A high-strength magnesium alloy and a method for improving the extrusion formability and strength of magnesium alloys
By adding Bi, Zr, Mg and Zn to ZK60 alloy, a Mg3Bi2 phase with high thermal stability was prepared, which solved the hot cracking problem of ZK60 alloy under high extrusion speed, improved extrusion formability and strength, and achieved efficient alloy processing.
Patent Information
- Application Number
- CN202611235854.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-14
- Publication Date
- 2026-11-17
AI Technical Summary
ZK60 alloy has problems such as a narrow processing window and susceptibility to hot cracking during hot working with large deformation or high extrusion speed. In addition, the cost of adding rare earth elements is high, making it difficult to use in the industrial field. Mg-Zn alloys cannot achieve both high extrusion speed and good mechanical properties.
Bi, Zr, Mg and Zn raw materials were added to ZK60 alloy, and alloy ingots were prepared by vacuum induction melting. After homogenization treatment, the ingots were water quenched and hot extruded. The extrusion ratio was set to 110:1, the temperature was 300~400℃, and the extrusion speed was 0.5~1.5mm/s, introducing the Mg3Bi2 phase with high thermal stability.
It significantly improves the hot cracking tendency of the alloy, refines the grains, enhances extrusion formability and strength, and achieves good surface quality and mechanical properties at higher extrusion speeds, with a significant increase in strength.
Smart Images

Figure CN123108374A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of magnesium alloy structural materials and their hot extrusion processing technology, specifically relating to a high-strength magnesium alloy and a method for improving the extrusion formability and strength of magnesium alloys. Background Technology
[0002] ZK60 alloy has gained increasing attention in aerospace, automotive, and digital 3C industries due to its high specific strength, low cost, and good electromagnetic shielding. However, in actual large deformation or high extrusion speed hot working processes, ZK60 alloy suffers from problems such as a narrow machinability window and susceptibility to hot cracking. Furthermore, the strength performance after hot extrusion is unsatisfactory. While adding rare earth elements can effectively improve extrusion performance and synergistically enhance strength, the high price of rare earth elements hinders large-scale industrial application. Therefore, synergistically improving the extrudability and strength of ZK60 alloy has become a critical issue that urgently needs to be addressed. In MgZn-based wrought magnesium alloys, there is also a trade-off between extrusion speed and mechanical properties. Generally, strength decreases with increasing extrusion speed. As a typical MgZn-based alloy, ZK60 alloy contains a low-melting-point MgZn phase (melting point approximately 340℃). With increasing extrusion speed and temperature within the extrusion barrel, the MgZn phase dissolves, leading to the loss of strengthening effect. This affects both extrusion speed and mechanical properties. Therefore, traditional ZK60 magnesium alloys typically achieve good performance at relatively low extrusion speeds. Synergistically improving the extrusion formability and strength properties of Mg-Zn alloys, and promoting their development, has become a key approach to achieving energy conservation, emission reduction, and green manufacturing. Summary of the Invention
[0003] To address or partially address the problems existing in related technologies, this invention proposes a high-strength magnesium alloy and a method for improving the extrusion formability and strength of the magnesium alloy.
[0004] This invention provides a method for improving the extrusion formability and strength of magnesium alloys, comprising the following steps: (1) Prepare alloy ingots by mixing Bi, Zr, Mg and Zn raw materials and using vacuum induction melting method; (2) The alloy ingot is homogenized, then water-quenched to obtain an extruded billet, and finally hot-extruded to obtain a high-strength magnesium alloy. The hot extrusion process specifically includes: preheating the extrusion billet, and then hot extruding it under the conditions of an extrusion ratio of 110:1, an extrusion temperature of 300~400℃, and a forward speed of the extrusion bar of 0.5~1.5mm / s.
[0005] Preferably, the Bi, Zr, Mg and Zn raw materials are formulated according to the following mass percentages of each element: Zn: 4.8~6.2%, Zr: 0~1%, Bi: 3.0~5.0%, Mg: balance.
[0006] More preferably, the Bi, Zr, Mg and Zn raw materials are formulated according to the following mass percentages of each element: Zn: 5.8~6.2%, Zr: 0.2~0.5%, Bi: 3.5~4.5%, Mg: balance.
[0007] More preferably, the Bi, Zr, Mg and Zn raw materials are formulated according to the following mass percentages of each element: Zn: 6.0%, Zr: 0.3%, Bi: 3.8%, Mg: balance.
[0008] Preferably, the Bi raw material is a Mg-30Bi master alloy, the Zr is a Mg-30Zr master alloy, the Zn raw material is Zn metal, and the Mg raw material is a Mg-30Bi master alloy and a Mg-30Zr master alloy.
[0009] Preferably, the vacuum induction melting method specifically includes: drawing a vacuum and introducing a protective gas, raising the temperature to 750°C within 30 minutes, holding the alloy at that temperature for 5 minutes after it melts, and then casting it into a mold and allowing it to cool naturally in the furnace to obtain an alloy ingot.
[0010] Preferably, the homogenization treatment is performed at a temperature of 370°C for 24 hours.
[0011] Preferably, the preheating temperature is 350-450℃ and the time is 1-3 hours.
[0012] This invention also claims protection for a high-strength magnesium alloy prepared by the method described above for improving the extrusion formability and strength of magnesium alloys. A non-rare earth high-strength magnesium alloy product possessing both high extrusion formability and high strength.
[0013] The technical solution provided by this invention has the following beneficial effects: This invention adds Bi element to the ZK60 alloy, introducing the Mg3Bi2 phase with high thermal stability into the alloy, significantly improving the alloy's hot cracking tendency and significantly refining the grain size. The alloy of this invention can be successfully extruded at a high extrusion speed of over 0.5 mm / s (extrusion pusher speed) under a large extrusion ratio of 110:1, improving the extrudability of the control group ZK60 by more than 100%. Simultaneously, the yield strength and ultimate tensile strength of the prepared alloy are significantly improved compared to the control group ZK60 alloy, while the elongation remains essentially unchanged. Therefore, this invention significantly improves the extrudability of ZK60 alloy while synergistically enhancing its strength. This method can be further extended to Mg-Zn alloys, synergistically improving the extrudability and strength of Mg-Zn alloys, which is of great significance for the further widespread application of Mg-Zn alloys. Attached Figure Description
[0014] Figure 1 A process flow diagram for high-strength magnesium alloys, methods for improving the extrusion formability and strength of magnesium alloys, and performance evaluation.
[0015] Figure 2 The images show the surface quality of the alloy materials prepared in Comparative Examples 1-3. (a) is Comparative Example 1, (b) is Comparative Example 2, and (c) is Comparative Example 3.
[0016] Figure 3 Comparison of the mechanical properties of the alloy materials prepared in Comparative Examples 1-2.
[0017] Figure 4 The images show the surface quality of the alloy materials prepared in Examples 1-3. (a) is Example 1, (b) is Example 2, and (c) is Example 3.
[0018] Figure 5 The graph shows a comparison of the mechanical properties of the alloy materials prepared in Examples 1-3.
[0019] Figure 6 The images are SEM-EDS images of the alloy materials prepared in Comparative Examples 1 and 2. (a) is Comparative Example 1, and (b) is Comparative Example 2.
[0020] Figure 7 The images show SEM-EDS images of the alloy materials prepared in Examples 1-3, with (a) representing Example 1, (b) representing Example 2, and (c) representing Example 3. Detailed Implementation
[0021] To better understand the technical content of this invention, specific embodiments are provided below to further illustrate this invention.
[0022] like Figure 1As shown, a high-strength magnesium alloy and a method for improving the extrusion formability and strength of the magnesium alloy include the following steps: Step 1: Based on commercially available ZK60 grade magnesium alloy, Bi element is melted to obtain ZK60-4Bi (ZKB604) alloy, whose chemical composition by mass percentage (wt%) is as follows: Zn: 4.8~6.2% Zr: 0~1% Bi: 3.0~5.0% Mg: Balance.
[0023] The chemical composition of the further optimized elements, expressed as a mass percentage (wt%), is as follows: Zn: 5.8~6.2% Zr: 0.2~0.5% Bi: 3.5~4.5% Mg: Balance.
[0024] The chemical composition of the further optimized elements, expressed as a mass percentage (wt%), is as follows: Zn: 6.0% Zr: 0.3% Bi: 3.8% Mg: Balance.
[0025] Step Two: Weigh the alloying elements according to the alloy composition designed in Step One. The Bi element is a Mg-30Bi master alloy, and the Zr element is a Mg-30Zr master alloy; Zn is an industrially pure metal (≥99.99wt%). The alloy ingot is prepared using a vacuum induction melting method. First, the proportioned alloy raw materials are placed in a graphite crucible, a vacuum is drawn, and a protective gas environment (SF6:CO2 volume ratio = 1:99) is introduced. By controlling the power of the vacuum induction furnace, the temperature is raised to 750℃ within 30 minutes. After the alloy melts, it is held at that temperature for 5 minutes and then poured into a stainless steel mold. After naturally cooling in the furnace for 40 minutes, the sample is removed, thus obtaining the ZKB604 alloy ingot.
[0026] Step 3: The ZKB604 alloy ingot obtained through melting and casting is homogenized at 370℃ for 24 hours and then water-quenched. After that, the surface oxide layer is ground off and the ingot is machined to obtain an ingot with a diameter of 95mm. The homogenized alloy ingot is then cut into extrusion blanks with a thickness of about 80mm using an EDM CNC wire cutting machine, and hot extrusion processing is carried out.
[0027] Step 4: Set the extrusion speed gradient and perform hot extrusion at different extrusion speeds. Hot extrusion experiments were conducted on homogenized extrusion billets. Before hot extrusion, the billets were preheated to 350–450°C for 1–3 hours. Simultaneously, the extrusion cylinder and die were preheated to 300–400°C for 1–3 hours. The extrusion parameters were: a maximum extrusion ratio of 110:1, an extrusion temperature of 300–400°C, and an extrusion speed of 0.5–1.5 mm / s.
[0028] Step 5: Surface quality and performance testing at different extrusion speeds Macroscopic surface quality observation and room temperature mechanical property testing were performed on the extruded ZKB604 alloy bars obtained in step four. First, a 2mm thick and 60mm long sheet was cut from the center of the extruded alloy bar along the extrusion direction using an EDM CNC wire cutter. Then, it was cut into "dog bone" tensile specimens conforming to the national standard GB / T 228.1-2021 "Metallic materials, tensile testing - Part 1: Test at room temperature" (gauge length 12mm; width 3mm; thickness 2mm). Tensile tests were then performed on the extruded alloy using a universal testing machine.
[0029] To make the technical means, creative features, objectives and effects of the present invention clearer, the present invention will be further described below in conjunction with specific embodiments and comparative examples.
[0030] Example 1 A method for improving the extrusion formability and strength of magnesium alloys, comprising the following steps: Step 1: Combine Mg-30Bi (wt.%) master alloy, Mg-30Zr (wt.%) master alloy, industrial pure Zn (≥99.99 wt%), and industrial pure Mg (≥99.99 wt%) according to the following alloy ratio (wt%): Zn 6.0% : Zr 0.3% : Bi 3.8%, with the balance being magnesium. Place the prepared alloy raw materials into a vacuum induction melting furnace under a protective gas environment (SF6:CO2=1:99); heat to 750℃, hold for 5 minutes after the alloy melts, and then cast. Cool in the furnace for 40 minutes to obtain ZKB604 magnesium alloy ingot.
[0031] Step 2: After homogenizing the magnesium alloy ingot obtained in Step 1 at 370℃ for 24 hours, water quench it, grind off the surface oxide layer, and then perform wire electrical discharge machining to obtain an extruded billet with a thickness of 80 mm and a diameter of 95 mm.
[0032] Step 3: The extruded billet obtained in Step 2 is subjected to hot extrusion. Before hot extrusion, the billet is preheated at 400℃ for 2 hours, and the extrusion cylinder and extrusion die are preheated at 350℃ for 2 hours. The extrusion ratio is 110:1, the extrusion temperature is 350℃, and the extrusion speed of the extrusion bar is 0.5 mm / s. This yields an extruded ZKB604 alloy bar with a diameter of 10 mm.
[0033] Step 4: Observe the surface quality and conduct room temperature tensile mechanical property tests on the extruded ZKB604 alloy bar obtained in Step 3. First, use an electrical discharge wire cutting device to cut the bar from the center into extruded alloy sheets with a thickness of 2 mm, a length of 60 mm, and a width of 10 mm. Then, according to the national standard GB / T 228.1-2021, cut dog-bone shaped tensile specimens from these sheets. The gauge length dimensions are: length 12 mm; width 3 mm; thickness 2 mm. Perform tensile property tests in a universal testing machine.
[0034] according to Figure 4 The ZKB604 alloy exhibits a smooth surface texture, a strong silvery-white metallic luster, and fine extrusion striations at an extrusion speed of 0.5 mm / s, indicating good surface quality. Under these conditions, the alloy demonstrates a yield strength of 344.99 MPa, a tensile strength of 461.40 MPa, and an elongation of 8.35%, exhibiting high strength properties.
[0035] Example 2 The only difference between this embodiment of a high-strength magnesium alloy and a method for improving the extrusion formability and strength of a magnesium alloy and the method for improving the extrusion formability and strength of a magnesium alloy in Embodiment 1 is that in step three, the extrusion speed of the extrusion bar is a relatively high 1.0 mm / s.
[0036] according to Figure 4 At this extrusion speed, the surface texture is relatively smooth, exhibiting a silvery-white metallic luster and fine extrusion striations, indicating good surface quality. The yield strength is 360.62 MPa; the tensile strength is 489.49 MPa; and the elongation is 11.46%. The remaining steps are consistent with Embodiment 1. In this embodiment, the alloy combines a relatively fast extrusion speed with high mechanical properties, thus confirming that the present invention achieves a synergistic improvement in extrudability and strength.
[0037] Example 3 The method for improving the extrusion formability and strength of magnesium alloys in this embodiment differs from the method for improving the extrusion formability and strength of magnesium alloys in Embodiment 1 only in that the extrusion speed of the extrusion bar in step three is a higher 1.5 mm / s. The remaining steps are the same as in Embodiment 1.
[0038] according to Figure 4 At this extrusion speed, the surface shows oxidation and blackening, accompanied by fine extrusion hot cracks. At this time, the yield strength of the alloy is 250.19 MPa; the tensile strength is 329.01 MPa; and the elongation is 7.02%.
[0039] Comparative Example 1 A method for preparing a high-strength magnesium alloy includes the following steps: Step 1: This comparative case uses traditional ZK60 magnesium alloy without added Bi. Its composition by mass percentage (wt%) is: Zn: 6.1%; Zr: 0.4%; balance Mg. Zr is incorporated through a Mg-30Zr binary alloy, Zn is industrially pure Zn (≥99.99 wt%), and Mg is industrially pure magnesium (≥99.9 wt%).
[0040] Step 2: The ZK60 magnesium alloy ingot obtained in Step 1 is homogenized and heat-treated at 370℃ for 24 hours, then water-quenched. After grinding off the surface oxide layer, it is subjected to wire electrical discharge machining to obtain an extruded billet with a thickness of 80 mm and a diameter of 95 mm.
[0041] Step 3: The ZK60 extruded billet obtained in Step 2 is subjected to hot extrusion. Before hot extrusion, the billet is preheated at 400℃ for 2 hours, and the extrusion cylinder and extrusion die are preheated at 350℃ for 2 hours. The extrusion ratio is 110:1, the extrusion temperature is 350℃, and the extrusion speed is 0.2 mm / s. This yields an extruded ZK60 alloy bar with a diameter of 10 mm.
[0042] Step 4: Observe and assess the surface quality of the extruded ZK60 alloy bar obtained in Step 3, and then conduct room temperature tensile mechanical property tests. First, use an electrical discharge wire cutting device to cut the bar from the center into extruded alloy sheets with a thickness of 2 mm, a length of 60 mm, and a width of 10 mm. Then, according to the national standard GB / T 228.1-2021, cut "dog bone" shaped tensile specimens from these sheets. The gauge length dimensions are: length 12 mm; width 3 mm; thickness 2 mm. Tensile property tests are then conducted in a universal testing machine.
[0043] according to Figure 2 The ZK60 alloy exhibits a smooth surface texture, a strong silvery-white metallic luster, and fine extrusion striations at an extrusion speed of 0.2 mm / s, indicating good surface quality. At this speed, the ZK60 alloy has a yield strength of 321.19 MPa, a tensile strength of 369.31 MPa, and an elongation of 6.90%. While this alloy possesses good strength, its high strength can only be achieved at a relatively low extrusion speed of 0.2 mm / s.
[0044] Comparative Example 2 The only difference between the preparation method of ZK60 magnesium alloy in this comparative example and the preparation method of ZK60 magnesium alloy in Comparative Example 1 is that in step three, the extrusion speed of the extrusion bar is a relatively high 0.5 mm / s.
[0045] according to Figure 2 At this extrusion speed, the surface quality of ZK60 alloy is generally poor. At this point, the alloy's yield strength is 199.23 MPa; tensile strength is 315.56 MPa; and elongation is 11.07%, indicating a significant decrease in strength properties.
[0046] according to Figure 6 and Figure 7 It can be seen that the alloys prepared in Examples 1-3 and Comparative Examples 1-2 have a uniform distribution of each element.
[0047] The ZK60 alloys prepared in Comparative Examples 1-2 contain a low-melting-point MgZn phase with poor thermal stability. Therefore, as the extrusion speed increases, the MgZn phase dissolves into the matrix. In contrast, the ZKB604 alloys prepared in Examples 1-3 introduce a high-melting-point Mg3Bi2 phase with excellent thermal properties. This phase remains stable with increasing extrusion speed, improving the hot cracking tendency and extrudability of the ZKB604 alloy, while also providing significant second-phase strengthening, thus further enhancing the alloy's strength. This results in a synergistic improvement in both the extrudability and strength of the alloy.
[0048] Comparative Example 3 The only difference between the preparation method of ZK60 magnesium alloy in this comparative example and the preparation method of ZK60 magnesium alloy in Comparative Example 1 is that in step three, the extrusion speed of the extrusion bar is a relatively high 1.0 mm / s.
[0049] according to Figure 2 At this extrusion speed, the ZK60 alloy exhibited slight oxidation on its surface, along with extrusion hot cracks. With increasing extrusion speed, the alloy's yield strength, tensile strength, and elongation showed a significant decreasing trend. Therefore, the alloy prepared in Comparative Example 3 had lower yield strength, tensile strength, and elongation than Comparative Example 2.
[0050] Comparative Example 4 This comparative example describes a method for preparing a ZK60-1.1Bi magnesium alloy. The difference from the high-strength magnesium alloy and the method for improving the extrusion formability and strength of the magnesium alloy in Example 1 is that: in step one, the mass percentage of Bi is 1.09%; in step three, the extrusion ratio is 60:1; and the extrusion speed is 0.5 m / min (equivalent to an extrusion bar forward speed of 0.14 mm / s).
[0051] Under these conditions, neither the extrudability nor the strength properties of the alloy were improved. This is because the Mg3Bi2 phase was not formed in the ZK60-1.1Bi magnesium alloy; instead, a compound rich in Zn, Zr, and Bi was formed. At an extrusion speed of 0.14 mm / s, the Mg3Bi2 phase, which can provide support, was absent, thus failing to improve the extrudability. Furthermore, its yield strength was 290 MPa and its tensile strength was 345 MPa. Compared to the ZK60 alloy in Comparative Example 1, which had a yield strength of 321.19 MPa and a tensile strength of 369.31 MPa, the strength decreased, and therefore, the strength properties of the alloy were not improved either.
[0052] Examples 1-3 and Comparative Examples 1-4 lead to the conclusion that adding Bi to ZK60 alloy to form ZK60-4Bi (ZKB604) alloy can successfully extrude at a high extrusion speed of 1.0 mm / s under a large extrusion ratio of 110:1, with good surface quality, and high yield strength, tensile strength and elongation, achieving a synergistic improvement in extrusion formability and strength.
[0053] The various embodiments of the present invention have been described above. These descriptions are exemplary and not exhaustive, nor are they limited to the disclosed embodiments. Many modifications and variations will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments. The terminology used herein is chosen to best explain the principles, practical application, or improvement of the technology in the market, or to enable others skilled in the art to understand the embodiments disclosed herein.
Claims
1. A method for improving the extrusion formability and strength of magnesium alloys, characterized in that, Includes the following steps: (1) Prepare alloy ingots by mixing Bi, Zr, Mg and Zn raw materials and using vacuum induction melting method; (2) The alloy ingot is homogenized, then water-quenched to obtain an extruded billet, and finally hot-extruded to obtain a high-strength magnesium alloy. The hot extrusion process specifically includes: preheating the extrusion billet, and then hot extruding it under the conditions of an extrusion ratio of 110:1, an extrusion temperature of 300~400℃, and a forward speed of the extrusion bar of 0.5~1.5mm / s.
2. The method for improving the extrusion formability and strength of magnesium alloys as described in claim 1, characterized in that, The Bi, Zr, Mg and Zn raw materials are formulated according to the following mass percentages of each element: Zn: 4.8~6.2%, Zr: 0~1%, Bi: 3.0~5.0%, Mg: balance.
3. The method for improving the extrusion formability and strength of magnesium alloys as described in claim 1, characterized in that, The Bi, Zr, Mg and Zn raw materials are formulated according to the following mass percentages of each element: Zn: 5.8~6.2%, Zr: 0.2~0.5%, Bi: 3.5~4.5%, Mg: balance.
4. The method for improving the extrusion formability and strength of magnesium alloys as described in claim 1, characterized in that, The Bi, Zr, Mg and Zn raw materials are formulated according to the following mass percentages of each element: Zn: 6.0%, Zr: 0.3%, Bi: 3.8%, Mg: balance.
5. The method for improving the extrusion formability and strength of magnesium alloys as described in claim 1, characterized in that, The Bi raw material is a Mg-30Bi master alloy, the Zr is a Mg-30Zr master alloy, the Zn raw material is Zn metal, and the Mg raw materials are a Mg-30Bi master alloy and a Mg-30Zr master alloy.
6. The method for improving the extrusion formability and strength of magnesium alloys as described in claim 1, characterized in that, The vacuum induction melting method specifically includes: drawing a vacuum and introducing a protective gas, raising the temperature to 700℃-800℃ within 30 minutes, holding the melted alloy at that temperature for 5-10 minutes, and then casting the molten alloy into a mold and allowing it to cool naturally in the furnace to obtain an alloy ingot.
7. The method for improving the extrusion formability and strength of magnesium alloys as described in claim 1, characterized in that, The homogenization process was carried out at a temperature of 370°C for 24 hours.
8. The method for improving the extrusion formability and strength of magnesium alloys as described in claim 1, characterized in that, The preheating temperature is 350-450℃, and the time is 1-3 hours.
9. The high-strength magnesium alloy prepared by the method for improving the extrusion formability and strength of magnesium alloy as described in claim 1.