Ultra-thick structural steel with excellent resistance to brittle fracture initiation and its manufacturing method
By controlling the alloy composition and manufacturing process, the problem of brittle fracture initiation resistance in the central part of ultra-thick high-strength steel was solved, achieving high strength and excellent brittle fracture initiation resistance, which is suitable for the manufacture of ultra-thick structural steel.
Patent Information
- Application Number
- CN202611302487.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2018-12-19
- Filing Date
- 2019-12-02
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies are insufficient to effectively improve the resistance to brittle fracture initiation in ultra-thick high-strength steel, especially when there are large low-temperature transformation phases or uneven defects in the central part, which leads to a significant reduction in the resistance to brittle fracture initiation, and the resistance to brittle fracture initiation in the welded area is difficult to guarantee.
By controlling the alloy composition and manufacturing process, the area fraction of acicular ferrite and granular bainite in ultra-thick structural steel is ensured to be 80% or greater, and the sum of crack lengths is 130 μm or less. Ultra-thick structural steel with excellent resistance to brittle fracture initiation is prepared by using RH refining, continuous casting, reheating, rough rolling, finish rolling and high cooling rate process.
It effectively reduces defects in the center of steel, ensures a yield strength of 500 MPa or higher, an average crack tip opening displacement of 0.4 mm or greater in the base material at -10℃, and an impact transition temperature of -40℃ or lower in the center, significantly improving resistance to brittle fracture initiation.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
[0001] This application is a divisional application of Chinese patent application filed on December 2, 2019, with application number "201980084490.9" and invention title "Ultra-thick structural steel with excellent resistance to brittle fracture initiation and its manufacturing method". The original application is the Chinese national phase application of international application PCT / KR2019 / 016840. Technical Field
[0002] This disclosure relates to ultra-thick structural steel with excellent resistance to brittle fracture initiation and a method for manufacturing the same. Background Technology
[0003] In recent years, there has been a need to develop ultra-thick, high-strength steel for structural design in shipbuilding and other industries both domestically and internationally. When high-strength steel is used in structural design, it can reduce the weight of such structures to achieve economic benefits, and it can also allow for thinner steel plates while ensuring ease of machining and welding.
[0004] Typically, when manufacturing high-strength steel using ultra-thick steel plates, the overall microstructure may not deform sufficiently due to the increased total reduction rate. Consequently, the microstructure may become coarser, and during quenching, the large thickness may lead to a difference in cooling rates between the surface and central portions. This can cause coarse low-temperature transformation phases, such as bainite, to form on the surface, making it difficult to ensure toughness.
[0005] In detail, existing marine structures alone require guarantees of resistance to brittle fracture initiation, a key indicator of structural stability. In recent years, there has been an increasing number of cases where even in shipbuilding, such as in very large vessels, primary structures require guarantees of resistance to brittle fracture initiation. However, when large low-temperature transformation phases or inhomogeneous defects are present in the central portion, the resistance to brittle fracture initiation can be significantly reduced. Therefore, improving the resistance to brittle fracture initiation in ultra-thick, high-strength steel can be extremely difficult.
[0006] Furthermore, while research has focused on ensuring the physical properties of the weld zone in the context of brittle fracture initiation resistance, the guarantee of the brittle fracture initiation resistance of the base material itself has been improving in recent years. However, when manufacturing ultra-thick steel plates, the addition of large amounts of alloying elements and the reduction in reduction rate can make it very difficult to remove defects that appear in the central portion. Due to such residual defects, it may be difficult to guarantee the brittle fracture initiation resistance of the base material itself. In addition, such residual defects may reduce the brittle fracture initiation resistance of the weld zone.
[0007] In the case of existing ultra-thick high-strength steels with yield strengths of 500 MPa or higher, efforts have been made to improve the resistance to brittle fracture initiation in the weld zone by: refining the microstructure of the heat-affected zone using titanium nitride (TiN) (see Patent Document 1), forming ferrite in the heat-affected zone using oxide metallurgy (see Patent Document 2), or designing and applying low-alloy components. Unfortunately, such efforts may offer some help in improving the resistance to brittle fracture initiation in the weld zone, but may not be a fundamental countermeasure against residual defects that have a major impact on reducing the resistance to brittle fracture initiation. Therefore, there is a need for new methods.
[0008] [Related Technical Documents]
[0009] (Patent Document 1) Japanese Patent Publication No. 2010-095781
[0010] (Patent Document 2) Japanese Patent Publication No. 2009-138255 Summary of the Invention
[0011] Technical issues
[0012] One aspect of this disclosure is to provide ultra-thick structural steel with excellent resistance to brittle fracture initiation and a method for manufacturing the same.
[0013] Technical solution
[0014] According to one aspect of this disclosure, the ultra-thick structural steel with excellent resistance to brittle fracture initiation comprises, by weight percent, C: 0.03% to 0.08%, Mn: 1.6% to 2.2%, Ni: 0.6% to 1.3%, Nb: 0.005% to 0.03%, Ti: 0.005% to 0.02%, Cu: 0.1% to 0.4%, P: 100 ppm or less, S: 40 ppm or less, H: 1.5 ppm or less, and the balance being Fe and unavoidable impurities. By area fraction, the sum of acicular ferrite and granular bainite in the microstructure is 80% or greater, per 1 mm in the region ±1 mm from the thickness center of the steel. 2 The total length of cracks with a size of 30 μm or larger per unit area is 130 μm or smaller, and the yield strength is 500 MPa or higher.
[0015] According to another aspect of this disclosure, a method for manufacturing ultra-thick structural steel with excellent resistance to brittle fracture initiation includes: preparing molten steel containing, by weight percent: C: 0.03% to 0.08%, Mn: 1.6% to 2.2%, Ni: 0.6% to 1.3%, Nb: 0.005% to 0.03%, Ti: 0.005% to 0.02%, Cu: 0.1% to 0.4%, P: 100 ppm or less, S: 40 ppm or less, H: 1.5%. ppm or less, and the balance of Fe and unavoidable impurities; continuous casting of molten steel to obtain a billet; reheating the billet to a temperature of 1000°C to 1150°C; rough rolling of the reheated billet at a temperature of 900°C to 1150°C; finish rolling of the rough-rolled billet at an Ar3 temperature or higher, based on 1 / 4t (where "t" is the thickness of the steel), to obtain hot-rolled steel; and cooling the hot-rolled steel to a temperature of 300°C to 600°C at a cooling rate of 3°C / second or higher, the preparation of molten steel including RH refining of molten steel for 15 minutes to 40 minutes.
[0016] Beneficial effects
[0017] As described above, defects in the central portion of steel can be effectively reduced to provide ultra-thick structural steel with excellent resistance to brittle fracture initiation and a method for manufacturing such steel. Detailed Implementation
[0018] The following describes ultra-thick structural steels with excellent resistance to brittle fracture initiation. First, the alloy composition of this disclosure will be described. Unless otherwise stated, the content of the alloy composition described below is expressed in weight percent.
[0019] C: 0.03% to 0.08%
[0020] Since carbon (C) is the most important element in ensuring basic strength, it may need to be included in steel within an appropriate range. When the C content exceeds 0.08%, a large amount of martensitic-austenitic (MA) components and low-temperature transformation phases may form in the base material and heat-affected zone, thereby deteriorating toughness. When the C content is below 0.03%, strength may decrease. Therefore, the C content is preferably in the range of 0.03% to 0.08%. The lower limit of the C content can be more specifically 0.035%, more specifically 0.037%, and even more specifically 0.04%. The upper limit of the C content can be more specifically 0.075%, more specifically 0.07%, and even more specifically 0.065%.
[0021] Mn: 1.6% to 2.2%
[0022] Mn can be a useful element for improving strength and hardenability through solid solution strengthening to form low-temperature transformation phases. To achieve the yield strength of 500 MPa obtained through this disclosure, Mn can be added in amounts of 1.6% or more. However, when the Mn content exceeds 2.2%, the excessive increase in hardenability promotes the formation of upper bainite and martensite, thereby significantly reducing impact toughness and resistance to brittle fracture initiation. Therefore, the Mn content can be specifically in the range of 1.6% to 2.2%. The lower limit of the Mn content can be specifically 1.65%, further specifically 1.7%, and even further specifically 1.8%. The upper limit of the Mn content can be specifically 2.15%, further specifically 2.1%, and even further specifically 2.05%.
[0023] Ni: 0.6% to 1.3%
[0024] Ni can be an important element for promoting dislocation cross-slip at relatively low temperatures to improve impact toughness and for improving hardenability to increase strength. To improve the impact toughness and resistance to brittle fracture initiation in high-strength steel with a yield strength of 500 MPa, Ni can be added in amounts of 0.6% or more. However, when the Ni content exceeds 1.3%, hardenability can be excessively increased, allowing the formation of low-temperature transformation phases, thereby reducing toughness and increasing manufacturing costs. Therefore, the Ni content can range from 0.6% to 1.3%. The lower limit of Ni content can be 0.65%, further 0.7%, and even further 0.75%. The upper limit of Ni content can be 1.25%, further 1.2%, and even further 1.15%.
[0025] Nb: 0.005% to 0.03%
[0026] Nitrogen (Nb) can precipitate in the form of NbC or NbCN to improve the strength of the base material. Furthermore, Nb dissolved during reheating to high temperatures can precipitate significantly finely as NbC during rolling, thus suppressing austenite recrystallization and refining the microstructure. To ensure this effect, Nb can be added in amounts of at least 0.005%. However, when the Nb content exceeds 0.03%, brittle cracks may appear at the edges of the steel, and a large amount of austenite (MA) may form in the base material, potentially reducing resistance to brittle fracture initiation. Therefore, the Nb content can be specifically in the range of 0.005% to 0.03%. The lower limit of the Nb content can be specifically 0.008%, further specifically 0.01%, and even further specifically 0.012%. The upper limit of the Nb content can be specifically 0.027%, further specifically 0.025%, and even further specifically 0.023%.
[0027] Ti: 0.005% to 0.02%
[0028] During reheating, Ti precipitates as TiN to suppress grain growth in the base material and the heat-affected zone, resulting in a significant improvement in low-temperature toughness. To achieve this effect, Ti can be added in amounts of 0.005% or more. However, when Ti is added in amounts exceeding 0.02%, the continuous casting nozzle may become clogged or the low-temperature toughness may decrease due to crystallization in the central portion. Therefore, the Ti content can be specifically in the range of 0.005% to 0.02%. The lower limit of the Ti content can be specifically 0.007%, further specifically 0.08%, and even further specifically 0.01%. The upper limit of the Ti content can be specifically 0.018%, further specifically 0.016%, and even further specifically 0.014%.
[0029] Cu: 0.1% to 0.4%
[0030] Cu can be an important element for improving hardenability and providing solid solution strengthening to increase the strength of steel, and it can also be a major element used to increase yield strength by forming υCu precipitates when tempering steel. Therefore, Cu can be added in amounts of 0.1% or more. However, when the Cu content exceeds 0.4%, slab cracking may occur due to hot brittleness during the steelmaking process. Therefore, the Cu content can be in the range of 0.1% to 0.4%. The lower limit of the Cu content can be 0.12%, further 0.15%, and even further 0.18%. The upper limit of the Cu content can be 0.38%, further 0.35%, and even further 0.32%.
[0031] P: 100 ppm or less
[0032] Phosphorus (P) is an element that causes brittleness at grain boundaries or the formation of coarse inclusions that lead to brittleness. To improve brittleness prevention, the P content can be controlled to less than 100 ppm or less. The P content can be more specifically 90 ppm or less, more specifically 80 ppm or less, and even more specifically 60 ppm or less.
[0033] S: 40 ppm or less
[0034] Similar to phosphorus (P), sulfur (S) is an element that causes brittleness at grain boundaries or the formation of coarse inclusions that lead to brittleness. To improve brittleness prevention, the S content can be controlled to 40 ppm or less. The S content can be more specifically 30 ppm or less, further more specifically 20 ppm or less, and even more specifically 10 ppm or less.
[0035] H: 1.5 ppm or less
[0036] When hydrogen is present in large quantities, it may accumulate in inclusions after cooling and may cause hydrogen-induced cracking (HIC), leading to microcracks. To improve resistance to brittle fracture initiation, the H content can be controlled to 1.5 ppm or less. The H content can be more specifically 1.3 ppm or less, more specifically 1.1 ppm or less, and even more specifically 0.9 ppm or less.
[0037] The balance in this disclosure can be iron (Fe). However, in general manufacturing processes, unavoidable impurities may be inevitably added from raw materials or the surrounding environment, and therefore it is impossible to eliminate these impurities. Those skilled in the art of general manufacturing processes can understand these impurities; therefore, a description of the impurities is not required in this disclosure.
[0038] The ultra-thick steel according to this disclosure can have a microstructure in which the sum of the area fractions of acicular ferrite and granular ferrite can be specifically 80% or greater. As described above, in this disclosure, high strength can be ensured by using a mixed microstructure comprising acicular ferrite and granular bainite as the main microstructure, and high strength can be obtained by first nucleating the acicular ferrite to prevent the bainite phase grains from becoming coarse. When the sum of acicular ferrite and granular bainite is less than 80% area, it may not be sufficient to achieve the above effects. Therefore, the sum of acicular ferrite and granular bainite can be 80% area or greater, specifically 85% area or greater, further specifically 90% area or greater, and even more specifically 95% area or greater. The remaining microstructure of the ultra-thick steel according to this disclosure can be one or more of upper bainite, martensitic-austenitic (MA) composition, and degraded pearlite. In this disclosure, the smaller the remaining microstructure, the more preferred. Degraded pearlite refers to pearlite tissue with small dimensions due to fragmented layered structure.
[0039] In the ultra-thick steel according to this disclosure, in the region ±1 mm from the center of thickness, every 1 mm 2 The total length of cracks with a size of 30 μm or larger per unit area can be 130 μm or less. As described above, defects occurring in the central portion of the steel can be suppressed to improve the resistance of the base material to brittle fracture initiation. The total length of the cracks can be more specifically 110 μm or less, more specifically 100 μm or less, and even more specifically 90 μm or less.
[0040] The ultra-thick steel provided by this disclosure can have a yield strength of 500 MPa or higher. Furthermore, at a temperature of -10°C, the average crack tip opening displacement (CTOD) value of the base material can be 0.4 mm or greater, and the impact transition temperature of the central portion can be -40°C or lower. By ensuring the excellent yield strength and resistance to brittle fracture initiation as described above, the ultra-thick steel of this disclosure can be specifically used as structural steel.
[0041] In the following, a method for manufacturing an ultra-thick structural steel with excellent resistance to brittle fracture initiation according to an exemplary embodiment of the present disclosure will be described.
[0042] Molten steel with the above alloy composition can be prepared. When preparing molten steel, the hydrogen (H) content can be controlled to 1.5 ppm or less by RH refining the molten steel for 15 minutes or longer. When the RH refining time is less than 15 minutes, it may be difficult to sufficiently reduce hydrogen, making it difficult to improve resistance to brittle fracture initiation. On the other hand, when the RH refining time is more than 40 minutes, it may be disadvantageous in terms of economy and cost compared to the H reduction effect. Therefore, the RH refining time can be specified from 15 minutes to 40 minutes. The lower limit of the RH refining time can be specified as 18 minutes, further specified as 20 minutes, and even further specified as 25 minutes. The upper limit of the RH refining time can be specified as 38 minutes, further specified as 36 minutes, and even further specified as 34 minutes.
[0043] The molten steel can then be continuously cast to obtain steel billets. All methods conventionally used in this art can be applied to continuous casting.
[0044] The steel billet can be reheated to a temperature of 1000°C to 1150°C. The reheating temperature can be specifically 1000°C or higher to dissolve the carbonitrides of titanium (Ti) and / or niobium (Nb) formed during casting. Since austenite may coarsen if the reheating temperature is too high, the reheating temperature can be specifically 1150°C or lower. Therefore, the reheating temperature can be specifically from 1000°C to 1150°C. The lower limit of the reheating temperature can be specifically 1010°C, further specifically 1030°C, and even further specifically 1050°C. The upper limit of the reheating temperature can be 1120°C, further specifically 1100°C, and even further specifically 1080°C.
[0045] The reheated steel billet can be rough rolled at a temperature of 900°C to 1150°C. Rough rolling can be performed to adjust the shape of the billet. Furthermore, rough rolling can achieve the effect of not only destroying the casting structure such as dendrites formed during rough rolling during casting, but also reducing the grain size through the recrystallization of coarse austenite. For this purpose, the rough rolling temperature can be higher than or equal to the austenite recrystallization cessation temperature Tnr, for example, it can be higher than or equal to 900°C. On the other hand, when the rough rolling temperature is 1150°C or higher, the austenite may coarsen. Therefore, the rough rolling temperature can be specifically between 900°C and 1150°C. The lower limit of the rough rolling temperature can be specifically 920°C, further specifically 930°C, and even further specifically 940°C. The upper limit of the rough rolling temperature can be specifically 1100°C, further specifically 1080°C, and even further specifically 1060°C.
[0046] To refine the microstructure through sufficient recrystallization, the total cumulative reduction during rough rolling can be controlled to 30% or more. The total cumulative reduction during rough rolling can be more specifically 40% or more, more specifically 45% or more, and even more specifically 50% or more.
[0047] Hot-rolled steel can be obtained by finish rolling a rough-rolled billet at a temperature of at least Ar3 (ferrite formation temperature) based on 1 / 4t (where "t" is the thickness of the steel). Finish rolling can be performed to transform the austenitic structure of the rough-rolled billet into a deformed austenitic structure and introduce a potential therein. When the finish rolling temperature is below Ar3, a large amount of air-cooled ferrite may form throughout the microstructure in the thickness direction, making it difficult to ensure a yield strength of 500 MPa or higher. Therefore, the finish rolling temperature can be Ar3 or higher. The finish rolling temperature can be more specifically Ar3 + 20°C or higher, more specifically Ar3 + 40°C or higher, and even more specifically Ar3 + 60°C or higher.
[0048] To improve resistance to brittle fracture initiation through refinement of the central microstructure, the total cumulative reduction during finishing rolling can be controlled to 40% or greater. The total cumulative reduction during finishing rolling can be more specifically 45% or greater, further more specifically 50% or greater, and even more specifically 53% or greater.
[0049] Hot-rolled steel can be cooled to temperatures between 300°C and 600°C at a cooling rate of 3°C / second or higher. When the cooling rate during cooling is less than 3°C / second or the cooling end temperature is higher than 600°C, the yield strength can be 500 MPa or lower as the microstructure softens. When the cooling end temperature is below 300°C, hydrogen may have difficulty escaping to the outside after cooling, resulting in a high probability of microcracks forming at the center. More specifically, austenitic structures with high hydrogen solid solution can be transformed by cooling into microstructures with low hydrogen solid solution, such as acicular ferrite and granular bainite. In this case, hydrogen can escape to the outer surface of the steel. However, when the cooling end temperature is below 300°C, hydrogen does not have sufficient time to escape to the outer surface of the steel, leaving hydrogen residue in the steel. Since the residual hydrogen acts as a crack initiation point, the cooling end temperature can be specifically 300°C or higher. The cooling rate can be specified as 3.1°C / sec or higher, more specifically 3.5°C / sec or higher, and even more specifically 3.7°C / sec or higher. The lower limit of the cooling termination temperature can be specified as 320°C, more specifically 340°C, and even more specifically 360°C. The upper limit of the cooling termination temperature can be specified as 560°C, more specifically 530°C, and even more specifically 500°C.
[0050] Invention Embodiments
[0051] The present disclosure will be described in more detail below by way of examples. However, it should be noted that the following examples are for illustrative purposes only and are not intended to limit the scope of the present disclosure. The scope of the present disclosure can be determined by the matters described in the claims and matters that can be reasonably inferred therefrom.
[0052] (Implementation Plan)
[0053] The molten steel was refined for the RH refining times specified in Table 1 to prepare steel with the alloy composition listed in Table 1. The prepared molten steel was continuously cast to produce billets with a thickness of 400 mm. The billets were reheated to a temperature of 1080°C and then rough-rolled at a temperature of 1030°C to prepare bars with a thickness of 200 mm. The cumulative reduction applied during rough rolling was 50%. After rough rolling, the bars were finish-rolled at a temperature range of 700°C to 850°C to obtain hot-rolled steel with the thicknesses listed in Table 2, and then cooled under the conditions listed in Table 2.
[0054] The microstructure, yield strength, and impact transition temperature of the central portion of the steel manufactured in the above manner were measured, and the results are listed in Table 2. Furthermore, a total thickness CTOD test was performed on the steel at -10°C, and the results are listed in Table 2. Optical imaging was performed 20 times along the length of the steel in a region ±1 mm from the center of the steel thickness, and the results were calculated for each 1 mm... 2The total length of cracks with a length of 30 μm or greater was calculated, and the results are listed in Table 2.
[0055] [Table 1]
[0056]
[0057] [Table 2]
[0058]
[0059] In the case of Invention Examples 1 to 5 that satisfy the alloy composition and manufacturing conditions proposed in this disclosure, it can be determined that the microstructure in the central portion of the steel is ensured to be a mixed phase of 80% or more of acicular ferrite and granular bainite, and that every 1 mm in a region ±1 mm from the thickness center of the steel... 2 The total length of cracks with a size of 30 μm or larger per unit area is 130 μm or less. Therefore, it can be determined that a yield strength of 500 MPa or higher, an average CTOD value of the base material with a diameter of 0.4 mm or larger, and an impact transition temperature of -40°C or lower at the center are guaranteed.
[0060] Comparative Example 1 satisfies the alloy composition proposed in this disclosure, but its yield strength is 500 MPa or lower because the cooling end temperature exceeds the range of this disclosure.
[0061] Comparative Example 2 satisfies the alloy composition proposed in this disclosure, but its cooling end temperature is lower than the range of this disclosure, resulting in insufficient escape of hydrogen (H) to the outside. Therefore, the crack length in the central portion is greater than 130 μm, and consequently, the impact transition temperature of the central portion is higher than -40°C, and the value of Comparative Example 2 in the -10°C CTOD test, which represents the resistance to brittle fracture initiation, is less than 0.4 mm.
[0062] Comparative Example 3 has a carbon (C) value greater than the range presented in this disclosure. Therefore, due to excessive hardenability, a large amount of upper bainite structure is formed, resulting in an impact transformation temperature in the central portion that is higher than -40°C.
[0063] Comparative Example 4 has a manganese (Mn) value greater than the range proposed in this disclosure. Therefore, due to excessive hardenability, a large amount of upper bainite is formed, resulting in an impact transformation temperature in the central portion exceeding -40°C. Furthermore, numerous microcracks appear in the central segregation zone, causing the comparative example to have a CTOD value of less than 0.4 mm at -10°C.
[0064] Comparative Example 5 has carbon (C) and manganese (Mn) values that are smaller than the ranges proposed in this disclosure, resulting in the formation of a large amount of polygonal ferrite and pearlite structure due to insufficient hardenability. Therefore, the yield strength of the comparative example is 500 MPa or lower.
[0065] Comparative Example 6 has values for nickel (Ni) and copper (Cu) that are greater than those proposed in this disclosure, resulting in the formation of a large amount of upper bainite due to excessive hardenability. Therefore, the impact transformation temperature of the central portion is higher than -40°C. Furthermore, a large number of microcracks appear in the central segregation zone, resulting in a CTOD value of less than 0.4 mm for Comparative Example 6 at -10°C.
[0066] Comparative Example 7 has values greater than those of titanium (Ti) and niobium (Nb) presented in this disclosure, resulting in the formation of a large amount of upper bainite due to excessive precipitate formation and increased hardenability. Therefore, the impact transformation temperature of the central portion is higher than -40°C.
[0067] Comparative Examples 8 and 9 have hydrogen (H) values exceeding the range proposed in this disclosure, resulting in a large number of microcracks in the central portion. Therefore, the values of the comparative examples in the -10°C CTOD test are less than 0.4 mm. In particular, in the case of Comparative Example 9, the impact transition temperature of the central portion is higher than -40°C.
Claims
1. Controlling the hydrogen content to 1.5 ppm or less is used to improve the yield strength and resistance to brittle fracture initiation of ultra-thick structural steel. The ultra-thick structural steel comprises, by weight percent, C: 0.03% to 0.08%, Mn: 1.6% to 2.2%, Ni: 0.6% to 1.3%, Nb: 0.005% to 0.03%, Ti: 0.005% to 0.02%, Cu: 0.1% to 0.4%, P: 100 ppm or less, S: 40 ppm or less, and the balance being Fe and unavoidable impurities. The sum of acicular ferrite and granular bainite in the microstructure of the base material of the steel, by area fraction, is 80% or greater. Every 1 mm in the region ±1 mm from the center of the thickness of the steel 2 The total length of cracks with a size of 30 μm or larger per unit area is 130 μm or smaller, and Yield strength is 500 MPa or higher.
2. The use according to claim 1, wherein the remaining microstructure is one or more of upper bainite, martensite-austenite (MA) component and degraded pearlite.
3. The use according to claim 1, wherein the average crack tip opening displacement (CTOD) of the base material of the steel at a temperature of -10°C is 0.4 mm or greater, and the impact transition temperature of the central portion of the steel is -40°C or lower.
4. A method for providing excellent resistance to brittle fracture initiation of ultra-thick structural steel by effectively reducing defects in the central portion of the steel. The ultra-thick structural steel comprising, by weight, 0.03% to 0.08% C, 1.6% to 2.2% Mn, 0.6% to 1.3% Ni, 0.005% to 0.03% Nb, 0.005% to 0.02% Ti, 0.1% to 0.4% Cu, 100 ppm or less P, 40 ppm or less S, and the balance Fe and unavoidable impurities. The sum of acicular ferrite and granular bainite in the microstructure of the base material of the steel, by area fraction, is 80% or greater. Every 1 mm in the region ±1 mm from the center of the thickness of the steel 2 The total length of cracks with a size of 30 μm or larger per unit area is 130 μm or smaller, and Yield strength is 500 MPa or higher.
5. The method according to claim 4, wherein the remaining microstructure is one or more of upper bainite, martensite-austenite (MA) component and degraded pearlite.
6. The method of claim 4, wherein the average crack tip opening displacement (CTOD) of the base material of the steel at a temperature of -10°C is 0.4 mm or greater, and the impact transition temperature of the central portion of the steel is -40°C or lower.
7. An ultra-thick structural steel with excellent resistance to brittle fracture initiation, said ultra-thick structural steel comprising, by weight %: C: 0.03% to 0.08%, Mn: 1.6% to 2.2%, Ni: 0.6% to 1.3%, Nb: 0.005% to 0.03%, Ti: 0.005% to 0.02%, Cu: 0.1% to 0.4%, P: 100 ppm or less, S: 40 ppm or less, H: 1.5 ppm or less, and the balance being Fe and unavoidable impurities. The sum of acicular ferrite and granular bainite in the microstructure of the base material of the steel, by area fraction, is 80% or greater. Every 1 mm in the region ±1 mm from the center of the thickness of the steel 2 The total length of cracks with a size of 30 μm or larger per unit area is 130 μm or smaller, and Yield strength is 500 MPa or higher.
8. The ultra-thick structural steel with excellent resistance to brittle fracture initiation according to claim 7, wherein the remaining microstructure is one or more of upper bainite, martensite-austenite (MA) composition and degraded pearlite, and / or wherein the base material of the steel has an average crack tip opening displacement (CTOD) of 0.4 mm or greater at a temperature of -10°C, and the impact transformation temperature of the central portion of the steel is -40°C or lower.
9. A method for manufacturing ultra-thick structural steel with excellent resistance to brittle fracture initiation, the method comprising: The steel is prepared by means of the following components by weight: C: 0.03% to 0.08%, Mn: 1.6% to 2.2%, Ni: 0.6% to 1.3%, Nb: 0.005% to 0.03%, Ti: 0.005% to 0.02%, Cu: 0.1% to 0.4%, P: 100 ppm or less, S: 40 ppm or less, H: 1.5 ppm or less, and the balance being Fe and unavoidable impurities. The molten steel is continuously cast to obtain a steel billet; The steel billet is then reheated to a temperature of 1000°C to 1150°C. The reheated steel billet is rough rolled at a temperature of 900℃ to 1150℃; Based on 1 / 4t, a rough-rolled steel billet is finished rolled at Ar3 or higher temperatures to obtain hot-rolled steel, where "t" is the thickness of the steel; and The hot-rolled steel is cooled to a temperature of 300°C to 600°C at a cooling rate of 3°C / second or higher. The preparation of the molten steel includes RH refining the molten steel for 15 to 40 minutes.
10. The method of manufacturing ultra-thick structural steel with excellent resistance to brittle fracture initiation according to claim 9, wherein the total cumulative reduction during rough rolling is 30% or more, and / or wherein the total cumulative reduction during finish rolling is 40% or more.