the sterilized sample. After incubation at 37 °C for 24 h, the sample was removed and fixed in 2.5% glutaraldehyde solution pre-cooled to 4 °C for 12 h. After rinsing with PBS buffer to remove residual fixative, the sample was sequentially dehydrated with 30%, 50%, 70%, 80%, 90%, and 100% ethanol solutions, with each dehydration stage lasting 10 min. After drying, the sample surface was observed and analyzed using SEM. E. coli and S. aureus The morphology of the bacterial cells.

[0131] (2) Experimental results like Figure 7 As shown, the Zr-Nb-Ti-Ag alloys prepared in Examples 1-3 all exhibited antibacterial rates ≥90%, with Example 1 showing an antibacterial rate of 97%, Example 2 showing an antibacterial rate of 93%, and Example 3 showing an antibacterial rate of 90%. This demonstrates that the Zr-Nb-Ti-Ag alloys prepared in Example 1 exhibited antibacterial rates ≥90%. 3.0 The alloy exhibits the best antibacterial properties.

[0132] In contrast, the antibacterial rates of the Zr-Nb-Ti-Ag alloys prepared in Comparative Examples 1 to 3 decreased significantly: the antibacterial rate of Comparative Example 1 was 56%, the antibacterial rate of Comparative Example 2 was 22%, and the antibacterial rate of Comparative Example 3 was 6%. None of the above comparative alloys could meet the standard of ≥90% antibacterial rate for clinical medical biomaterials in GB / T 4789.2-2010.

[0133] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.

Claims

1. A method for producing a Zr-Nb-Ti-Ag alloy, characterized by, Comprising the following steps: S1. Under a protective gas atmosphere, stack the Ag metal ingot coated with Ti foil, Ti metal ingot, Zr metal ingot and Nb metal ingot in turn from bottom to top, melt Zr and Nb to form a liquid phase and coat solid Ti and Ag at 250-280 A, then reduce the current to 180-220 A to completely melt Ti and Ag, perform a turnover smelting, and after cooling, suction casting to obtain an alloy plate; S2. Anneal the alloy plate obtained in step S1 at 1100-1300 ℃, cool, cold roll, and roll to a plate deformation of 80-85%, then perform aging treatment on the rolled plate at 600-700 ℃, cool, and obtain a Zr-Nb-Ti-Ag alloy; The atomic percentage of Ag, Ti, Zr and Nb is (1.3-3.2):(8-10):(52-54):(34-36). The single pass reduction is controlled to be 14-17% during cold rolling. The thickness of the Ti foil is 0.15-0.25 mm.

2. The method of claim 1, wherein, The annealing temperature is 1150-1250 ℃.

3. The preparation method according to claim 1, characterized in that, The aging treatment temperature is 625-675 ℃.

4. The preparation method according to claim 1, characterized in that, The atomic percentage of Ag, Ti, Zr and Nb is (1.5-3):(8.8-9.8):(52.8-53.8):(34.8-35.8).

5. The method of claim 1, wherein the step of forming the first and second layers is performed by a process selected from the group consisting of: sputtering, evaporation, and chemical vapor deposition. The annealing time is 1-5 h.

6. The method of claim 1, wherein the step of forming the first and second layers is performed by a process selected from the group consisting of: sputtering, evaporation, and chemical vapor deposition. The aging treatment time is 1-5 h.

7. The method of claim 1, wherein the step of forming the first and second layers is performed by a process selected from the group consisting of: sputtering, evaporation, and chemical vapor deposition. The turnover smelting is performed 8-10 times.

8. The Zr-Nb-Ti-Ag alloy prepared by the preparation method of any one of claims 1-7.

9. The use of the Zr-Nb-Ti-Ag alloy of claim 8 in preparing a medical implant material.

10. A medical implant material, characterized by The medical implant material is prepared from raw materials comprising the Zr-Nb-Ti-Ag alloy of claim 8.

Citation Information

Patent Citations

  • Preparation method of antibacterial Ti-Nb-Zr-Ag alloy ingot

    CN109022853A