A 1500MPa grade high-strength and high-ductility wire rod and its production method
By using a low-carbon C-Si-Mn-Cr-Mo composite alloy system and a full-process temperature control technology, combined with online salt bath treatment, the problem of matching strength and plasticity of high-strength wire rod was solved, enabling stable mass production of 1500MPa-grade high-strength and high-ductility hot-rolled wire rod and improving the performance of downstream products.
Patent Information
- Application Number
- CN202611073726.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-20
- Publication Date
- 2026-11-17
AI Technical Summary
Existing high-strength wire rods cannot simultaneously achieve tensile strength ≥1500MPa and reduction of area ≥60%. High carbon segregation leads to embrittlement, and there is a lack of suitable continuous hot rolling and online salt bath complete processes, resulting in poor mass production stability.
A low-carbon C-Si-Mn-Cr-Mo composite alloy system is adopted, and a whole-process synergistic temperature control process is used to control the multiphase structure of bainite and tempered martensite. Combined with online salt bath treatment, high-strength and high-ductility hot-rolled wire rods are prepared.
Stable mass production of 1500MPa-grade high-strength and high-ductility wire rods has been achieved, reducing the risk of breakage during downstream processing and improving the uniformity of the material's mechanical properties and the continuity of production.
Smart Images

Figure CN123108434A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of hot-rolled wire rod manufacturing technology, and in particular to a 1500MPa grade high-strength and high-ductility hot-rolled wire rod and its preparation method, which is applicable to the production of raw materials for bridge cables, prestressed steel strands for buildings, and precision steel wires for high-end machinery. Background Technology
[0002] Wire rod is the core base material for high-strength steel wire and prestressed steel strand. The industry requires the base material to possess both ultra-high tensile strength and excellent plasticity to prevent wire breakage and scrap during downstream cold drawing and twisting processes. Currently, the mainstream high-strength wire rod technology falls into two main categories: 1) High-carbon sorbitic wire rod (patent CN118814082B): Utilizing a high-carbon C-Si-Mn-Cr-V-Ti composition system with C≥0.65%, it relies on a large amount of sorbite to enhance strength. The drawback is that the high carbon content easily leads to carbon segregation in the center of the continuously cast billet, and the precipitation of network cementite during controlled cooling significantly reduces the material's plasticity. Existing technology achieves a maximum tensile strength of 1430 MPa, with a reduction of area of only 37%~40%, failing to consistently reach the 1500 MPa level. It also suffers from a high wire breakage rate during cold drawing, making it difficult to produce high-elongation steel wire of the 1860 MPa grade. Although patent CN118814082B discloses high-carbon steel for 2300 MPa grade steel strand, the entire cooling process is controlled to pursue a fully sorbitic structure, abandoning bainite control, resulting in a significant shortcoming in plasticity.
[0003] 2) Medium carbon bainitic wire rod (patent CN120575017B): It adopts a medium-high carbon C-Si-Mn-Cr-V system, and obtains a mixed structure of sorbite and tempered martensite by salt bath tempering. The maximum tensile strength is 1420MPa and the reduction of area is only 40%. This system does not add Mo, and high-temperature ferrite is easily generated during the cooling process, which seriously deteriorates the plasticity. In addition, the proportion of bainite is not quantitatively controlled, resulting in poor strength and plasticity matching.
[0004] In summary, existing technologies suffer from three major drawbacks: ① It is difficult to simultaneously achieve a tensile strength ≥1500MPa and a reduction of area ≥60% for wire rods; ② High carbon segregation and cementite embrittlement lead to "high strength and low ductility"; ③ There is a lack of suitable continuous hot rolling and online salt bath processes, resulting in poor mass production stability. This invention addresses these shortcomings by developing a low-carbon C-Si-Mn-Cr-Mo composite alloy system and a full-process synergistic temperature control technology to achieve stable mass production of 1500MPa-grade high-strength, high-ductility wire rods. Summary of the Invention
[0005] The purpose of this invention is to provide a 1500MPa grade high-strength and high-ductility hot-rolled wire rod and its preparation method, which overcomes the defect that the strength and plasticity of existing high-strength wire rods cannot be balanced. It adopts a low-carbon design to eliminate carbon segregation in the center of the billet, suppress the precipitation of network cementite, solve the problem of steel brittleness, and provide a continuous preparation process that is compatible with existing hot rolling and online salt bath production lines to achieve low-cost large-scale production.
[0006] To achieve the above objectives, the present invention provides the following technical solution: A 1500MPa grade high-strength and high-ductility hot-rolled wire rod, characterized in that the components of the wire rod, by mass percentage, are: C 0.30~0.40%, Si 1.30~1.60%, Mn 1.55~1.80%, Cr 0.45~0.75%, Mo 0.10~0.35%, S≤0.01%, P≤0.02%, with the balance being Fe and unavoidable impurities.
[0007] The role of each alloying element and the reasons for limiting its content: 1) Carbon (C, 0.30~0.40%): This invention adopts a low-carbon design, which differs from traditional high-carbon wire rods. Carbon can stabilize untransformed austenite, ensuring the strength of the bainite-tempered martensite multiphase structure; C < 0.30%, solid solution strengthening is insufficient, and the tensile strength cannot exceed 1500MPa; C > 0.40%, carbide precipitation increases, plasticity decreases, and segregation in the continuous casting center is aggravated.
[0008] 2) Silicon (Si, 1.30~1.60%): Si is a non-carbide forming element that can inhibit the precipitation of brittle cementite during the bainitic phase transformation process and improve the plasticity of steel. If Si < 1.30%, the cementite inhibition effect is insufficient. If Si > 1.60%, the iron oxide scale on the surface of the steel will be thickened, increasing the cost of dephosphorization, cold drawing and pickling.
[0009] 3) Manganese (Mn, 1.55~1.80%): Mn delays the high-temperature ferrite phase transformation, improves the stability of austenite, and retains an appropriate amount of metastable austenite to improve plasticity; Mn < 1.55%, proeutectoid ferrite is easily precipitated; Mn > 1.80%, the austenite stability is too high, the bainite transformation is incomplete in the salt bath isothermal stage, the proportion of martensite is too high, and the plasticity drops sharply.
[0010] 4) Chromium (Cr, 0.45~0.75%): Cr lowers the austenite phase transformation temperature, inhibits the formation of high-temperature ferrite, and refines bainite laths; Cr < 0.45%, the phase transformation inhibition effect is insufficient; Cr > 0.75%, the alloy cost increases, while the hardenability of steel is improved, and there is too much residual martensite after salt bath.
[0011] 5) Molybdenum (Mo, 0.10~0.35%): Mo works synergistically with Cr to significantly widen the bainitic transformation window and completely avoid ferrite precipitation during the cooling process; when Mo is missing, a large amount of ferrite is generated in the microstructure, and the reduction of area drops to below 45% (verified by Comparative Example 1); when Mo < 0.10%, the synergistic inhibition effect is insufficient; when Mo > 0.35%, the cost of precious metals increases significantly, and the economic efficiency deteriorates.
[0012] 6) Sulfur and phosphorus (S≤0.01%, P≤0.02%): S and P are harmful impurities that easily form plastic inclusions and grain boundary segregation, which greatly reduce the reduction of area. Therefore, the upper limit is strictly limited.
[0013] Preferably, the microstructure of the wire rod comprises bainite and tempered martensite, wherein the volume fraction of bainite is 80-90 vol.%.
[0014] Preferably, the mechanical properties of the wire rod meet the following requirements: tensile strength ≥ 1500 MPa, and reduction of area ≥ 60%.
[0015] Preferably, the diameter of the wire rod is 6mm to 12mm.
[0016] This invention also provides a 1500MPa grade high-strength, high-ductility hot-rolled wire rod and its preparation method, comprising the following steps: S1. Batching, smelting and continuous casting: Batching materials are prepared according to the alloy composition, and after smelting and refining, they are continuously cast to obtain qualified continuous casting billets. S2. Segmented hot rolling forming: After heating the continuously cast billet and descaling it with high-pressure water, it is rolled in two segments, rough rolling and finish rolling, to obtain rolled wire; wherein the billet heating temperature is 1130~1180℃, the rough rolling start temperature is 1030~1080℃, and the finish rolling finish temperature is ≥900℃. S3, Wire forming: The rolled wire is fed into the wire forming machine and spun at 800~830℃ to obtain the initial wire rod; S4. Salt bath isothermal treatment and tempering: The initial wire rod is subjected to online or offline salt bath isothermal treatment at a salt bath temperature of 360~390℃ for 5~10 minutes. After the salt bath is completed, tempering is performed at a tempering temperature of 300~400℃. After cooling, the finished hot-rolled wire rod is obtained.
[0017] The present invention also provides a cold-drawn steel wire for 1770MPa grade prestressed steel strand, wherein the steel wire is made from the wire rod described in any one of claims 1 to 4 by pickling and multiple cold drawing processes; the tensile strength of the steel wire is ≥1770MPa and the elongation after fracture is ≥12%.
[0018] The present invention also provides a cold-drawn steel wire for 1860MPa grade prestressed steel strand, wherein the steel wire is made from the wire rod described in any one of claims 1 to 4 by pickling and multiple cold drawing processes; the tensile strength of the steel wire is ≥1860MPa and the elongation after fracture is ≥10%.
[0019] Compared with the prior art, the beneficial effects of the present invention are: 1) Breakthrough in matching strength and plasticity: The wire rod strength is ≥1500MPa and the section reduction rate is ≥60%, which greatly improves the strength and plasticity of the wire rod and significantly reduces the risk of breakage in downstream processing; 2) Low carbon and low segregation: C≤0.40%, completely solving the problems of carbon segregation in the center of high carbon wire rod and embrittlement of network cementite, resulting in uniform mechanical properties of wire rod throughout the rod; 3) Collaborative innovation of alloy system: Cr+Mo composite addition completely suppresses high-temperature ferrite, precisely controls the 80~90 vol.% bainite multiphase structure, and supports plasticity through high proportion of tough bainite, while tempered martensite ensures tensile strength; 4) Process adaptation for mass production: The parameters of the entire rolling-coating-salt bath-tempering system are matched with the existing online salt bath production line of the steel plant. No new special equipment is required, and continuous industrial production is possible. 5) Versatility of downstream products: One set of wire rod base material can produce two grades of prestressed steel wire with strengths of 1770MPa and 1860MPa. Its elongation performance is better than that of traditional high-carbon sorbitic base material, and it is suitable for long-span bridges, high-speed sleepers and large hydraulic prestressed components. Attached Figure Description
[0020] Figure 1 Example 1: Microstructure of wire rod (6mm, bainite + tempered martensite). Figure 2 Example 2: Microstructure of wire rod (8.5 mm, uniform bainitic matrix); Figure 3 Example 3: Room temperature tensile stress-strain curve of wire rod; Figure 4 Comparative Example 1 microstructure (no Mo, large amount of ferrite precipitation); Figure 5 Comparative Example 2: Microstructure (salt bath overheating, coarsening of bainite, excessive martensite). Figure 6 Example 1: Tensile curve of 5.25mm cold-drawn steel wire; Figure 7 Example 2: Tensile curve of cold-drawn 5.04mm steel wire. Detailed Implementation
[0021] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, the specific embodiments of the present invention will be described in detail below through examples.
[0022] Many specific details are set forth in the following description in order to provide a full understanding of the invention. However, the invention may also be practiced in other ways different from those described herein, and those skilled in the art can make similar extensions without departing from the spirit of the invention. Therefore, the invention is not limited to the specific embodiments disclosed below.
[0023] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The phrase "in one embodiment" appearing in different places in this specification does not necessarily refer to the same embodiment, nor is it a single or selective embodiment that is mutually exclusive with other embodiments.
[0024] The rationality of the components and process parameters of this invention is verified through 4 sets of examples and 3 sets of comparative examples. The chemical components are shown in Table 1, and the process parameters and performance results are shown in Table 2.
[0025] Table 1. Chemical composition of steel in each embodiment and comparative example (wt.%) Example 1
[0026] A method for producing 1500MPa high-strength, high-ductility hot-rolled wire rod involves batching materials according to the alloy composition in Table 1, smelting and continuously casting to obtain a continuously cast billet; reheating and descaling the billet, followed by rolling, including roughing and finishing rolling stages, to obtain rolled wire; winding the rolled wire through a wire rod mill to obtain initial wire rod; and tempering the initial wire rod after online or offline salt bath treatment to obtain final wire rod. The heating temperature during rolling is 1150℃, the roughing start temperature is 1080℃, and the finishing finish temperature is 920℃. The salt bath temperature is 370℃, the salt bath time is 5 min, and the tempering temperature is 300℃. Example 2
[0027] A method for producing 1500MPa high-strength, high-ductility hot-rolled wire rod involves batching materials according to the alloy composition in Table 1, smelting and continuously casting to obtain a continuously cast billet; reheating and descaling the billet, followed by rolling, including roughing and finishing rolling stages, to obtain rolled wire; winding the rolled wire through a wire rod mill to obtain initial wire rod; and tempering the initial wire rod after online or offline salt bath treatment to obtain final wire rod. The heating temperature during rolling is 1130℃, the roughing start temperature is 1030℃, and the finishing finish temperature is 910℃. The salt bath temperature is 360℃, the salt bath time is 10 min, and the tempering temperature is 400℃. Example 3
[0028] A method for producing 1500MPa high-strength, high-ductility hot-rolled wire rod involves batching materials according to the alloy composition in Table 1, smelting and continuously casting to obtain a continuously cast billet; reheating and descaling the billet, followed by rolling, including roughing and finishing rolling stages, to obtain rolled wire; winding the rolled wire through a wire rod mill to obtain initial wire rod; and tempering the initial wire rod after online or offline salt bath treatment to obtain final wire rod. The heating temperature during rolling is 1180℃, the roughing start temperature is 1080℃, and the finishing finish temperature is 920℃. The salt bath temperature is 380℃, the salt bath time is 5 min, and the tempering temperature is 300℃. Example 4
[0029] A method for producing 1500MPa high-strength, high-ductility hot-rolled wire rod involves batching materials according to the alloy composition in Table 1, smelting and continuously casting to obtain a continuously cast billet; reheating and descaling the billet, followed by rolling, including roughing and finishing rolling stages, to obtain rolled wire; winding the rolled wire through a wire rod mill to obtain initial wire rod; and tempering the initial wire rod after online or offline salt bath treatment to obtain final wire rod. The heating temperature during rolling is 1150℃, the roughing start temperature is 1040℃, and the finishing finish temperature is 910℃. The salt bath temperature is 370℃, the salt bath time is 7 min, and the tempering temperature is 320℃.
[0030] Comparative Example 1: The composition and process are the same as in Example 1, except that Mo was not added.
[0031] Comparative Example 2: The composition and process are the same as in Example 2, except that the salt bath temperature is higher than the design range, at 420°C.
[0032] Comparative Example 3: The composition and process are the same as those in Example 3, except that the tempering temperature is higher than the design range, which is 450°C.
[0033] The microstructure and mechanical properties of each embodiment and comparative example were characterized, and the results are shown in Table 2.
[0034] Table 2. Microstructure and Mechanical Properties of Each Example and Comparative Example
[0035] Example 1: The wire rod diameter is 6 mm, and the microstructure is as follows. Figure 1 As shown, it includes bainite and tempered martensite, has a tensile strength of 1524 MPa, and a reduction of area of 65%.
[0036] Example 2: The wire rod diameter is 8.5 mm, and the microstructure is as follows. Figure 2As shown, it includes bainite and tempered martensite, with a tensile strength of 1574 MPa and a reduction of area of 62%.
[0037] Example 3: The wire rod diameter is 10.5 mm, and the stretching curve is as follows. Figure 3 As shown, the tensile strength is 1645 MPa and the reduction of area is 60%.
[0038] Example 4: The wire rod diameter is 11.5 mm, the tensile strength is 1537 MPa, and the reduction of area is 61%.
[0039] Comparative Example 1 has a wire rod diameter of 6 mm, and its composition does not meet the design requirements. The microstructure is as follows: Figure 4 As shown, due to the absence of Mo, high-temperature ferrite appears in the microstructure, which does not meet the microstructure design requirements of this invention. The tensile strength is 1588 MPa, and the reduction of area is 42%, which does not meet the performance requirements, proving that Mo is an essential alloying element.
[0040] Comparative Example 2: The wire rod diameter was 8.5 mm, and the salt bath temperature did not meet the requirements; the microstructure was as follows. Figure 5 As shown, the bainite structure has a wide size and low content, while the martensite volume fraction is high, resulting in a significant decrease in plasticity, which does not meet the microstructure design requirements of this invention. The tensile strength is 1709 MPa, and the reduction of area is 44%, which does not meet the performance requirements.
[0041] Comparative Example 3 has a wire rod diameter of 10.5 mm and a high tempering temperature. After tempering, the strength decreased significantly, with a tensile strength of 1399 MPa and a reduction of area of 61%. The tensile strength does not meet the performance requirements.
[0042] The wire rod obtained in Example 1 was pickled and cold-drawn into steel wire with a diameter of 5.25 mm. The tensile curve is shown below. Figure 6 As shown, the tensile strength is 1810 MPa and the elongation after fracture is 14%. The wire rod obtained in Example 2 was pickled and cold-drawn into steel wire with a diameter of 5.04 mm. The tensile curve is shown below. Figure 7 As shown, the tensile strength is 1862 MPa and the elongation after fracture is 14.5%.
[0043] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.
Claims
1. A 1500MPa grade high-strength, high-ductility hot-rolled wire rod, characterized in that, The components of the wire rod, by mass percentage, are: C 0.30~0.40%, Si 1.30~1.60%, Mn 1.55~1.80%, Cr 0.45~0.75%, Mo 0.10~0.35%, S≤0.01%, P≤0.02%, with the balance being Fe and unavoidable impurities.
2. The 1500MPa grade high-strength, high-ductility hot-rolled wire rod according to claim 1, characterized in that, The microstructure of the wire rod comprises bainite and tempered martensite, wherein the volume fraction of bainite is 80-90 vol.
3. The 1500MPa grade high-strength, high-ductility hot-rolled wire rod according to claim 1, characterized in that, The mechanical properties of the wire rod meet the following requirements: tensile strength ≥ 1500 MPa, and reduction of area ≥ 60%.
4. The 1500MPa grade high-strength, high-ductility hot-rolled wire rod according to claim 1, characterized in that, The diameter of the wire rod is 6mm to 12mm.
5. A method for producing 1500MPa grade high-strength, high-ductility hot-rolled wire rod according to any one of claims 1-4, characterized in that, The steps are as follows: S1. Batching, smelting and continuous casting: Batching materials are prepared according to the alloy composition, and after smelting and refining, they are continuously cast to obtain qualified continuous casting billets. S2. Segmented hot rolling forming: After heating the continuously cast billet and descaling it with high-pressure water, it is rolled in two segments, rough rolling and finish rolling, to obtain rolled wire; wherein the billet heating temperature is 1130~1180℃, the rough rolling start temperature is 1030~1080℃, and the finish rolling finish temperature is ≥900℃. S3, Wire forming: The rolled wire is fed into the wire forming machine and spun at 800~830℃ to obtain the initial wire rod; S4. Salt bath isothermal treatment and tempering: The initial wire rod is subjected to online or offline salt bath isothermal treatment at a salt bath temperature of 360~390℃ for 5~10 minutes. After the salt bath is completed, tempering is performed at a tempering temperature of 300~400℃. After cooling, the finished hot-rolled wire rod is obtained.
6. A cold-drawn steel wire for 1770MPa grade prestressed steel strand, characterized in that, The steel wire is made from any of the wire rods described in claims 1 to 4 through pickling and multiple cold drawing processes; the tensile strength of the steel wire is ≥1770MPa, and the elongation after fracture is ≥12%.
7. A cold-drawn steel wire for 1860MPa grade prestressed steel strand, characterized in that, The steel wire is made from any of the wire rods described in claims 1 to 4 through pickling and multiple cold drawing processes; the tensile strength of the steel wire is ≥1860MPa, and the elongation after fracture is ≥10%.
Citation Information
Patent Citations
A 2300MPa grade ultra-high strength steel strand steel and its production method and a 2300MPa grade ultra-high strength steel strand
CN118814082B
1400mpa grade high strength tool steel wire rod and method of manufacturing the same
CN120575017B