A method for producing 1180MPa grade galvanized duplex steel strip for automotive structures
By employing a synergistic process encompassing smelting and continuous casting, hot rolling, pickling and cold rolling, and continuous annealing and hot-dip galvanizing, several problems in the production of galvanized duplex steel strip in existing technologies have been solved. This has enabled stable production of 1180MPa grade steel strip and good coating adhesion, meeting the performance requirements of automotive structural components.
Patent Information
- Application Number
- CN202611393477.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-09
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies for producing 1180MPa grade galvanized duplex steel strip suffer from problems such as low elongation, stamping cracking, insufficient hole expansion and bending performance, insufficient cooling capacity of hot-dip galvanizing lines, difficulty in controlling martensite volume fraction and uniformity, high alloy cost, and narrow process window, making it difficult to achieve stable production and good coating adhesion.
The entire process of smelting and continuous casting → hot rolling → pickling and cold rolling → continuous annealing and hot-dip galvanizing → finishing is adopted. Through specific chemical composition design and process parameter control, including composition design, smelting and continuous casting, hot rolling, pickling and cold rolling, continuous annealing and hot-dip galvanizing and finishing processes, the performance of steel strip and coating quality are ensured.
It achieves stable production with low cost and wide process window. The tensile strength, yield strength, elongation after fracture and hole expansion rate of the steel strip meet the requirements. The coating has good adhesion and is suitable for automotive structural parts, improving the forming performance and corrosion resistance.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of automotive high-strength steel manufacturing technology, and particularly relates to a production method of 1180MPa grade galvanized duplex steel strip for automotive structures. Background Technology
[0002] The pursuit of lightweighting and improved crash safety in automobiles is driving the upgrade of vehicle body structural components to 1180MPa-grade ultra-high-strength dual-phase steel; continuous hot-dip galvanizing, combining high strength, formability, and corrosion resistance, is the mainstream technological approach. Existing technologies face the following bottlenecks:
[0003] 1. High strength can easily lead to low elongation, stamping cracking, and insufficient hole expansion and bending performance;
[0004] 2. Insufficient cooling capacity of hot-dip galvanizing lines makes it difficult to control the volume fraction and uniformity of martensite, resulting in large performance fluctuations;
[0005] 3. The alloy has high cost and narrow process window, making it difficult to achieve both stable industrial production and coating adhesion and surface quality.
[0006] This invention achieves stable industrial production by coordinating the entire process of composition, hot rolling, cold rolling, continuous annealing, hot-dip galvanizing, and finishing, thus meeting the service requirements of automotive structural components. Summary of the Invention
[0007] The purpose of this invention is to provide a low-cost, wide-process-window, and stable production method for 1180MPa grade galvanized duplex steel strip, ensuring tensile strength ≥1180MPa, yield strength ≥820MPa, elongation after fracture ≥10%, hole expansion rate ≥35%, and uniform and well-adhered coating, suitable for structural components such as automotive B-pillars, door sill beams, and crash beams.
[0008] To solve the above-mentioned technical problems, the present invention adopts the following technical solution:
[0009] This invention discloses a method for producing 1180MPa grade galvanized duplex steel strip for automotive structures, comprising: smelting and continuous casting → hot rolling → pickling and cold rolling → continuous annealing and hot-dip galvanizing → finishing; characterized in that: specifically:
[0010] (1) Design of chemical composition by mass percentage
[0011] C: 0.12–0.18%; Si: 0.20–0.50%; Mn: 1.80–2.40%; Als: 0.020–0.060%; Cr: 0.20–0.50%; Nb: 0.010–0.030%; Ti: 0.008–0.025%; P≤0.015%; S≤0.003%; N≤0.004%; O≤0.003%; Balance Fe and unavoidable impurities;
[0012] (2) Smelting and continuous casting
[0013] Converter / electric furnace smelting → LF refining → RH vacuum degassing → continuous casting billet; control hydrogen ≤ 2.0 ppm and oxygen ≤ 30 ppm; continuous casting billet thickness 180~230 mm, no surface defects and low segregation;
[0014] (3) Hot rolling process
[0015] Reheating of the billet: 1190~1250℃, holding time to ensure homogenization and full solution dissolution of the alloy;
[0016] Descaling: High-pressure water descaling ≥ 2 times, descaling pressure ≥ 18MPa;
[0017] Rough rolling: initial rolling temperature 1050~1150℃, total reduction ≥65%;
[0018] Finishing rolling: finishing rolling temperature 860~910℃, total reduction rate ≥75%;
[0019] Laminar flow cooling: ultra-fast cooling, winding temperature 520~580℃;
[0020] The target thickness of the hot-rolled coil is 2.0 to 4.0 mm, with a microstructure of ferrite and pearlite and uniform hardness.
[0021] (4) Pickling and cold rolling
[0022] Continuous pickling removes iron oxide scale, and the matching of acid temperature, speed and concentration ensures surface cleanliness;
[0023] The cold rolling reduction rate is 50-70%, and the thickness after cold rolling is 0.6-2.5 mm; the sheet shape is good and the thickness accuracy is ±0.01 mm;
[0024] (5) Continuous annealing hot-dip galvanizing
[0025] Preheating: Raise the temperature to 250-350℃ to remove residual oil and moisture;
[0026] Pre-oxidation: Control the dew point to -10 to +10℃ to form a uniform thin oxide layer, which improves subsequent reduction and wettability;
[0027] Reduction homogenization: 780~820℃, holding for 60~120s; protective atmosphere: H23~6vol%, balance N2, dew point -40~-60℃; achieving complete recrystallization + partial austenitization.
[0028] Rapidly cool to galvanizing temperature: cool to 450-470℃ at 30-60℃ / s, then place in the zinc pot;
[0029] Hot-dip galvanizing: Zinc bath Al 0.20~0.35wt%, temperature 455~475℃, strip steel temperature difference upon entering the bath ≤±3℃; air knife controls coating thickness to 40~90g / m² on one side. 2 ;
[0030] Rapid cooling after galvanizing: Cooling to ≤200℃ at ≥50℃ / s to stabilize the duplex structure and inhibit tempering softening;
[0031] Over-aging: 180~220℃, hold for 30~80s, adjust residual stress, improve forming and expand hole;
[0032] (6) Smoothing
[0033] The finishing elongation is 0.4-1.2%, eliminating the yield plateau, improving the shape and surface roughness, and enhancing the stability of stamping.
[0034] Furthermore, product performance
[0035] Mechanical properties: Rm≥1180MPa, Rp0.2≥820MPa, A≥10%, HV 360~420;
[0036] Microstructure: Ferrite + 18-28% homogeneous martensite, grain size 5-10 μm;
[0037] Forming: Pore expansion ratio ≥35%, no cracks after 90° bending (d=a);
[0038] Coating: Pure zinc GI / alloyed GA optional, with good adhesion, no missed plating, and no zinc dross.
[0039] Further, the chemical composition by mass percentage is designed as follows: C 0.15%, Si 0.35%, Mn 2.10%, Als 0.040%, Cr 0.35%, Nb 0.020%, Ti 0.015%, P 0.010%, S 0.002%; balance Fe and unavoidable impurities.
[0040] Further, the chemical composition by mass percentage is designed as follows: C 0.14%, Si 0.30%, Mn 2.00%, Als 0.040%, Cr 0.30%, Nb 0.018%, Ti 0.012%, P 0.010%, S 0.002%; balance Fe and unavoidable impurities.
[0041] Furthermore, the coating is GI pure zinc, with a single-sided coating of 40–90 g / m². 2 .
[0042] Furthermore, it is used to produce steel strips with a thickness of 0.6–2.5 mm and a width of 800–1850 mm.
[0043] Compared with the prior art, the beneficial technical effects of the present invention are as follows:
[0044] 1. Strength-plasticity balance: Rm≥1180MPa, A≥10%, meeting the stamping requirements of complex structural parts;
[0045] 2. Controllable microstructure: Ferrite + 18-28% uniform martensite, with performance fluctuation ≤ ±50MPa;
[0046] 3. Excellent coating: no missed plating, no zinc slag, qualified adhesion, and corrosion resistance meets the requirements of the whole vehicle;
[0047] 4. Low cost: Less Mo and Ni, micro-alloyed Nb / Ti refines grain size, reducing costs by 10-20%;
[0048] 5. Stable industrial production: Wide process window, compatible with conventional hot-dip galvanizing lines, with a yield rate of ≥97%. Detailed Implementation
[0049] Example 1 (thickness 1.40mm)
[0050] Composition (wt%): C 0.15%, Si 0.35%, Mn 2.10%, Als 0.040%, Cr 0.35%, Nb 0.020%, Ti0.015%, P 0.010%, S 0.002%.
[0051] Hot rolling: heating at 1220℃; final rolling at 880℃; coiling at 550℃; hot rolling thickness 3.00mm.
[0052] Cold rolling: reduction rate 53.3%; finished product thickness 1.40mm.
[0053] Annealing and galvanizing: soaking at 800℃ / 90s; H2 5vol%; dew point -50℃; cooling to 460℃; zinc liquid 465℃; Al 0.28%; post-cooling at 70℃ / s; over-aging at 200℃ / 60s.
[0054] Finishing: 0.8% elongation.
[0055] Performance: Rm=1210MPa, Rp0.2=860MPa, A=12.0%, hole expansion rate=38%; coating weight per side 60g / m 2 The bending test is satisfactory.
[0056] Example 2 (thickness 1.00mm)
[0057] Composition (wt%): C 0.14%, Si 0.30%, Mn 2.00%, Als 0.040%, Cr 0.30%, Nb 0.018%, Ti0.012%, P 0.010%, S 0.002%.
[0058] Hot rolling: heating to 1210℃; final rolling at 875℃; coiling at 540℃, hot-rolled thickness 2.60mm.
[0059] Cold rolling: reduction rate 62.5%; finished product thickness 1.00mm.
[0060] Annealing and galvanizing: heat treatment at 795℃ / 80s; cooling to 460℃; post-cooling at 65℃ / s; aging at 190℃ / 50s.
[0061] Finishing: 0.6% elongation.
[0062] Performance: Rm=1195MPa, Rp0.2=845MPa, A=11.5%, expansion rate=37%.
[0063] This invention is applicable to continuous hot-dip galvanizing production lines and can produce steel strips with a thickness of 0.6 to 2.5 mm and a width of 800 to 1850 mm for use in automotive B-pillars, door sills, anti-collision beams, longitudinal beams, and other structural components, and is compatible with mainstream automotive material standards.
[0064] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.
Claims
1. A method for producing 1180MPa grade galvanized duplex steel strip for automotive structures, comprising: Smelting and continuous casting → hot rolling → pickling and cold rolling → continuous annealing and hot-dip galvanizing → finishing; characterized in that: specifically: (1) Design of chemical composition by mass percentage C: 0.12–0.18%; Si: 0.20–0.50%; Mn: 1.80–2.40%; Als: 0.020–0.060%; Cr: 0.20–0.50%; Nb: 0.010–0.030%; Ti: 0.008–0.025%; P≤0.015%; S≤0.003%; N≤0.004%; O≤0.003%; Balance Fe and unavoidable impurities; (2) Smelting and continuous casting Converter / electric furnace smelting → LF refining → RH vacuum degassing → continuous casting billet; control hydrogen ≤ 2.0 ppm and oxygen ≤ 30 ppm; continuous casting billet thickness 180~230 mm, no surface defects and low segregation; (3) Hot rolling process Reheating of the billet: 1190~1250℃, holding time to ensure homogenization and full solution dissolution of the alloy; Descaling: High-pressure water descaling ≥ 2 times, descaling pressure ≥ 18MPa; Rough rolling: initial rolling temperature 1050~1150℃, total reduction ≥65%; Finishing rolling: finishing rolling temperature 860~910℃, total reduction rate ≥75%; Laminar flow cooling: ultra-fast cooling, winding temperature 520~580℃; The target thickness of the hot-rolled coil is 2.0 to 4.0 mm, with a microstructure of ferrite and pearlite and uniform hardness. (4) Pickling and cold rolling Continuous pickling removes iron oxide scale, and the matching of acid temperature, speed and concentration ensures surface cleanliness; The cold rolling reduction rate is 50-70%, and the thickness after cold rolling is 0.6-2.5 mm; the sheet shape is good and the thickness accuracy is ±0.01 mm; (5) Continuous annealing hot-dip galvanizing Preheating: Raise the temperature to 250-350℃ to remove residual oil and moisture; Pre-oxidation: Control the dew point to -10 to +10℃ to form a uniform thin oxide layer, which improves subsequent reduction and wettability; Reduction homogenization: 780~820℃, holding for 60~120s; protective atmosphere: H23~6vol%, balance N2, dew point -40~-60℃; achieving complete recrystallization + partial austenitization. Rapidly cool to galvanizing temperature: cool to 450-470℃ at 30-60℃ / s, then place in the zinc pot; Hot-dip galvanizing: Zinc bath Al 0.20~0.35wt%, temperature 455~475℃, strip steel temperature difference upon entering the bath ≤±3℃; air knife controls coating thickness to 40~90g / m² on one side. 2 ; Rapid cooling after galvanizing: Cooling to ≤200℃ at ≥50℃ / s to stabilize the duplex structure and inhibit tempering softening; Over-aging: 180~220℃, hold for 30~80s, adjust residual stress, improve forming and expand hole; (6) Smoothing The finishing elongation is 0.4-1.2%, eliminating the yield plateau, improving the shape and surface roughness, and enhancing the stability of stamping.
2. The method for producing 1180MPa grade galvanized duplex steel strip for automotive structures according to claim 1, characterized in that: The mechanical properties of the obtained steel strip meet the following requirements: Rm≥1180MPa, Rp0.2≥820MPa, A≥10%, and expansion ratio≥35%; The microstructure consists of ferrite + 18-28% martensite.
3. The method for producing 1180MPa grade galvanized duplex steel strip for automotive structures according to claim 1, characterized in that: Grain size 5–10 μm.
4. The method for producing 1180MPa grade galvanized duplex steel strip for automotive structures according to claim 1, characterized in that: Chemical composition design by mass percentage: C 0.15%, Si 0.35%, Mn 2.10%, Als 0.040%, Cr 0.35%, Nb 0.020%, Ti 0.015%, P 0.010%, S 0.002%; balance Fe and unavoidable impurities.
5. The method for producing 1180MPa grade galvanized duplex steel strip for automotive structures according to claim 1, characterized in that: Chemical composition design by mass percentage: C 0.14%, Si 0.30%, Mn 2.00%, Als 0.040%, Cr 0.30%, Nb 0.018%, Ti 0.012%, P 0.010%, S 0.002%; balance Fe and unavoidable impurities.
6. The method for producing 1180MPa grade galvanized duplex steel strip for automotive structures according to claim 1, characterized in that: The coating is made of GI pure zinc, with a single-sided coating of 40–90 g / m². 2 .
7. The method for producing 1180MPa grade galvanized duplex steel strip for automotive structures according to claim 1, characterized in that: Used for producing steel strips with a thickness of 0.6–2.5 mm and a width of 800–1850 mm.