A composite seed layer material, a solar cell and its preparation method

By using CuNiX ternary alloy as the composite seed layer material, the problems of high cost of silver-containing seed layers and easy oxidation of copper-containing seed layers have been solved, realizing low-cost and high-efficiency solar cell production, simplifying the process and maintaining cell conversion efficiency.

CN123108355APending Publication Date: 2026-11-17DONGFANG HUANSHENG PHOTOVOLTAIC (JIANGSU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611264552.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-19
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing back-contact solar cells, silver-containing seed layers are costly, while copper-containing seed layers are prone to diffusion and oxidation, affecting long-term reliability.

Method used

A CuNiX ternary alloy is used as the composite seed layer material, comprising 70%~94.5% Cu, 5%~25% Ni, and the balance being at least one of Cr, Mn, Al, and Ti. This forms a first and second seed layer with alternating P-type and N-type doped regions in contact. The seed layer contacts the doped regions through contact windows, forming a NiSix diffusion barrier layer and a self-passivating oxide layer to prevent copper diffusion and oxidation.

Benefits of technology

It reduced material costs, prevented seed layer oxidation, maintained or improved battery conversion efficiency, simplified the process, and reduced metallization costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108355A_ABST
    Figure CN123108355A_ABST
Patent Text Reader

Abstract

This invention discloses a composite seed layer material, a solar cell, and a method for preparing the same, belonging to the field of solar cell technology. The composite seed layer material comprises a CuNiX ternary alloy, where X includes at least one of Cr, Mn, Al, and Ti, and X is not Ag. By using a silver-free CuNiX alloy instead of a pure silver seed layer, the material cost can be reduced by more than 70%. Furthermore, X is a self-passivating element, allowing a dense oxide layer to spontaneously form on the seed layer surface. This oxide layer film has the characteristics of preventing oxygen diffusion into the interior, controllable thickness, and rapid dissolution in the electroplating solution, eliminating the need for acid pickling and activation before electroplating, simplifying the process, and avoiding the problems of uneven removal of the oxide layer and significant increase in contact resistance on the surface of pure copper seed layers. Solar cells containing the above-mentioned composite seed layer material can maintain a cell conversion efficiency comparable to or even better than that of pure silver.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of solar cell technology, and more specifically, to a composite seed layer material, a solar cell, and a method for preparing the same. Background Technology

[0002] Back-contact solar cells refer to high-efficiency cell structures where both the emitter and base electrodes are located on the back of the cell. Among them, tunneling oxide passivated back-contact (TBC) cells are a new generation of high-efficiency solar cells that combine a back-contact structure with TOPCon passivation contact technology. Currently, most mainstream TBC cells use silver-containing seed layers, which are costly; while copper-containing seed layers suffer from problems such as easy diffusion and oxidation, affecting long-term reliability.

[0003] In view of this, the present invention is proposed. Summary of the Invention

[0004] The purpose of this invention is to provide a composite seed layer material, a solar cell, and a method for preparing the same, so as to solve or improve the above-mentioned technical problems.

[0005] This invention can be implemented as follows: In a first aspect, the present invention provides a composite seed layer material comprising a CuNiX ternary alloy, wherein, by atomic percentage, the CuNiX ternary alloy comprises 70%~94.5% Cu, 5%~25% Ni, and the balance being X; wherein X comprises at least one of Cr, Mn, Al, and Ti, and X is not Ag.

[0006] In a second aspect, the present invention provides a solar cell, the solar cell comprising a silicon substrate, wherein a tunneling oxide layer, a doped polycrystalline silicon layer, a back passivation layer, a composite seed layer and a conductive layer are sequentially stacked on the back side of the silicon substrate. The doped polycrystalline silicon layer includes alternating P-type doped regions and N-type doped regions; The back passivation layer has a contact window; The composite seed layer is formed from the composite seed layer material of the aforementioned embodiments; the composite seed layer includes a first seed layer and a second seed layer, wherein the first seed layer is in contact with the P-type doped region through a contact window, and the second seed layer is in contact with the N-type doped region through a contact window.

[0007] In an optional implementation, the first seed layer has at least one of the following characteristics: Feature 1: In the first seed layer, the Ni content is 12%~25%, and the X content is 1%~4%; Feature 2: The thickness of the first seed layer is 80nm~120nm; Feature 3: The first seed layer includes a first diffusion barrier layer, a first alloy body layer, and a first self-passivating oxide layer, which are sequentially disposed from the direction closest to the silicon substrate to the direction furthest from the silicon substrate; The first alloy body layer is composed of a CuNiX ternary alloy; the first diffusion barrier layer is formed in situ by Ni in the first alloy body layer and Si in the P-type doped region using NiSi. x Composition: The first self-passivating oxide layer is composed of oxides formed from X in the first alloy body layer.

[0008] In an optional implementation, the first diffusion barrier layer has a dense crystalline structure.

[0009] In an optional implementation, the thickness of the first diffusion barrier layer is 2 nm to 8 nm.

[0010] In an optional embodiment, the thickness of the first self-passivating oxide layer is 2 nm to 10 nm.

[0011] In an optional implementation, the second seed layer has at least one of the following characteristics: Feature 4: In the second seed layer, the Ni content is 5%~12%, and the X content is 0.5%~3%; Feature 5: The thickness of the second seed layer is 60nm~100nm; Feature 6: The second seed layer includes a second diffusion barrier layer, a second alloy body layer, and a second self-passivating oxide layer, which are sequentially disposed from the direction closest to the silicon substrate to the direction furthest from the silicon substrate; The second alloy body layer is composed of a CuNiX ternary alloy; the second diffusion barrier layer is formed in situ by NiSi from the Ni in the second alloy body layer and Si in the N-type doped region. x Composition: The second self-passivating oxide layer is composed of oxides formed by X in the second alloy body layer.

[0012] In an optional implementation, the thickness of the second diffusion barrier layer is 2 nm to 8 nm.

[0013] In an optional embodiment, the thickness of the second self-passivating oxide layer is 2 nm to 10 nm.

[0014] In an optional embodiment, the solar cell also has at least one of the following features: Feature 7: The thickness of the tunneling oxide layer is 1nm~2nm; Feature 8: The thickness of the doped polycrystalline silicon layer is 100nm~200nm; Feature 9: The back passivation layer includes an Al2O3 layer with a thickness of 3nm~10nm and a SiN layer with a thickness of 50nm~100nm. x layer; Feature 10: The thickness of the conductive layer is 5μm~15μm; preferably, the thickness of the conductive layer is 8μm~12μm.

[0015] Thirdly, the present invention provides a method for preparing a solar cell as described in any of the foregoing embodiments, comprising the following steps: sequentially depositing a tunneling oxide layer, a doped polycrystalline silicon layer, a back passivation layer, a composite seed layer, and a conductive layer on the back side of a silicon substrate.

[0016] In an optional embodiment, a tunneling oxide layer and an intrinsic polysilicon layer are sequentially deposited on the back side of the silicon substrate; boron diffusion and phosphorus diffusion are performed in a predetermined region of the intrinsic polysilicon layer to form alternating P-type doped layers and N-type doped layers; a back passivation layer is deposited on the surface of the doped polysilicon layer; a contact window is opened in the region of the back passivation layer corresponding to the P-type doped layer and the N-type doped layer; a composite seed layer is deposited in the contact window; and a conductive layer is electroplated on the surface of the composite seed layer.

[0017] In an optional embodiment, the deposition of the composite seed layer includes: depositing alloy body layers with different Ni contents on the surfaces of the P-type doped region and the N-type doped region, respectively; annealing the silicon substrate with the deposited alloy body layer to allow the Ni in the alloy body layer to react in situ with the Si in the doped layer to form a diffusion barrier layer at the interface; and after annealing, exposing the silicon substrate to an oxygen-containing atmosphere to allow the X element in the alloy body layer to oxidize and form a self-passivating oxide layer. The deposition conditions include: background vacuum level < 5 × 10⁻⁶. -4 Pa, working gas pressure is 0.2Pa~0.8Pa, sputtering power is 100W~500W, deposition temperature is 25℃~150℃, and deposition time is 1min~10min; The annealing temperature is 200℃~400℃, the time is 30s~120s, and the heating rate is 30℃ / s~60℃ / s. The oxygen-containing atmosphere has a temperature of 20℃~30℃, a relative humidity of 40%~60%, and an exposure time of 5min~30min.

[0018] In an optional embodiment, the electroplating solution used for the conductive layer includes 150 g / L to 250 g / L CuSO4·5H2O, 80 g / L to 120 g / L H2SO4, and 40 ppm to 60 ppm Cl. - ; In an optional embodiment, the electroplating conditions include: a current density of 1 ASD to 5 ASD, a temperature of 20°C to 50°C, and a time of 5 min to 15 min. In an optional implementation, a stepped start-up method is adopted in the initial stage of electroplating, gradually increasing the current density from 0 to the set value within 10s to 30s.

[0019] Fourthly, the present invention provides a solar cell module, including the solar cell of any of the foregoing embodiments.

[0020] The beneficial effects of this invention include: The composite seed layer material provided by the present invention includes a CuNiX ternary alloy. By atomic percentage, the CuNiX ternary alloy includes 70%~94.5% Cu, 5%~25% Ni, and the balance is X; wherein X includes at least one of Cr, Mn, Al, and Ti, and X is not Ag.

[0021] Using the aforementioned CuNiX ternary alloy as a seed layer material, instead of traditional pure silver or silver-containing pastes, can significantly reduce costs. Furthermore, the Ni contained in the alloy can preferentially react with Si in the doped layer to form NiSi in situ. x A diffusion barrier layer prevents further diffusion of Cu; the X element contained in the alloy can spontaneously form a dense surface oxide layer when the seed layer is exposed to air, preventing further oxidation of the internal copper layer. Therefore, the composite seed layer material provided by this invention not only effectively reduces costs, but also avoids the problems of pure copper or binary alloy seed layers being easily oxidized and requiring additional protective layers or acid pickling activation.

[0022] Solar cells containing the aforementioned composite seed layer material can maintain a cell conversion efficiency comparable to or even better than that of pure silver. Attached Figure Description

[0023] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.

[0024] Figure 1 This is a cross-sectional schematic diagram of the solar cell of the present invention; Figure 2 for Figure 1 A schematic diagram of the structure of the first composite seed layer; Figure 3 for Figure 1 A schematic diagram of the structure of the second composite seed layer.

[0025] Icons: 10-Silicon substrate; 20-Tunneling oxide layer; 30-Doped polycrystalline silicon layer; 31-P-type doped region; 32-N-type doped region; 40-Back passivation layer; 41-Contact window; 50-Composite seed layer; 51-First seed layer; 511-First diffusion barrier layer; 512-First alloy body layer; 513-First self-passivating oxide layer; 52-Second seed layer; 521-Second diffusion barrier layer; 522-Second alloy body layer; 523-Second self-passivating oxide layer; 60-Conductive layer. Detailed Implementation

[0026] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.

[0027] The composite seed layer material, solar cell, and preparation method provided by this invention will be described in detail below.

[0028] The present invention provides a composite seed layer material comprising a CuNiX ternary alloy, wherein the CuNiX ternary alloy comprises 70%~94.5% Cu, 5%~25% Ni, and the balance being X, by atomic percentage; wherein X comprises at least one of Cr, Mn, Al, and Ti, and X is not Ag.

[0029] In some alternative embodiments, the atomic percentage of Cu in the CuNiX ternary alloy can be 70%, 75%, 80%, 85%, 90%, or 94.5%, or other values ​​within the range of 70% to 94.5%. The aforementioned Cu is mainly used to provide electrical conductivity. Setting the atomic percentage of Cu to 70% to 94.5% ensures that the CuNiX ternary alloy has superior electrical conductivity. However, if the Cu content is higher than 94.5%, the content of Ni and X will be diluted accordingly, potentially leading to insufficient diffusion barrier capability and a decrease in self-passivation effect.

[0030] In CuNiX ternary alloys, the atomic percentage of Ni can be 5%, 8%, 10%, 12%, 15%, 18%, 20%, 22%, or 25%, or other values ​​within the range of 5% to 25%. Ni is mainly used to form NiSi in situ with Si in the doped layer. x Diffusion barrier layer. If the Ni content is less than 5%, it is difficult to form a continuous and effective NiSi layer at the interface. x The diffusion barrier layer, copper, is not effective enough in blocking diffusion; if the Ni content is higher than 25%, the resistivity of the alloy increases significantly, and excessive Ni segregation may lead to an increase in interface defects.

[0031] After oxidation, X forms a passivation oxide layer. Within the dosage range provided by this invention, it ensures self-passivation while avoiding adverse effects on the alloy's conductivity. Furthermore, this passivation oxide layer prevents oxygen diffusion inwards, has controllable thickness, and dissolves rapidly in the electroplating solution. This eliminates the need for pre-electroplating acid pickling and activation, simplifying the process and avoiding the problems of uneven removal of the oxide layer on the pure copper seed layer surface and a significant increase in contact resistance.

[0032] Continuing from the above, this invention uses the aforementioned CuNiX ternary alloy as the seed layer material, replacing traditional pure silver or silver-containing pastes, which can significantly reduce costs. Furthermore, the Ni contained in the alloy can preferentially react with Si in the doped layer to form NiSi in situ. x A diffusion barrier layer prevents further diffusion of Cu; the X element contained in the alloy can spontaneously form a dense surface oxide layer when the seed layer is exposed to air, preventing further oxidation of the internal copper layer. Therefore, the composite seed layer material provided by this invention not only effectively reduces costs, but also avoids the problems of pure copper or binary alloy seed layers being easily oxidized and requiring additional protective layers or acid pickling activation.

[0033] Accordingly, the present invention also provides a solar cell, please refer to [link / reference]. Figure 1 The solar cell includes a silicon substrate 10, on the back side of which a tunneling oxide layer 20, a doped polycrystalline silicon layer 30, a back passivation layer 40, a composite seed layer 50 and a conductive layer 60 are sequentially stacked. The doped polysilicon layer 30 includes alternating P-type doped regions 31 and N-type doped regions 32; The back passivation layer 40 has a contact window 41; The composite seed layer 50 is formed from the above-mentioned composite seed layer material; the composite seed layer 50 includes a first seed layer 51 and a second seed layer 52, wherein the first seed layer 51 is in contact with the P-type doped region 31 through the contact window 41, and the second seed layer 52 is in contact with the N-type doped region 32 through the contact window 41.

[0034] In some optional embodiments, the Ni content in the first seed layer 51 is 12%~25%, and the X content is 1%~4%. Exemplarily, the Ni content in the first seed layer 51 can be 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, or 25%, or other values ​​within the range of 12%~25%. The X content can be 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, or 4%, or other values ​​within the range of 1%~4%. The higher Ni content in the first seed layer 51 effectively solves the problem of low-resistance ohmic contacts in the P-type doped polysilicon region 31 due to low hole concentration and high contact barrier, by utilizing the characteristic that Ni forms a lower contact barrier with P-type doped polysilicon. If the Ni content in the first seed layer 51 is less than 12%, it is not conducive to forming a continuous and dense NiSi. x The diffusion barrier layer, while effective, has insufficient copper diffusion barrier properties; a Ni content exceeding 25% is detrimental to controlling the alloy's bulk resistivity, and the NiSi... x If the diffusion barrier layer is too thick, it will increase the series resistance and reduce the battery fill factor. If the content of X in the first seed layer 51 is less than 1%, it is not conducive to the formation of a continuous and dense self-passivating oxide film, and it is difficult to effectively prevent oxygen from diffusing into the interior. If the content of X is higher than 4%, it is not conducive to controlling the thickness of the oxide film, and the electron tunneling conductivity may be affected due to the oxide film being too thick (>10nm), which will increase the contact resistance.

[0035] In some optional embodiments, the Ni content in the second seed layer 52 is 5% to 12%, and the X content is 0.5% to 3%. Exemplarily, the Ni content in the second seed layer 52 can be 5%, 6%, 7%, 8%, 9%, 10%, 11%, or 12%, or other values ​​within the range of 5% to 12%. The X content can be 0.5%, 1%, 1.5%, 2%, 2.5%, or 3%, or other values ​​within the range of 0.5% to 3%. The lower Ni content in this second seed layer 52 utilizes the characteristic that N-type polysilicon is insensitive to Ni content, further reducing contact resistance while ensuring good ohmic contact, and reducing the amount of Ni used, thus lowering material costs. If the Ni content in the second seed layer 52 is less than 5%, it is not conducive to the formation of continuous and dense NiSi. x The diffusion barrier layer is insufficient in copper diffusion barrier effect; the Ni content is higher than 12%, which is not conducive to controlling contact resistance. N-type polysilicon is not sensitive to Ni, and excessive Ni content increases cost and does not benefit performance; if the X content in the second seed layer 52 is lower than 0.5%, it is not conducive to forming a continuous and dense self-passivating oxide film, and it is difficult to effectively block oxygen diffusion into the interior; if the X content is higher than 3%, it is not conducive to controlling the oxide film thickness, the tunneling conductivity decreases, and the contact resistance increases accordingly.

[0036] This invention creatively employs a first seed layer 51 and a second seed layer 52 with different Ni contents to address the different metal contact requirements of the P-type and N-type regions, respectively. Specifically, the P-type region utilizes a high-Ni design, leveraging the low contact barrier formed between Ni and P-type polysilicon to achieve good ohmic contact and avoid the contact difficulties encountered in the prior art for the P-type region. The N-type region utilizes a low-Ni design, taking advantage of the insensitivity of N-type polysilicon to Ni content to further reduce contact resistance.

[0037] In some optional embodiments, the thickness of the composite seed layer 50 can be 30 nm to 150 nm, such as 30 nm, 50 nm, 80 nm, 100 nm, 120 nm, or 150 nm, or other values ​​within the range of 30 nm to 150 nm. By controlling the thickness of the composite seed layer 50 within the above range, it is possible to ensure that the seed layer provides sufficiently low lateral conductivity to provide a uniform current distribution for subsequent copper electroplating, and also to ensure that sufficient Ni atoms diffuse to the interface during annealing to form a continuous and effective NiSi. x Diffusion barrier layer. If the thickness of the composite seed layer 50 is greater than 150 nm, it can easily lead to excessive internal stress in the seed layer, resulting in phenomena such as peeling or cracking.

[0038] In some optional embodiments, the thickness of the first seed layer 51 can be 80nm~120nm, such as 80nm, 90nm, 100nm, 110nm, or 120nm, or other values ​​within the range of 80nm~120nm. The thickness of the second seed layer 52 can be 60nm~100nm, such as 60nm, 70nm, 80nm, 90nm, or 100nm, or other values ​​within the range of 60nm~100nm. The above thicknesses provide sufficient Ni atom reserves for both the P-type and N-type regions, ensuring that continuous and dense NiSi can diffuse to the interface during annealing. x A diffusion barrier layer is used while maintaining good conductivity.

[0039] In some alternative implementations, please refer to Figure 2 The first seed layer 51 includes a first diffusion barrier layer 511, a first alloy body layer 512, and a first self-passivating oxide layer 513, sequentially disposed from near the silicon substrate 10 to away from the silicon substrate 10. The first alloy body layer 512 is composed of a CuNiX ternary alloy, providing a low-resistance conductive path; the first diffusion barrier layer 511 is formed in situ from Ni in the first alloy body layer 512 and Si in the P-type doped region 31 using NiSi. x The structure can prevent copper atoms from diffusing into the interior; the first self-passivating oxide layer 513 is composed of oxides formed by X in the first alloy body layer 512, which can prevent the seed layer from oxidizing before electroplating.

[0040] The aforementioned first diffusion barrier layer 511 is located between the first alloy body layer 512 and the p-type doped layer. During the deposition of the first alloy body layer 512 and subsequent annealing, nickel silicide (NiSi) is generated in situ from Ni atoms and Si atoms. x The first diffusion barrier layer 511 has a dense crystal structure. The thickness of the first diffusion barrier layer 511 can be 2nm to 8nm, such as 2nm, 3nm, 4nm, 5nm, 6nm, 7nm, or 8nm, or other values ​​within the range of 2nm to 8nm. If the thickness of the first diffusion barrier layer 511 is less than 2nm, it is difficult to prevent copper atoms from entering the silicon substrate to form deep-level recombination centers, leading to cell efficiency degradation, and at the same time, discontinuous interface coverage and poor ohmic contact. If the thickness of the second diffusion barrier layer 521 is greater than 8nm, it is not conducive to reducing contact resistance, and NiSi... x The resistivity is higher than that of the alloy body layer. An excessively thick barrier layer will increase the series resistance and reduce the battery fill factor.

[0041] The first alloy body layer 512 is composed of a CuNiX ternary alloy, with Cu serving as the conductive host to provide low body resistance, and Ni in the first alloy body layer 512 being uniformly distributed in the Cu matrix.

[0042] The first self-passivating oxide layer 513 includes at least one of Cr2O3, MnO2, Al2O3, and TiO2. The first self-passivating oxide layer 513 possesses density, self-limiting properties, and electron tunneling conductivity, preventing the oxidation of the first alloy body layer 512. The thickness of the first self-passivating oxide layer 513 can be 2nm to 10nm, such as 2nm, 3nm, 4nm, 5nm, 6nm, 7nm, 8nm, 9nm, or 10nm, or other values ​​within the range of 2nm to 10nm. If the thickness of the first self-passivating oxide layer 513 is less than 2nm, it is difficult to effectively prevent oxygen atoms from diffusing into the interior, the seed layer body is easily oxidized, and the contact resistance increases. If the thickness of the first self-passivating oxide layer 513 is greater than 10nm, uneven oxide layer removal during electroplating can easily cause fluctuations in contact resistance, and the tunneling conductivity decreases.

[0043] In some alternative implementations, please refer to Figure 3 The second seed layer 52 includes a second diffusion barrier layer 521, a second alloy body layer 522, and a second self-passivating oxide layer 523, sequentially disposed from near the silicon substrate 10 to away from the silicon substrate 10. The second alloy body layer 522 is composed of a CuNiX ternary alloy; the second diffusion barrier layer 521 is formed in situ from Ni in the second alloy body layer 522 and Si in the N-type doped region 32 using NiSi. x Composition: The second self-passivating oxide layer 523 is composed of oxides formed from X in the second alloy body layer 522.

[0044] The aforementioned second diffusion barrier layer 521 is located between the second alloy body layer 522 and the N-type doped layer. During the deposition of the second alloy body layer 522 and subsequent annealing, nickel silicide (NiSi) is generated in situ from Ni atoms and Si atoms. x The second diffusion barrier layer 521 can have a thickness of 2nm to 8nm, such as 2nm, 3nm, 4nm, 5nm, 6nm, 7nm or 8nm, or other values ​​within the range of 2nm to 8nm.

[0045] The second alloy body layer 522 is composed of a CuNiX ternary alloy. The low Ni content in this layer structure helps to reduce contact resistance.

[0046] The second self-passivating oxide layer 523 includes at least one of Cr2O3, MnO2, Al2O3, and TiO2. This second self-passivating layer also possesses density, self-limiting properties, and electron tunneling conductivity, preventing the oxidation of the second alloy body layer 522. The thickness of the second self-passivating oxide layer 523 can be 2nm to 10nm, such as 2nm, 3nm, 4nm, 5nm, 6nm, 7nm, 8nm, 9nm, or 10nm, or other values ​​within the range of 2nm to 10nm. Similarly, if the thickness of the second self-passivating oxide layer 523 is less than 2nm, it is difficult to effectively prevent oxygen atoms from diffusing into the interior; if the thickness of the second self-passivating oxide layer 523 is greater than 10nm, it can easily lead to uneven oxide layer removal during electroplating, causing fluctuations in contact resistance.

[0047] In this invention, the composite seed layer 50 is located within the contact window 41 of the back passivation layer 40, filling the contact window 41 and possibly slightly covering the edge of the window of the back passivation layer 40.

[0048] In some alternative embodiments, the thickness of the tunneling oxide layer 20 can be 1 nm to 2 nm, such as 1 nm, 1.5 nm or 2 nm, or other values ​​in the range of 1 nm to 2 nm.

[0049] In some alternative embodiments, the thickness of the doped polysilicon layer 30 can be 100nm to 200nm, such as 100nm, 120nm, 150nm, 180nm or 200nm, or other values ​​in the range of 100nm to 200nm.

[0050] In some optional embodiments, the back passivation layer 40 includes an Al2O3 layer with a thickness of 3 nm to 10 nm and a SiN layer with a thickness of 50 nm to 100 nm. xThe Al2O3 layer can have a thickness of 3nm, 4nm, 5nm, 6nm, 7nm, 8nm, 9nm, or 10nm, or other values ​​within the range of 3nm to 10nm. SiN x The thickness of the layer can be 50nm, 60nm, 70nm, 80nm, 90nm or 100nm, or other values ​​within the range of 50nm to 100nm.

[0051] In some optional embodiments, the conductive layer 60 is a copper conductive layer 60, which can be formed by electroplating. It grows from the surface of the composite seed layer 50, covering the first seed layer 51, the second seed layer 52, and at least a portion of the back surface, forming a dense, flat copper grid. The thickness of the conductive layer 60 can be 5μm to 15μm, such as 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, or 15μm, or other values ​​within the range of 5μm to 15μm. In some preferred embodiments, the thickness of the conductive layer 60 is 8μm to 12μm.

[0052] In some alternative embodiments, the contact resistivity of the P-region seed layer of the solar cell does not exceed 0.45 mΩ·cm. 2 For example, it can be 0.38 mΩ·cm 2 ~0.45mΩ·cm 2 .

[0053] In some alternative embodiments, the contact resistivity of the N-region seed layer of the solar cell does not exceed 0.38 mΩ·cm. 2 For example, it can be 0.32mΩ·cm 2 ~0.38mΩ·cm 2 .

[0054] In some optional implementations, the photoelectric conversion efficiency of the solar cell is not less than 25.6%, such as 25.6% to 26.1%.

[0055] In some alternative implementations, the open-circuit voltage of the solar cell is not less than 728V, such as 728V~734V.

[0056] In some alternative implementations, the fill factor of the solar cell is not less than 84.7%, such as 84.7% to 85.5%.

[0057] In some alternative implementations, the diffusion depth of copper in the solar cell does not exceed 35 nm, such as 22 nm to 35 nm.

[0058] In addition, the present invention also provides a method for preparing the above-mentioned solar cell, comprising the following steps: sequentially depositing a tunneling oxide layer 20, a doped polycrystalline silicon layer 30, a back passivation layer 40, a composite seed layer 50 and a conductive layer 60 on the back side of a silicon substrate 10.

[0059] In some alternative embodiments, the silicon substrate 10 may be an N-type monocrystalline silicon wafer.

[0060] In some optional embodiments, the fabrication of the solar cell may include: sequentially depositing a tunneling oxide layer 20 and an intrinsic polycrystalline silicon layer on the back side of a silicon substrate 10; performing boron diffusion and phosphorus diffusion in a predetermined region of the intrinsic polycrystalline silicon layer to form alternating P-type doped layers and N-type doped layers; depositing a back passivation layer 40 on the surface of the doped polycrystalline silicon layer 30; opening a contact window 41 in the region of the back passivation layer 40 corresponding to the P-type doped layer and the N-type doped layer; depositing a composite seed layer 50 in the contact window 41; and electroplating a conductive layer 60 on the surface of the composite seed layer 50.

[0061] For example, boron diffusion and phosphorus diffusion can be performed in a predetermined region of the intrinsic polysilicon layer using a mask-diffusion process to form alternating P-type and N-type doped layers, and then a back passivation layer 40 can be deposited on the surface of the doped polysilicon layer 30.

[0062] For example, a contact window 41 can be opened in the region of the back passivation layer 40 corresponding to the P-type doped layer and the N-type doped layer by using a laser film-opening process, so as to expose the surface of the doped layer to be metallized.

[0063] In some optional embodiments, the deposition of the composite seed layer 50 may include: depositing alloy body layers with different Ni contents on the surfaces of the P-type doped region 31 and the N-type doped region 32 respectively; annealing the silicon substrate 10 on which the alloy body layer is deposited so that the Ni in the alloy body layer reacts in situ with the Si in the doped layer to form a diffusion barrier layer at the interface; after annealing, exposing the silicon substrate 10 to an oxygen-containing atmosphere so that the X element in the alloy body layer is oxidized to form a self-passivating oxide layer.

[0064] For example, the following process can be performed: The seed layer of the P-type region can be covered by a mask covering the N-type region and the non-deposition area, with the mask opening precisely aligned with the contact window 41 of the P-type region; deposition is performed in a magnetron sputtering chamber using a CuNiX alloy target (the target contains 12%~25% Ni and 1%~4% X); after deposition, the mask is removed. The seed layer of the N-type region can be covered by a mask covering the deposited P-type region and the non-deposition area, with the mask opening precisely aligned with the contact window 41 of the N-type region; the silicon substrate is placed in a magnetron sputtering chamber and deposited using a CuNiX alloy target (the target contains 5%~12% Ni and 0.5%~3% X); after deposition, the mask is removed, and the solar cell with the P-type and N-type seed layers deposited is placed in a rapid thermal annealing apparatus and heat-treated under a N2 protective atmosphere to achieve in-situ generation of the interface diffusion barrier layer. After annealing, the battery cells are removed and exposed to a clean oxygen-containing atmosphere, where a dense, self-passivating oxide film spontaneously forms on the surface of the seed layer.

[0065] During the rapid thermal annealing process described above, Ni atoms acquire sufficient diffusion energy, selectively migrate to the doped layer interface, and undergo a solid-state reaction with Si in the doped layer, forming NiSi in situ at the interface. x Diffusion barrier layer; the NiSi x The diffusion barrier layer has a dense crystalline structure with very few grain boundaries. The diffusion coefficient of copper atoms in its lattice is reduced by 2 to 3 orders of magnitude compared to that in copper grain boundaries. Only a continuous thin layer of 2 nm to 8 nm is needed to effectively block the thermal diffusion of copper. In a clean oxygen-containing atmosphere, the X element segregates to the surface and preferentially oxidizes to form a self-passivating oxide layer, ultimately obtaining a three-layer composite seed layer structure consisting of a diffusion barrier layer, an alloy body layer, and a self-passivating oxide layer. Both the diffusion barrier layer and the self-passivating oxide layer are generated in situ, requiring no additional separate deposition.

[0066] In some alternative embodiments, the deposition can be performed using magnetron sputtering. Deposition conditions include: a background vacuum of <5 × 10⁻⁶. -4 The working gas pressure is 0.2Pa~0.8Pa (e.g., 0.2Pa, 0.3Pa, 0.4Pa, 0.5Pa, 0.6Pa, 0.7Pa, or 0.8Pa), the sputtering power is 100W~500W (e.g., 100W, 200W, 300W, 400W, or 500W), the deposition temperature is 25℃~150℃ (e.g., 25℃, 50℃, 80℃, 100℃, 120℃, or 150℃), and the deposition time is 1min~10min (e.g., 1min, 2min, 5min, 8min, or 10min). The background vacuum is <5×10⁻⁶ Pa. -4Pa ensures a clean deposition environment and reduces impurity incorporation; a working gas pressure of 0.2 Pa to 0.8 Pa and a sputtering power of 100 W to 500 W ensure a moderate sputtering rate and a dense and uniform film; a deposition temperature of 25℃ to 150℃ avoids damage to the underlying structure, and a deposition time of 1 min to 10 min facilitates precise control of the seed layer thickness while taking into account process efficiency.

[0067] The annealing temperature is 200℃~400℃ (e.g., 200℃, 250℃, 300℃, 350℃, or 400℃), the time is 30s~120s (e.g., 30s, 50s, 80s, 100s, or 120s), and the heating rate is 30℃ / s~60℃ / s (e.g., 30℃ / s, 40℃ / s, 50℃ / s, or 60℃ / s). A rapid heating rate of 30℃ / s to 60℃ / s can quickly activate the diffusion of Ni atoms, promote the solid-state reaction between Ni and Si at the interface, and efficiently generate dense NiSi. x The diffusion barrier layer not only avoids copper diffusion problems caused by prolonged high temperatures, but also prevents premature diffusion of copper atoms and excessive grain growth due to the shortened high-temperature dwell time.

[0068] The oxygen-containing atmosphere has a temperature of 20℃~30℃ (e.g., 20℃, 25℃, or 30℃), a relative humidity of 40%~60% (e.g., 40%, 45%, 50%, 55%, or 60%), and an exposure time of 5min~30min (e.g., 5min, 10min, 15min, 20min, 25min, or 30min). The 40%~60% relative humidity helps to uniformly oxidize element X, forming a dense and uniform oxide layer, ensuring the consistency and reliability of the self-passivation effect.

[0069] In some optional embodiments, the electroplating solution used for the conductive layer 60 may include 150 g / L to 250 g / L (e.g., 150 g / L, 180 g / L, 200 g / L, 220 g / L, or 250 g / L, etc.) of CuSO4·5H2O, 80 g / L to 120 g / L (e.g., 80 g / L, 90 g / L, 100 g / L, 110 g / L, or 120 g / L, etc.) of H2SO4, and 40 ppm to 60 ppm (e.g., 40 ppm, 45 ppm, 50 ppm, 55 ppm, or 60 ppm, etc.) of Cl. - .

[0070] The aforementioned electroplating solution is an acidic system. The self-passivating oxide layer on the seed layer surface dissolves rapidly or forms conductive microchannels upon immersion in the solution, allowing electroplating to be started directly without a delay in energizing, thus simplifying the operation. CuSO4·5H2O is used to provide the copper ion source; a concentration of 150 g / L to 250 g / L ensures a sufficient deposition rate. 80 g / L to 120 g / L of H2SO4 improves conductivity and coating uniformity. 40 ppm to 60 ppm of Cl... - It can refine the grain size of the coating and improve the density and smoothness of the coating.

[0071] In some optional embodiments, after preparing the composite seed layer 50, the battery cell with the composite seed layer 50 is placed in the electroplating solution and left to stand for 2 to 5 seconds to remove surface bubbles. Then, the power is turned on, and electroplating is performed with the composite seed layer 50 as the cathode and the copper plate as the anode to form a copper conductive layer 60. After electroplating, the battery cell is cleaned with deionized water and dried with N2.

[0072] In some optional embodiments, the electroplating conditions include: a current density of 1 ASD to 5 ASD (e.g., 1 ASD, 2 ASD, 3 ASD, 4 ASD, or 5 ASD), a temperature of 20°C to 50°C (e.g., 20°C, 30°C, 40°C, or 50°C), and a time of 5 min to 15 min (e.g., 5 min, 10 min, or 15 min). "ASD" stands for A / dm². 2 The abbreviation for Ampere specifically refers to the current intensity (ampere) passing through a unit area (1 square decimeter).

[0073] In some optional embodiments, a stepped start-up method is used in the initial stage of electroplating, gradually increasing the current density from 0 to a set value within 10s to 30s (e.g., 10s, 15s, 20s, 25s, or 30s). This stepped start-up method avoids the impact of a sudden large current on the seed layer during the initial stage of electroplating, preventing localized overheating or delamination at the interface between the seed layer and the silicon substrate 10 due to current concentration, thus ensuring the integrity and contact performance of the seed layer. Furthermore, the gradually increasing current density helps copper ions to uniformly nucleate and grow on the surface of the seed layer, improving the uniformity and density of the coating, and avoiding coating thickness differences caused by uneven current distribution in the initial stage.

[0074] Building upon the above, this invention employs a mask-magnetron sputtering combined process, with equipment compatible with existing back-contact solar cell production lines, requiring no large-scale modifications. By replacing the pure silver seed layer with a silver-free CuNiX alloy, material costs can be reduced by more than 70%. Compared to existing technologies, this invention, through precise interface contact control, can maintain a cell conversion efficiency comparable to or even better than that of pure silver, while reducing metallization costs by more than 80%, truly achieving low-cost, high-efficiency silver-free metallization.

[0075] In addition, the present invention also provides a solar cell module including the above-described solar cell.

[0076] The features and performance of the present invention will be further described in detail below with reference to embodiments.

[0077] Example 1 This embodiment provides a solar cell, which includes a silicon substrate 10. A tunneling oxide layer 20, a doped polycrystalline silicon layer 30, a back passivation layer 40, a composite seed layer 50, and a conductive layer 60 are sequentially stacked on the back side of the silicon substrate 10. The doped polycrystalline silicon layer 30 includes alternating P-type doped regions 31 and N-type doped regions 32. The back passivation layer 40 has a contact window 41. The composite seed layer 50 includes a first seed layer 51 and a second seed layer 52, wherein the first seed layer 51 contacts the P-type doped region 31 through the contact window 41, and the second seed layer 52 contacts the N-type doped region 32 through the contact window 41. The first seed layer 51 includes a first diffusion barrier layer 511, a first alloy body layer 512, and a first self-passivating oxide layer 513 sequentially arranged from near the silicon substrate 10 to away from the silicon substrate 10. The second seed layer 52 includes a second diffusion barrier layer 521, a second alloy body layer 522, and a second self-passivating oxide layer 523 sequentially arranged from near the silicon substrate 10 to away from the silicon substrate 10.

[0078] The method for fabricating this solar cell includes the following steps: S1: Preparation and windowing of silicon substrate precursor.

[0079] Using an N-type single-crystal silicon wafer as the silicon substrate 10, a tunneling oxide layer 20 with a thickness of 1.5 nm and an intrinsic polycrystalline silicon layer with a thickness of 150 nm are sequentially deposited on its back side. Boron diffusion and phosphorus diffusion are performed in predetermined regions of the intrinsic polycrystalline silicon layer using masking and diffusion processes, respectively, to form alternating P-type doped regions 31 and N-type doped regions 32, which together constitute the doped polycrystalline silicon layer 30. Subsequently, a back passivation layer 40 is deposited on the surface of the doped polycrystalline silicon layer 30. This back passivation layer 40 includes a 5 nm thick Al2O3 layer and an 80 nm thick SiN layer. x Finally, using a laser film-opening process, contact windows 41 are opened at the positions of the back passivation layer 40 corresponding to the P-type doped region 31 and the N-type doped region 32, respectively, to expose the surface of the doped layer to be metallized.

[0080] S2: Deposition of the first seed layer 51 in the P-type region.

[0081] A mask is used to cover the N-type region and the non-deposition area, aligning the mask opening with the contact window 41 of the P-type region. Deposition is performed in the magnetron sputtering chamber using a first CuNiX alloy target (where Ni comprises 18% atomic percentage, X comprises 2% atomic percentage, and X is Cr). The sputtering process parameters are: base vacuum < 5 × 10⁻⁶. -4 The working pressure was 0.5 Pa, the sputtering power was 300 W, the deposition temperature was 100 °C, and the deposition time was 5 min. After deposition, the mask was removed to obtain a first seed layer 51 with a thickness of approximately 100 nm.

[0082] S3: Second seed layer 52 deposition in the N-type region.

[0083] A mask is used to cover the deposited P-type region and the non-deposited region, aligning the mask opening with the contact window 41 of the N-type region. Deposition is performed in the magnetron sputtering chamber using a second CuNiX alloy target (where Ni comprises 8% atomic percentage, X comprises 1.5% atomic percentage, and X is Cr). The sputtering process parameters are the same as in S2. After deposition, the mask is removed, yielding a second seed layer 52 with a thickness of approximately 80 nm.

[0084] S4: Rapid thermal annealing and self-passivation treatment.

[0085] The solar cells with seed layer deposition completed were placed in a rapid thermal annealing apparatus and annealed under N2 protection to form a NiSi layer with a thickness of approximately 5 nm. x Diffusion is blocked, and Cr elements segregate to the surface. The annealing temperature is 350℃, the annealing time is 60s, and the heating rate is 50℃ / s. After annealing, the cell is removed and exposed to clean air at 25℃ and 50% relative humidity for 20min. Cr elements preferentially oxidize, spontaneously forming a dense self-passivating oxide layer with a thickness of approximately 5nm on the surface. The alloy bulk layer lies between the diffusion-blocking layer and the self-passivating oxide layer.

[0086] S5: Electroplated copper conductive layer 60.

[0087] The treated battery cells were placed in a copper sulfate electroplating solution and allowed to stand for 3 seconds to remove air bubbles. Then, the power was turned on, and electroplating was performed using the composite seed layer 50 as the cathode and the copper plate as the anode. The copper sulfate electroplating solution contained 200 g / L CuSO4·5H2O, 100 g / L H2SO4, and 50 ppm Cl. - A stepped start-up method was adopted, gradually increasing the current density from 0 to the set value of 3 ASD within 20 seconds. Electroplating was performed at 30°C for 10 minutes to form a dense copper conductive layer 60 with a thickness of approximately 10 μm. After electroplating, the layer was cleaned with deionized water and dried with N2 to obtain the solar cell.

[0088] Example 2 This embodiment also provides a solar cell, whose main structure is the same as that of Embodiment 1, the difference being the preparation method and layer thickness: S1: Preparation and windowing of silicon substrate precursor.

[0089] Using an N-type single-crystal silicon wafer as the silicon substrate 10, a tunneling oxide layer 20 with a thickness of 1 nm and an intrinsic polycrystalline silicon layer with a thickness of 100 nm are sequentially deposited on its back side. Boron diffusion and phosphorus diffusion are performed in predetermined regions of the intrinsic polycrystalline silicon layer using masking and diffusion processes, respectively, to form alternating P-type doped regions 31 and N-type doped regions 32, which together constitute the doped polycrystalline silicon layer 30. Subsequently, a back passivation layer 40 is deposited on the surface of the doped polycrystalline silicon layer 30. This back passivation layer 40 includes an Al2O3 layer with a thickness of 3 nm and a SiN layer with a thickness of 50 nm. x Finally, using a laser film-opening process, contact windows 41 are opened at the positions of the back passivation layer 40 corresponding to the P-type doped region 31 and the N-type doped region 32, respectively, to expose the surface of the doped layer to be metallized.

[0090] S2: Deposition of the first seed layer 51 in the P-type region.

[0091] A mask is used to cover the N-type region and the non-deposition area, aligning the mask opening with the contact window 41 of the P-type region. Deposition is performed in the magnetron sputtering chamber using a first CuNiX alloy target (containing 12% Ni and 1% X, where X is Cr). The sputtering process parameters are: background vacuum < 5 × 10⁻⁶. -4 The working pressure was 0.2 Pa, the sputtering power was 100 W, the deposition temperature was 25 °C, and the deposition time was 1 min. After deposition, the mask was removed to obtain a first seed layer 51 with a thickness of approximately 80 nm.

[0092] S3: Second seed layer 52 deposition in the N-type region.

[0093] A mask is used to cover the deposited P-type region and the non-deposited region, aligning the mask opening with the contact window 41 of the N-type region. Deposition is performed in the magnetron sputtering chamber using a second CuNiX alloy target (containing 5% Ni and 0.5% X, where X is Mn). The sputtering process parameters are the same as in S2. After deposition, the mask is removed, yielding a second seed layer 52 with a thickness of approximately 60 nm.

[0094] S4: Rapid thermal annealing and self-passivation treatment.

[0095] The solar cells with seed layer deposition completed are placed in a rapid thermal annealing apparatus and annealed under N2 protection to form a NiSi layer with a thickness of approximately 2 nm. xDiffusion is blocked, and Cr elements segregate to the surface. The annealing temperature is 200℃, the annealing time is 30s, and the heating rate is 30℃ / s. After annealing, the cell is removed and exposed to clean air at 20℃ and 40% relative humidity for 5 minutes. Cr elements preferentially oxidize, spontaneously forming a dense self-passivating oxide layer with a thickness of approximately 2nm on the surface. The alloy bulk layer lies between the diffusion-blocking layer and the self-passivating oxide layer.

[0096] S5: Electroplated copper conductive layer 60.

[0097] The treated battery cells were placed in a copper sulfate electroplating solution, allowed to stand for 2 seconds to remove air bubbles, and then the power was turned on. Electroplating was performed using the composite seed layer 50 as the cathode and the copper plate as the anode. The copper sulfate electroplating solution contained 150 g / L CuSO4·5H2O, 100 g / L H2SO4, and 40 ppm Cl. - A stepped start-up method was adopted, gradually increasing the current density from 0 to the set value of 1 ASD within 10 seconds. Electroplating was carried out at 20℃ for 5 minutes to form a dense copper conductive layer 60 with a thickness of approximately 5 μm. After electroplating, the layer was cleaned with deionized water and dried with N2 to obtain the solar cell.

[0098] Example 3 This embodiment also provides a solar cell, whose main structure is the same as that of Embodiment 1, the difference being the preparation method and layer thickness: S1: Preparation and windowing of silicon substrate precursor.

[0099] Using an N-type single-crystal silicon wafer as the silicon substrate 10, a tunneling oxide layer 20 with a thickness of 2 nm and an intrinsic polycrystalline silicon layer with a thickness of 200 nm are sequentially deposited on its back side. Boron diffusion and phosphorus diffusion are performed in predetermined regions of the intrinsic polycrystalline silicon layer using masking and diffusion processes, respectively, to form alternating P-type doped regions 31 and N-type doped regions 32, which together constitute the doped polycrystalline silicon layer 30. Subsequently, a back passivation layer 40 is deposited on the surface of the doped polycrystalline silicon layer 30. This back passivation layer 40 includes an Al₂O₃ layer with a thickness of 10 nm and a SiN layer with a thickness of 100 nm. x Finally, using a laser film-opening process, contact windows 41 are opened at the positions of the back passivation layer 40 corresponding to the P-type doped region 31 and the N-type doped region 32, respectively, to expose the surface of the doped layer to be metallized.

[0100] S2: Deposition of the first seed layer 51 in the P-type region.

[0101] A mask is used to cover the N-type region and the non-deposition area, aligning the mask opening with the contact window 41 of the P-type region. Deposition is performed in the magnetron sputtering chamber using a first CuNiX alloy target (containing 25% Ni and 4% X, where X is Cr). The sputtering process parameters are: base vacuum < 5 × 10⁻⁶. -4 The working pressure was 0.8 Pa, the sputtering power was 500 W, the deposition temperature was 150 °C, and the deposition time was 10 min. After deposition, the mask was removed to obtain a first seed layer 51 with a thickness of approximately 120 nm.

[0102] S3: Second seed layer 52 deposition in the N-type region.

[0103] A mask is used to cover the deposited P-type region and the non-deposited region, aligning the mask opening with the contact window 41 of the N-type region. Deposition is performed in the magnetron sputtering chamber using a second CuNiX alloy target (containing 12% Ni and 3% X, where X is Al). The sputtering process parameters are the same as in S2. After deposition, the mask is removed, yielding a second seed layer 52 with a thickness of approximately 100 nm.

[0104] S4: Rapid thermal annealing and self-passivation treatment.

[0105] The solar cells with seed layer deposition completed were placed in a rapid thermal annealing apparatus and annealed under N2 protection to form a NiSi layer with a thickness of approximately 8 nm. x Diffusion is blocked, and Cr elements segregate to the surface. The annealing temperature is 450℃, the annealing time is 120s, and the heating rate is 60℃ / s. After annealing, the cell is removed and exposed to clean air at 30℃ and 60% relative humidity for 30min. Cr elements preferentially oxidize, spontaneously forming a dense self-passivating oxide layer with a thickness of approximately 10nm on the surface. An alloy bulk layer lies between the diffusion-blocking layer and the self-passivating oxide layer.

[0106] S5: Electroplated copper conductive layer 60.

[0107] The treated battery cells were placed in a copper sulfate electroplating solution and allowed to stand for 5 seconds to remove air bubbles. Then, the power was turned on, and electroplating was performed using the composite seed layer 50 as the cathode and the copper plate as the anode. The copper sulfate electroplating solution contained 250 g / L CuSO4·5H2O, 100 g / L H2SO4, and 60 ppm Cl. - A stepped start-up method was adopted, gradually increasing the current density from 0 to the set value of 5 ASD within 30 seconds. Electroplating was then performed at 50°C for 15 minutes to form a dense copper conductive layer 60 with a thickness of approximately 15 μm. After electroplating, the layer was cleaned with deionized water and dried with N2 to obtain the solar cell.

[0108] Example 4 The difference between this embodiment and Embodiment 1 is that the self-passivating element X is replaced by Mn instead of Cr, while the other material composition, content and preparation process parameters remain the same as in Embodiment 1.

[0109] Comparative Example 1 The difference between this comparative example and Example 1 is that a pure copper seed layer with a thickness of 100 nm was deposited on the back of the solar cell using magnetron sputtering, and then copper was electroplated to form a conductive layer 60 with a thickness of 10 μm. After electroplating, tin was electroplated as a protective layer (with a thickness of 1 μm).

[0110] That is, in this comparative example, the seed layer is a pure copper layer that does not contain Ni and X elements. It is deposited on all surfaces of the back passivation layer 40.

[0111] Comparative Example 2 The difference between this comparative example and Example 1 is that: a CuNi binary alloy seed layer is deposited in sections using magnetron sputtering deposition, with the atomic percentage of Ni in the first seed layer 51 being 18% and the atomic percentage of Ni in the second seed layer 52 being 8%. Then, copper is electroplated to form a conductive layer 60 with a thickness of 10 μm, and after electroplating, tin is electroplated as a protective layer (with a thickness of 1 μm).

[0112] Comparative Example 3 The difference between this comparative example and Example 1 is that a CuNiCr alloy seed layer is deposited by magnetron sputtering, but the deposition process does not distinguish between the P-region and the N-region, and the same composition is deposited over the entire area. Specifically, in the CuNiCr alloy, the atomic percentage of Ni is 12% and the atomic percentage of Cr is 2%. Then, copper is electroplated to form a conductive layer 60 with a thickness of 10 μm. After electroplating, tin is electroplated as a protective layer (with a thickness of 1 μm).

[0113] Comparative Example 4 The difference between this comparative example and Example 1 is that element X is an element that cannot be self-passivated by oxidation, specifically Sn.

[0114] Comparative Example 5 The difference between this comparative example and Example 1 is that the Ni content in the first seed layer 51 is 6%.

[0115] Comparative Example 6 The difference between this comparative example and Example 1 is that the Ni content in the first seed layer 51 is 32%.

[0116] Comparative Example 7 The difference between this comparative example and Example 1 is that the Cr content in the first seed layer 51 is 0.5%.

[0117] Comparative Example 8 The difference between this comparative example and Example 1 is that the Cr content in the first seed layer 51 is 6%.

[0118] Comparative Example 9 The difference between this comparative example and Example 1 is that the thickness of the first seed layer 51 is 40 nm.

[0119] Comparative Example 10 The difference between this comparative example and Example 1 is that the thickness of the first seed layer 51 is 160 nm.

[0120] Comparative Example 11 The difference between this comparative example and Example 1 is that the Ni content in the second seed layer 52 is 3%.

[0121] Comparative Example 12 The difference between this comparative example and Example 1 is that the Ni content in the second seed layer 52 is 15%.

[0122] Comparative Example 13 The difference between this comparative example and Example 1 is that the Cr content in the second seed layer 52 is 0.2%.

[0123] Comparative Example 14 The difference between this comparative example and Example 1 is that the Cr content in the second seed layer 52 is 5%.

[0124] Comparative Example 15 The difference between this comparative example and Example 1 is that the thickness of the second seed layer 52 is 20 nm.

[0125] Comparative Example 16 The difference between this comparative example and Example 1 is that the thickness of the second seed layer 52 is 140 nm.

[0126] Test case The solar cells (182mm × 210mm in size) prepared in Examples 1-4 and Comparative Examples 1-16 were subjected to performance testing, and the testing methods are as follows: (1) Seed layer contact resistivity test: The total resistance was measured using a semiconductor parameter analyzer. The contact resistivity was calculated by plotting the spacing of parallel linear electrodes (spacing 20μm~100μm, width 100μm). Ten samples were prepared for each condition, and ten sets of data were measured for each sample. The average value was taken. The unit is mΩ·cm. 2 .

[0127] (2) Electrical performance testing: A solar simulator (Wavelabs Sinus-70, AAA grade) was used under standard test conditions (AM1.5G, 1000W / m). 2The photoelectric conversion efficiency (Eta), open circuit voltage (Uoc), and fill factor (FF) of the cells were tested at 25±1℃. Before the test, standard silicon cells were used for calibration, and the average value of 5 cells was taken for each condition.

[0128] (3) Copper diffusion depth test: The secondary ion mass spectrometry (SIMS) method was used. The sample was annealed in a nitrogen atmosphere at 400℃ for 30 min. The SIMS device was used to perform depth analysis from the sample surface to the interior. The distribution of copper ion signal intensity with depth was detected. The depth corresponding to the copper signal dropping to the background noise level was taken as the copper diffusion depth. Five samples were tested under each condition, and the average value was taken. The unit is nm.

[0129] The results are shown in Table 1.

[0130] Table 1 Test Results

[0131] As can be seen from Table 1: By comparing Example 1 with Comparative Examples 1-2 and Comparative Example 4, it can be seen that the pure copper seed layer in Comparative Example 1, which does not contain Ni and X, cannot block copper diffusion at all, resulting in the worst performance. Comparative Example 2 lacks the self-passivating element X, leading to a narrower process window and decreased performance. In Comparative Example 4, element X is an element that cannot self-passivate oxidation, and the corresponding solar cell also has poor overall performance.

[0132] A comparison of Example 1 and Comparative Example 3 shows that the lack of partitioning of the P-region and N-region leads to a decrease in the photoelectric conversion efficiency of the solar cell. A comparison of Example 1 with Comparative Examples 5-8 and 11-14 shows that improper settings of the Ni and Cr content in the first seed layer 51 or the second seed layer 52 both result in a decrease in the overall performance of the solar cell.

[0133] By comparing Example 1 with Comparative Examples 9-10 and 15-16, it can be seen that if the thickness of the first seed layer 51 or the second seed layer 52 deviates from the preferred range, if it is too thin, it will lead to insufficient Ni supply and discontinuity of the diffusion barrier layer; if it is too thick, it will cause the film layer to crack due to increased internal stress. Both of these will lead to a significant reduction in the overall performance of the solar cell.

[0134] In summary, the solution provided by this invention has at least the following advantages: (1) In view of the different requirements of metal contact for the P-type region and N-type region of the back contact battery, the present invention sets up CuNiX seed layers with high Ni and low Ni respectively; the P-type region adopts a high Ni design, which utilizes Ni to form a low contact barrier with P-type polycrystalline silicon to achieve good ohmic contact and solves the problem of difficult contact in the P-type region in the prior art; the N-type region adopts a low Ni design, which utilizes the characteristic that N-type polycrystalline silicon is not sensitive to Ni content to further reduce contact resistance and achieve simultaneous optimization of bipolar contact performance.

[0135] (2) By introducing self-passivating elements such as Cr, Mn, Al, and Ti into the CuNiX alloy, the present invention enables the spontaneous formation of a dense oxide layer on the surface of the seed layer. This oxide layer film has the characteristics of preventing oxygen from diffusing into the interior, having controllable thickness, and being able to dissolve rapidly in acidic electroplating solutions. Compared with the prior art, the present invention does not require acid pickling and activation before electroplating, which simplifies the process, reduces equipment and chemical costs, and avoids the problems of the oxide layer on the surface of pure copper seed layer being difficult to remove evenly and the contact resistance increasing significantly.

[0136] (3) After the seed layer is deposited by magnetron sputtering in this invention, Ni atoms obtain sufficient diffusion energy during rapid thermal annealing, selectively migrate to the interface of the doped layer, and undergo a solid-state reaction with Si in the doped layer to generate NiSi in situ. x The compound has a dense crystal structure with very few grain boundaries. The diffusion coefficient of copper atoms in its lattice is reduced by 2 to 3 orders of magnitude compared to that in copper grain boundaries. Only a continuous thin layer of 2 nm to 8 nm is needed to effectively block the thermal diffusion of copper. Compared with the existing technology that requires the deposition of a barrier layer of tens of nanometers, it achieves high efficiency barrier under low cost conditions.

[0137] (4) The present invention adopts a mask-magnetron sputtering combination process, and the equipment is compatible with the existing back contact solar cell production line without large-scale modification; the use of silver-free CuNiX alloy to replace the pure silver seed layer can reduce the material cost by more than 70%; compared with the prior art, the present invention can maintain a cell conversion efficiency comparable to or even better than that of pure silver through precise interface contact control, while reducing the metallization cost by more than 80%, truly realizing low-cost and high-efficiency silver-free metallization.

[0138] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A composite seed layer material, characterized by, The composite seed layer material comprises a CuNiX ternary alloy, which, by atomic percentage, comprises 70%~94.5% Cu, 5%~25% Ni, and the balance being X; wherein X comprises at least one of Cr, Mn, Al, and Ti, and X is not Ag.

2. A solar cell, characterized by, The solar cell includes a silicon substrate, and a tunneling oxide layer, a doped polycrystalline silicon layer, a back passivation layer, a composite seed layer and a conductive layer are sequentially stacked on the back side of the silicon substrate. The doped polycrystalline silicon layer includes alternating P-type doped regions and N-type doped regions; The back passivation layer has a contact window; The composite seed layer is formed from the composite seed layer material of claim 1; the composite seed layer includes a first seed layer and a second seed layer, wherein the first seed layer is in contact with the P-type doped region through the contact window, and the second seed layer is in contact with the N-type doped region through the contact window.

3. The solar cell according to claim 2, characterized in that, The first seed layer has at least one of the following characteristics: Feature 1: In the first seed layer, the Ni content is 12%~25%, and the X content is 1%~4%; Feature 2: The thickness of the first seed layer is 80nm~120nm; Feature 3: The first seed layer includes a first diffusion barrier layer, a first alloy body layer, and a first self-passivating oxide layer, which are sequentially disposed from the direction close to the silicon substrate to the direction away from the silicon substrate; wherein the first alloy bulk layer is composed of a CuNiX ternary alloy; the first diffusion barrier layer is composed of NiSi formed in-situ by Ni in the first alloy bulk layer and Si in the P-type doped region x ; the first self-passivating oxide layer is composed of an oxide of X in the first alloy bulk layer. Preferably, the first diffusion barrier layer has a dense crystal structure; Preferably, the thickness of the first diffusion barrier layer is 2nm~8nm; Preferably, the thickness of the first self-passivating oxide layer is 2nm to 10nm.

4. The solar cell of claim 2, wherein The second seed layer has at least one of the following characteristics: Feature 4: In the second seed layer, the Ni content is 5%~12% and the X content is 0.5%~3%; Feature 5: The thickness of the second seed layer is 60nm~100nm; Feature 6: The second seed layer includes a second diffusion barrier layer, a second alloy body layer, and a second self-passivating oxide layer, which are sequentially disposed from near the silicon substrate to away from the silicon substrate; wherein the second bulk alloy layer is composed of a CuNiX ternary alloy; the second diffusion barrier layer is formed in-situ by Ni in the second bulk alloy layer and Si in the N-type doped region as NiSi x ; the second self-passivating oxide layer is composed of an oxide formed by X in the second bulk alloy layer. Preferably, the thickness of the second diffusion barrier layer is 2nm~8nm; Preferably, the thickness of the second self-passivating oxide layer is 2nm to 10nm.

5. The solar cell according to claim 2, characterized in that, The solar cell also has at least one of the following characteristics: Feature 7: The thickness of the tunneling oxide layer is 1 nm to 2 nm; Feature 8: The thickness of the doped polycrystalline silicon layer is 100nm~200nm; Feature 9: the back passivation layer comprises an Al2O3 layer with a thickness of 3 nm to 10 nm and a SiN layer with a thickness of 50 nm to 100 nm x layer; feature 10: The thickness of the conductive layer is 5μm to 15μm; preferably, the thickness of the conductive layer is 8μm to 12μm.

6. A method for preparing a solar cell according to any one of claims 2 to 5, characterized in that, Includes the following steps: The tunneling oxide layer, the doped polycrystalline silicon layer, the back passivation layer, the composite seed layer, and the conductive layer are sequentially disposed on the back side of the silicon substrate.

7. The preparation method according to claim 6, characterized in that, The tunneling oxide layer and the intrinsic polycrystalline silicon layer are sequentially deposited on the back side of the silicon substrate; boron diffusion and phosphorus diffusion are performed in a predetermined region of the intrinsic polycrystalline silicon layer to form alternating P-type doped layers and N-type doped layers; a back passivation layer is deposited on the surface of the doped polycrystalline silicon layer; a contact window is opened in the region of the back passivation layer corresponding to the P-type doped layer and the N-type doped layer; a composite seed layer is deposited in the contact window; and a conductive layer is electroplated on the surface of the composite seed layer.

8. The preparation method according to claim 7, characterized in that, The deposition of the composite seed layer includes: depositing alloy body layers with different Ni contents on the surfaces of the P-type doped region and the N-type doped region respectively; and annealing the silicon substrate on which the alloy body layers are deposited to allow the Ni in the alloy body layer to react in situ with the Si in the doped layer to form a diffusion barrier layer at the interface. After annealing, the silicon substrate is exposed to an oxygen-containing atmosphere to oxidize the X element in the alloy body layer to form a self-passivating oxide layer. The deposition conditions include: base vacuum < 5*10 -4 Pa, working pressure 0.2 Pa~0.8 Pa, sputtering power 100 W~500 W, deposition temperature 25℃~150℃, deposition time 1 min~10 min; The annealing temperature is 200℃~400℃, the time is 30s~120s, and the heating rate is 30℃ / s~60℃ / s; The oxygen-containing atmosphere has a temperature of 20℃~30℃, a relative humidity of 40%~60%, and an exposure time of 5min~30min.

9. The preparation method according to claim 7, characterized in that, The plating solution used for the conductive layer includes 150 g / L to 250 g / L of CuSO4·5H2O, 80 g / L to 120 g / L of H2SO4, 40 ppm to 60 ppm of Cl - ; Preferably, the electroplating conditions include: a current density of 1 ASD to 5 ASD, a temperature of 20°C to 50°C, and a time of 5 min to 15 min; Preferably, a stepped start-up method is adopted in the initial stage of electroplating, gradually increasing the current density from 0 to the set value within 10s to 30s.

10. A solar cell module, characterized in that, Includes the solar cell described in any one of claims 2 to 5.