An anodizable die-cast aluminum alloy and its applications

By using die-cast aluminum alloys with specific compositions and a low-temperature aging process, a nanoscale continuous interface layer is formed, which solves the problems of fluidity and anodizing inhomogeneity in die-cast aluminum alloys. This achieves a synergistic breakthrough in high fluidity, thermal conductivity, and excellent anodized appearance, making it suitable for metal casings of consumer electronic devices.

CN123108360APending Publication Date: 2026-11-17ZHONGLIHONG (SHENZHEN) NEW MATERIAL TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611238228.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing die-cast aluminum alloys present a contradiction in achieving high fluidity, good thermal conductivity, and top-quality anodized appearance. Current technologies have failed to systematically address the issues of insufficient fluidity in low-silicon melts and electrochemical inhomogeneity during anodizing.

Method used

Using die-cast aluminum alloys with specific compositions, including a combination of elements such as Si, Mg, Mn, Ca, Ti, Zr, Er, Be, Ga, Hf, Zn, Sr, Ce, and La, a nanoscale continuous interface layer rich in Ga and Ca is formed through a low-temperature aging process. This layer combines Er with heterogeneous nucleation cores of Hf, Zr, and Ti to prevent dendrite cross-linking, thereby achieving high fluidity and excellent anodized appearance.

Benefits of technology

It achieves high fluidity (spiral flow length ≥700 mm), good thermal conductivity (≥100 W·m-1·K-1) and top-quality anodized appearance (ΔE≤1.2), avoiding the use of expensive elements and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108360A_ABST
    Figure CN123108360A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of non-ferrous metal materials and precision manufacturing, and discloses an anodizable die-cast aluminum alloy and its applications. The alloy composition includes Si, Mg, Mn, Ca, Ti, Zr, Fe, Er, Be, Ga, Hf, Zn, Sr, Ce, and La, with the balance being Al and unavoidable impurities; wherein the individual impurity is ≤0.05%, and the total is ≤0.15%. This invention achieves a dendrite arm spacing ≤15μm and a spiral flow length ≥700mm in the as-cast state through the synergistic effect of Hf, Zr, Er, and Ti promoting nucleation and Ce and La inhibiting growth. By adding Ga and Ca and combining it with low-temperature aging, a Ga- and Ca-rich interface layer is formed at the second phase / matrix interface during anodizing, resulting in a color difference ΔE ≤1.2 and a thermal conductivity ≥100 W / (m·K).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of non-ferrous metal materials and precision manufacturing, specifically to an anodizable die-cast aluminum alloy and its applications. Background Technology

[0002] As consumer electronics devices strive for ultra-thinness and high performance, their metal casings must simultaneously meet stringent requirements for excellent heat dissipation, superior surface finish, and reliable formability under demanding thin-walled conditions. Currently, the mainstream technologies for achieving metal casings in laptops, tablets, and other electronic devices primarily rely on two main material systems: (1) High-silicon die-cast aluminum alloy route Traditional die-cast aluminum alloys, such as ADC12, possess excellent casting fluidity due to their high silicon content (typically 10–13%), making them suitable for efficient die casting of complex thin-walled structures. However, the abundant presence of coarse primary silicon and eutectic silicon phases severely disrupts the aluminum matrix, resulting in a low thermal conductivity (typically below 70 W·m). -1 ·K -1 Meanwhile, these silicon phases exhibit differences in conductivity during the anodizing process, leading to difficult-to-eliminate appearance defects such as uneven film layer, darkening, and the appearance of "black spots" or "flow marks".

[0003] (2) High-strength wrought aluminum alloy route (such as 6-series and 7-series alloys) Wrought aluminum alloys, represented by 6-series and 7-series alloys, have a uniform and bright appearance after anodizing due to their low silicon content, and also have good thermal conductivity. However, their forming method relies on hot extrusion of blanks combined with a large amount of CNC milling, resulting in a material removal rate of over 70%, high costs, and severely limited design freedom due to the extrusion cross-sectional shape, making it impossible to efficiently form consumer electronics casing structures with complex internal cavities, undercuts, and irregular curved surfaces.

[0004] In an attempt to reconcile the contradictions between the two major material systems, numerous improvements have been made to existing technologies, but none have systematically solved the problem. For example, existing technology (CN101503773A) achieved a concentration greater than 150 W·m³ by using high silicon content and adding rare earth elements. -1 ·K -1 While improving thermal conductivity, the high silicon content still compromises the appearance of anodized products. Another existing technology (CN117888004A) reduces the silicon content to extremely low levels (Si≤0.08%) and adds up to 5.0–12.0% of rare earth elements such as Ce to achieve high thermal conductivity. While this is beneficial for anodizing, the high cost of rare earth elements and the alteration of melt properties make it difficult to widely adopt in the consumer electronics casing market, which prioritizes cost-effectiveness. Research has designed low-silicon alloys such as Al-(0.5–1.5)Mg-1Fe-0.5Si, which have thermal conductivity of (160–180 W·m⁻¹). -1·K -1 While significantly improved, its fluidity is only 60-85% of ADC12, and it still contains 1% iron (Fe), which easily forms a coarse and brittle phase, posing a potential risk to the uniformity and reliability of anodizing.

[0005] It is evident that existing technologies for improving such alloys face two prominent problems during die casting: firstly, the low-silicon melt lacks fluidity, and under quenching conditions, rapid cross-linking of α-Al dendrites blocks the flow channels, leading to incomplete filling or hot cracking; secondly, the second phase in the alloy exhibits electrochemical inhomogeneity at the interface with the matrix during anodizing, resulting in color differences and poor adhesion of the film. Therefore, there is an urgent need to develop a die-cast aluminum alloy that simultaneously satisfies high fluidity, good thermal conductivity, and a superior anodized appearance. Summary of the Invention

[0006] The purpose of this invention is to overcome at least one deficiency of the prior art and to provide a high-fluidity, anodizable die-cast aluminum alloy and its preparation method.

[0007] The technical solution adopted in this invention is: A first aspect of the invention provides: an anodizable die-cast aluminum alloy, wherein the alloy comprises, by weight percentage: Si: 0.05–0.75%, Mg: 0.35–1.0%, Mn: 1.5–2.5%, Ca: 0.015–0.045%, Ti: 0.1–0.30%, Zr: 0.1–0.3%, Fe: 0.1–0.35%, Er: 0.1–0.65%, Be: 0.01–0.015%, Ga: 0.14–0.23%, Hf: 0.10–0.15%, Zn: 0.05–0.8%, Sr: 0.03–0.25%, sum of Ce and La: 0.25–0.35%, with the balance being Al and unavoidable impurities.

[0008] Optionally, the alloy composition, by mass percentage, is as follows: Si: 0.25–0.55%, Mg: 0.7–0.95%, Mn: 1.6–2.0%, Ca: 0.025–0.040%, Ti: 0.15–0.20%, Zr: 0.1–0.15%, Fe: 0.2–0.30%, Er: 0.3–0.55%, Be: 0.01–0.015%, Ga: 0.15–0.22%, Hf: 0.10–0.15%, Zn: 0.15–0.25%, Sr: 0.05–0.15%, sum of Ce and La: 0.28–0.32%, with the balance being Al and unavoidable impurities. Preferably, the mass ratio of Ce to La is (0.19–0.21):(0.09–0.11).

[0009] Optionally, the mass ratio of Ca:Ga is 1:(3.75–7.2). Experimental results show that this mass ratio is beneficial for obtaining anodized layers with lower color difference.

[0010] Optionally, after die casting, the die-cast part is held at 170–190°C for 45–75 minutes, and then cooled. Experimental results show that this facilitates the migration of Ga and Ca to the second phase / matrix interface under Joule heating during anodizing, forming a continuous nanoscale interface layer rich in Ga and Ca in situ, thereby significantly reducing the color difference in appearance after anodizing.

[0011] Optionally, the Er element content in the die-cast aluminum alloy is 0.3-0.55%.

[0012] Optionally, the total amount of unavoidable impurities is ≤0.15%.

[0013] Optionally, the content of a single unavoidable impurity is ≤0.05%.

[0014] Optionally, the alloy composition, by mass percentage, is: Si 0.40%, Mg 0.70%, Mn 1.80%, Ca 0.025%, Ga 0.18%, Ti 0.18%, Zr 0.12%, Hf 0.12%, Fe 0.25%, Er 0.30%, Be 0.012%, Zn 0.20%, Sr 0.08%, Ce and La sum 0.30%, with the balance being Al and unavoidable impurities.

[0015] Optionally, the alloy composition, by mass percentage, is: Si 0.55%, Mg 0.85%, Mn 2.00%, Ca 0.035%, Ga 0.22%, Ti 0.20%, Zr 0.15%, Hf 0.14%, Fe 0.30%, Er 0.40%, Be 0.015%, Zn 0.25%, Sr 0.05%, Ce and La sum 0.32%, with the balance being Al and unavoidable impurities.

[0016] Optionally, the alloy composition, by mass percentage, is: Si 0.25%, Mg 0.95%, Mn 1.60%, Ca 0.040%, Ga 0.15%, Ti 0.15%, Zr 0.10%, Hf 0.10%, Fe 0.20%, Er 0.55%, Be 0.010%, Zn 0.15%, Sr 0.15%, Ce and La sum 0.28%, with the balance being Al and unavoidable impurities.

[0017] Optionally, the method for preparing the die-cast aluminum alloy includes the following steps: (1) Raw material melting and alloying: The raw materials are melted at 700-760℃ according to the proportion and stirred thoroughly; (2) Refining and degassing: The alloy melt is subjected to rotary argon gas refining and degassing treatment at 710-740℃; (3) Die casting: The treated melt is transferred to a die casting machine at 700-730℃ and die casting is carried out under vacuum conditions ≤50 mbar, with an injection speed ≥4 m / s; (4) Heat treatment: Hold the die casting at 170-190℃ for 45-75 minutes, then air cool.

[0018] These features can be combined arbitrarily as long as they do not conflict with each other.

[0019] A second aspect of the present invention provides the use of the die-cast aluminum alloy described in the first aspect of the present invention in the manufacture of metal casings for consumer electronic devices.

[0020] A third aspect of the invention provides: a metal casing made of the die-cast aluminum alloy described in the first aspect of the invention.

[0021] The beneficial effects of this invention are: The die-cast aluminum alloys of some embodiments of the present invention have the following advantages: (1) For the first time, the anodized appearance quality of wrought aluminum alloys was achieved in die-cast aluminum alloys. Through the substitution of low silicon, high magnesium and manganese, the synergy of element control such as Ga and Ca and low temperature aging process, and the synergistic interface regulation of Ga and Ca (the two migrate together to the second phase / matrix interface under the Joule heat drive of anodizing, forming a nanoscale continuous interface layer rich in Ga and Ca in situ), the defects such as color difference and black spots commonly found after anodizing of low silicon die-cast aluminum alloys were unexpectedly eliminated, achieving ΔE≤1.2.

[0022] (2) The bottleneck of insufficient fluidity in low-silicon die-casting alloys has been solved. Through the synergistic combination of Er with Hf, Zr, and Ti to form a highly efficient heterogeneous nucleation core, coupled with the dendrite growth-inhibiting effects of Ce and La, the average dendrite arm spacing in the as-cast state is ≤15 μm, achieving a spiral flow length ≥700 mm at extremely low silicon content, thus ensuring thin-walled die-casting. Sr is a highly surface-active element; during solidification, it adsorbs at the silicon crystal growth interface, blocking the rapid unidirectional growth of silicon, inducing a large number of five-fold twins, forcing silicon to continuously branch, and ultimately transforming into a fine, short rod / fibrous, uniformly dispersed coral-like silicon phase. This helps improve the mechanical properties of die-cast parts and makes the filling of thin-walled complex parts more stable.

[0023] (3) It achieves high fluidity and good thermal conductivity (≥100 W·m). -1 ·K -1The synergistic breakthrough of the combination of high-quality die casting and top-grade anodized appearance avoids expensive elements such as Sc and Ag. Stable production can be achieved using conventional die casting equipment and low-temperature aging process, with controllable costs, making it suitable for large-scale industrial applications. Attached Figure Description

[0024] Figure 1 The image shows a comparison of the as-cast metallographic structures of Example 1 (Figure a) and Comparative Example 3 (Figure b).

[0025] Figure 2 This is an interface element distribution diagram after anodizing in Example 1, wherein... Figure 2 a represents the cross-sectional morphology of the anodic oxide film. Figure 2 b is the EDS elemental surface scan spectrum at the membrane / substrate interface.

[0026] Figure 3 These are comparative photographs of the appearance of Example 1 and Comparative Example 1 after anodizing, in which... Figure 3 a represents the uniform, glossy surface of Example 1. Figure 3 b represents the surface of Comparative Example 1 (excluding Ga and Ca).

[0027] Figure 4 This is a comparison diagram of the spiral flow length of Embodiments 1-3 of the present invention with Comparative Examples 3 and 4. Detailed Implementation

[0028] The following disclosure provides many different implementations or examples for different ways of implementing the present invention.

[0029] To verify the synergistic performance of the die-cast aluminum alloy described in this invention, various embodiments and comparative examples were prepared according to the composition in Table 1 (unless otherwise stated, the content of other impurity elements besides the alloying elements explicitly listed above is ≤0.05% for a single element and ≤0.15% for the total content). The preparation method of each embodiment includes the following steps: (1) Raw material melting and alloying: The raw materials are melted at 700-760℃ according to the proportion and stirred thoroughly; (2) Refining and degassing: The alloy melt is subjected to rotary argon gas refining and degassing treatment at 710-740℃; (3) Die casting: The treated melt is transferred to a die casting machine at 700-730℃ and die casting is carried out under vacuum conditions ≤50 mbar, with an injection speed ≥4 m / s; (4) Heat treatment: Hold the die casting at 170-190℃ for 45-75 minutes, then air cool.

[0030] Table 1: Alloy composition design for examples and comparative examples (wt%, balance Al) element Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 3 Comparative Example 4 Si 0.4 0.55 0.25 0.4 0.4 10.5 Mg 0.7 0.85 0.95 0.7 0.7 0.8 Mn 1.8 2 1.6 1.8 1.8 0.3 Ca 0.025 0.035 0.04 — 0.025 — Ti 0.18 0.2 0.15 0.18 0.18 — Zr 0.12 0.15 0.1 0.12 0.12 — Fe 0.25 0.3 0.2 0.25 0.25 0.9 Er 0.3 0.4 0.55 0.25 0.25 — Be 0.012 0.015 0.01 0.012 0.012 — Ga 0.18 0.22 0.15 — 0.025 — Hf 0.12 0.14 0.1 0.12 0.12 — Zn 0.2 0.25 0.15 0.2 0.2 — Sr 0.08 0.05 0.15 — — — Ce+La 0.20+0.10 0.21+0.11 0.19+0.09 0.20+0.10 — — Note: Comparative Example 1 does not contain Ga or Ca; Comparative Example 3 does not contain Ce or La; Comparative Example 4 is an ADC12 alloy.

[0031] Comparative Example 2 has the same composition as Example 1, but after die casting, it does not undergo the low-temperature aging (170~190℃×45~75min) of step (4), but instead undergoes the following T6 heat treatment: ① Solution treatment: Heat the die casting to 530℃ and hold for 1 hour, then quickly remove it and quench it in water (water temperature 25±5℃). ② Artificial aging: After solution quenching, heat to 175℃ and hold for 8 hours, then air cool.

[0032] The remaining steps (raw material melting, refining and degassing, and die casting) are the same as in Example 1.

[0033] Except for Comparative Example 2, the other samples were prepared using the same low-temperature aging method as in the examples (170-190℃ × 45-75 min).

[0034] The testing and characterization methods for each embodiment and comparative example are as follows: Flowability test: A metal mosquito coil mold was used for casting flowability testing. The mold cavity cross-section was 6 mm × 6 mm, and the total length of the spiral path was approximately 1000 mm. The melt was heated to 700–730°C and poured into a mold preheated to 150–250°C under normal pressure. After cooling, the length of the spiral path when the melt was completely filled was measured. Each sample was tested at least 3 times, and the average value was taken.

[0035] Microstructure analysis: The average dendrite arm spacing was measured using a metallographic microscope. The morphology and composition of the second phase were observed using a scanning electron microscope and an energy dispersive spectroscopy (EDS) instrument. EDS line scans were performed on the second phase / matrix interface of Example 1 and Comparative Example 1 to analyze the distribution of Ga and Ca elements.

[0036] Thermal conductivity testing: Thermal conductivity was measured using the laser flash method. The sample was a circular disc with a diameter of 12.7 mm and a thickness of 2 mm, cut from the die-cast part and coated with graphite on both sides. The test temperature was 25 ℃, and each sample was measured 5 times, with the average value taken.

[0037] Anodizing and Appearance Evaluation: The samples were anodized for 25 minutes under the conditions of 180 g / L sulfuric acid solution, 18±2 ℃, DC voltage of 16 V, and current density of 1.2 A / dm². After anodizing, routine sealing treatment was performed. The surface color difference ΔE value was measured using a colorimeter.

[0038] The results of comparing the properties and microstructures of different casting alloys are shown in Table 2 below.

[0039] Table 2: Performance test and microstructure characterization results of different casting alloys type Spiral flowability (mm) Average SDAS (μm) <![CDATA[Thermal conductivity (W·m -1 ·K -1 )]]> ΔE Example 1 715 14 102 0.8 Example 2 722 13 105 0.7 Example 3 710 15 100 0.9 Comparative Example 1 713 14 101 3.5 Comparative Example 2 718 17 102 3.0 Comparative Example 3 650 25 95 1.6 Comparative Example 4 800 — 60 8.0 The thermal conductivity of the examples is comparable to that of Comparative Examples 1 and 2, indicating that the thermal conductivity mainly comes from the Mn-containing matrix design and is not negatively affected by Ga / Ca addition and low-temperature heat treatment.

[0040] Results analysis: 1) Low silicon, high fluidity Examples 1-3, with extremely low silicon content (0.25–0.55%), exhibited spiral flow lengths (≥715 mm) and average dendrite arm spacing ≤15 μm, approaching those of high-silicon ADC12 (Comparative Example 4, 800 mm). The fundamental reason for this breakthrough lies in the construction of a microscopic mechanism that synergistically promotes nucleation and inhibits growth. During the melting and filling stages, Er, Hf, Zr, Ti, and Al preferentially form high-melting-point compound particles such as Al3(Zr, Hf, Er) and Al3Ti. Er must synergize with Zr, Ti, and Hf to preferentially solidify and form (Al, Zr, Hf, Er) composite precipitates with extremely low lattice mismatch, thus serving as highly efficient heterogeneous nucleation cores to promote the abundant and uniform nucleation of α-Al grains, while avoiding the coarsening tendency caused by excessive Er alone.

[0041] This change is reflected in the metallographic structure ( Figure 1 This provides direct microstructural support, such as... Figure 1 As shown in Figure a, Example 1 formed a fine equiaxed crystal structure, demonstrating the decisive role of the "primary inhibition phase network" in refining grains and preventing dendrite cross-linking. In contrast, Figure 1 Although Comparative Example 3 (excluding Ce and La) in b contains nucleating elements such as Er, Hf, Zr, and Ti, it exhibits a coarse dendritic morphology, and large areas of shrinkage cavities appear around the coarse dendrites.

[0042] Combination Figure 4 The flowability comparison bar chart shows that, in the absence of Ce and La hindering growth, heterogeneous nucleation alone is insufficient to prevent dendrite cross-linking. Ce and La must segregate at the dendrite growth front to reduce the diffusion and attachment rate of aluminum atoms at the solid-liquid interface, strongly hindering the unidirectional extension of the main dendrite and the coarsening of secondary dendrite arms. This synergistic mechanism transforms the solidification structure from coarse dendrites to fine equiaxed crystals, fundamentally preventing large-scale cross-linking of the dendrite framework and ensuring the connectivity of the liquid phase feeding channels at higher solid fractions.

[0043] 2) Excellent anodized appearance The anodized color difference ΔE of Examples 1-3 is ≤0.9, and the surface is uniform and glossy. Figure 2 The TEM and EDS test results clearly reveal the microscopic interface mechanism underlying this macroscopic performance. For example... Figure 2As shown in a and 2b, the anodic oxide film of Example 1 has a uniform and intact cross-section without obvious cracks. EDS surface scans show that the anodic film formed by anodizing in sulfuric acid is mainly composed of aluminum oxide and contains anions (sulfate ions). O, S, and Al generated by the electrolyte are uniformly distributed on the anodic film, and gallium is deposited in situ and attached to the second phase. EDS analysis shows that after anodizing in Example 1, Ga and Ca are significantly enriched at the interface between the second phase and the aluminum matrix. This enrichment mechanism actively regulates the electrochemical activity of the interface. Comparative Example 1, which does not contain Ga and Ca, shows a significantly increased color difference ΔE to 3.5.

[0044] Comparative Example 2 had the same composition as Example 1 but underwent conventional T6 heat treatment, resulting in a color difference ΔE that increased to 3.0, and a coarsening of the dendritic structure (SDAS was 17 μm). This indicates that high-temperature solid solution treatment destroys the in-situ interfacial segregation layer of Ca and Ga, conversely proving that the performance of this invention originates from solidification segregation rather than aging precipitation, thus eliminating the need for high-temperature solid solution treatment. Figure 3 The visual comparison further confirms the indispensability of this mechanism: Comparative Example 1, which lacks Ga and Ca ( Figure 3 b) Not only did it exhibit severe color difference visible to the naked eye, but the surface also showed thermal cracking defects, while Example 1 ( Figure 3 a) The surface is uniform and free of defects.

[0045] This invention successfully achieves active control of the interface between the second phase and the matrix by adding specific elements in conjunction with a low-temperature aging process of 170–190 °C. Under the Joule heating driven by anodic oxidation, Ca in a supersaturated solid solution state and Ga with a low melting point and high diffusion coefficient migrate together to the second phase interface, forming a continuous nanoscale interface layer rich in Ga and Ca in situ. This mechanism ensures the continuity of the interface layer while avoiding local over-corrosion caused by excessive Ga. This invention controls the contents of Ca and Ga within the preferred ranges of 0.015–0.045% and 0.14–0.23%, respectively, based on a systematic consideration of the aforementioned interface control mechanism: if Ca is below 0.015%, the continuity of the interface layer is insufficient; if Ca is above 0.045%, coarse Ca-containing particles are easily formed, disrupting the interface uniformity; if Ga is below 0.14%, it cannot effectively fill the interface micro-regions; if Ga is above 0.23%, the risk of local over-corrosion increases sharply. Furthermore, the synergistic effect is optimal when the mass ratio of Ca to Ga is controlled within the range of 1:(3 to 18). The Ca / Ga ratios of Examples 1-3 (1:7.2, 1:6.3, 1:3.75) all fall within this range, and their ΔE is ≤0.9.

[0046] 3) Good thermal conductivity The thermal conductivity of Examples 1-3 all reached 100 W·m. -1 ·K -1 The above is significantly higher than 60 W·m of ADC12.-1 ·K -1 The thermal conductivity of Comparative Example 3 decreased to 95 W·m. -1 ·K -1 This indicates that, in addition to relying on low-temperature aging to precipitate Mg2Si and purify the matrix, Figure 1 The fine equiaxed crystal morphology shown in example a also played a crucial role, compared to the coarse network structure that produced large areas of voids in Comparative Example 3. Figure 1 (b) The fine and dispersed distribution of the second phase effectively reduces the scattering of hot carriers by solid solution atoms, which indicates that the segregation of Ce and La at the grain boundaries not only helps to suppress dendrite growth, but also plays a role in purifying the grain boundaries and reducing the interfacial thermal resistance.

[0047] (4) Comprehensive comparison Figure 4 This invention visually demonstrates the performance advantages of the alloy of this invention. While traditional high-silicon alloys (Comparative Example 4, ADC12) exhibit excellent fluidity, they suffer from low thermal conductivity and extremely poor anodized appearance (ΔE as high as 8.0). This invention, through the microscopic synergistic effect of multiple elements, successfully achieves high fluidity (≥700 mm) and good thermal conductivity (≥100 W·m). -1 ·K -1 The breakthrough in achieving a unified result in terms of appearance, top-tier anodized finish (ΔE≤0.9) has extremely high value for industrial applications.

[0048] The above is a further detailed description of the present invention and should not be considered as a limitation on the specific implementation of the present invention. For those skilled in the art, simple deductions or substitutions without departing from the concept of the present invention are all within the protection scope of the present invention.

Claims

1. An anodizable die-cast aluminum alloy, characterized in that, The alloy composition, by mass percentage, is: Si: 0.05–0.75%, Mg: 0.35–1.0%, Mn: 1.5–2.5%, Ca: 0.015–0.045%, Ti: 0.1–0.30%, Zr: 0.1–0.3%, Fe: 0.1–0.35%, Er: 0.1–0.65%, Be: 0.01–0.015%, Ga: 0.14–0.23%, Hf: 0.10–0.15%, Zn: 0.05–0.8%, Sr: 0.03–0.25%, Ce and La (total): 0.25–0.35%, balance being Al and unavoidable impurities.

2. The die-cast aluminum alloy according to claim 1, characterized in that, The Er element content in the die-cast aluminum alloy is 0.3-0.55%; and / or the Sr element content in the die-cast aluminum alloy is 0.05-0.15%.

3. The die-cast aluminum alloy according to claim 1, characterized in that, The total amount of unavoidable impurities is ≤0.15%.

4. The die-cast aluminum alloy according to claim 1 or 3, characterized in that, Of the unavoidable impurities, the content of a single impurity is ≤0.05%.

5. The die-cast aluminum alloy according to claim 1, characterized in that, The alloy comprises, by mass percentage: Si 0.40%, Mg 0.70%, Mn 1.80%, Ca 0.025%, Ga 0.18%, Ti 0.18%, Zr 0.12%, Hf 0.12%, Fe 0.25%, Er 0.30%, Be 0.012%, Zn 0.20%, Sr 0.08%, Ce and La sum 0.30%, with the balance being Al and unavoidable impurities.

6. The die-cast aluminum alloy according to claim 1, characterized in that, The alloy comprises, by mass percentage: Si 0.55%, Mg 0.85%, Mn 2.00%, Ca 0.035%, Ga 0.22%, Ti 0.20%, Zr 0.15%, Hf 0.14%, Fe 0.30%, Er 0.40%, Be 0.015%, Zn 0.25%, Sr 0.05%, Ce and La sum 0.32%, with the balance being Al and unavoidable impurities.

7. The die-cast aluminum alloy according to claim 1, characterized in that, The alloy comprises, by mass percentage: Si 0.25%, Mg 0.95%, Mn 1.60%, Ca 0.040%, Ga 0.15%, Ti 0.15%, Zr 0.10%, Hf 0.10%, Fe 0.20%, Er 0.55%, Be 0.010%, Zn 0.15%, Sr 0.15%, Ce and La sum 0.28%, with the balance being Al and unavoidable impurities.

8. The die-cast aluminum alloy according to any one of claims 1-3 and 5-7, characterized in that, The method for preparing the die-cast aluminum alloy includes the following steps: (1) Raw material melting and alloying: The raw materials are melted at 700-760℃ according to the proportion and stirred thoroughly; (2) Refining and degassing: The alloy melt is subjected to rotary argon gas refining and degassing treatment at 710-740℃; (3) Die casting: The treated melt is transferred to a die casting machine at 700-730℃ and die casting is carried out under vacuum conditions ≤50 mbar, with an injection speed ≥4 m / s; (4) Heat treatment: Hold the die casting at 170-190℃ for 45-75 minutes, then air cool.

9. The use of the die-cast aluminum alloy according to any one of claims 1 to 8 in the manufacture of metal casings for consumer electronic devices.

10. A metal casing, characterized in that, Made of the die-cast aluminum alloy as described in any one of claims 1 to 8.

Citation Information

Patent Citations

  • Heat resisting low expansion silumin and preparation thereof

    CN101503773A

  • High-thermal-conductivity heat-treatment-free die-casting rare earth aluminum alloy and method for die

    CN117888004A