An austenitic stainless steel resistant to intergranular stress corrosion cracking by supercritical carbon dioxide, its preparation method and application

By optimizing the composition and heat treatment process, an austenitic stainless steel resistant to intergranular stress corrosion cracking of supercritical carbon dioxide was prepared, solving the problems of grain boundary oxidation and stress corrosion of existing materials in supercritical carbon dioxide environment, and achieving an improvement in high-temperature corrosion resistance.

CN123108436APending Publication Date: 2026-11-17SHANGHAI JIAOTONG UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611276442.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing austenitic stainless steels are prone to grain boundary oxidation and intergranular stress corrosion cracking in supercritical carbon dioxide environments, becoming a key bottleneck in Brayton cycle systems. Existing modified steels are difficult to effectively prevent the rapid propagation of stress corrosion cracks along grain boundaries during dynamic tensile processes.

Method used

By optimizing the composition design and adding an appropriate amount of aluminum to the alloy, a highly protective aluminum-rich oxide film is formed, which inhibits the diffusion of metal cations and generates the NiAl phase, thus hindering oxygen penetration. At the same time, by adjusting the heat treatment process, austenitic stainless steel resistant to intergranular stress corrosion cracking caused by supercritical carbon dioxide is prepared.

Benefits of technology

Under 600℃ and 20 MPa SC-CO2 conditions, the oxide film thickness on the material surface is less than 1 μm, the intergranular oxidation depth is less than 4 μm, and there are no obvious intergranular cracks when tensile fractured. It has excellent resistance to IGSCC and meets the material requirements of the Brayton cycle system.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108436A_ABST
    Figure CN123108436A_ABST
Patent Text Reader

Abstract

This invention discloses an austenitic stainless steel resistant to supercritical carbon dioxide intergranular stress corrosion cracking, its preparation method, and its applications. The austenitic stainless steel comprises nickel, chromium, aluminum, manganese, silicon, niobium, carbon, copper, titanium, and molybdenum, with the balance being iron. Specifically, by mass percentage, the composition is as follows: nickel 25.5-26.5%, chromium 18.5-19.5%, aluminum 2-3%, manganese 1.8-2.2%, silicon 0.5-0.7%, niobium 0.3-0.5%, carbon 0.05-0.08%, copper 0.8-1.2%, titanium 0.2-0.5%, molybdenum 1.5-2.2%, with the balance being Fe. This invention effectively suppresses preferential oxidation at grain boundaries; the fracture surface after tensile fracture exhibits transgranular fracture characteristics dominated by dimples, with no obvious intergranular cracks, demonstrating excellent resistance to intergranular stress corrosion cracking.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of high-temperature corrosion-resistant alloy materials, specifically relating to an austenitic stainless steel resistant to supercritical carbon dioxide intergranular stress corrosion cracking, its preparation method, and its application. Background Technology

[0002] Currently, candidate materials for Brayton cycle systems mainly include ferritic / martensitic (F / M) steel, austenitic stainless steel, and nickel-based alloys. Although F / M steel has good thermal conductivity and resistance to radiation swelling, it is prone to severe oxidation in supercritical carbon dioxide (SC-CO2) environments and is at risk of σ-phase embrittlement at high temperatures, leading to a significant decrease in toughness. While nickel-based alloys exhibit excellent high-temperature strength and corrosion resistance, the high cost of adding elements such as nickel and molybdenum greatly limits their economic feasibility in SC-CO2 Brayton cycle systems.

[0003] In contrast, austenitic stainless steel achieves a better balance between cost and performance through reasonable composition design. However, existing materials such as 20Cr25NiNb type austenitic stainless steel and 316LN austenitic stainless steel still face severe failure challenges in high-temperature SC-CO2 environments. Existing research shows that materials are highly susceptible to preferential intergranular oxidation (PIO) in this environment. This process not only leads to significant Cr depletion in the grain boundary regions of the material matrix, weakening the self-healing ability of the passivation film, but also acts as a core precursor to stress corrosion cracking, inducing crack initiation under dynamic tensile stress. At the same time, the rapid intrusion of the corrosive medium along the grain boundaries triggers the Kirkendall effect, leaving a large number of micropores at the grain boundaries, which may couple with carburizing and creep damage, jointly driving the material to undergo sudden intergranular brittle fracture. Therefore, intergranular stress corrosion cracking (IGSCC) has become the most important failure mode of austenitic stainless steel in SC-CO2 environment, and a key bottleneck restricting the engineering application of SC-CO2 Brayton cycle systems.

[0004] To further enhance the high-temperature corrosion resistance of materials, some related patents in recent years, such as CN114318169A and CN118345314A, have proposed the development of aluminum-containing austenitic stainless steel. The core role of adding aluminum is to generate a more protective aluminum-rich oxide film, inhibiting the outward diffusion of metal cations and hindering the inward penetration of oxygen, thus preventing oxidation failure. At the same time, aluminum-containing precipitates such as B2-NiAl can stabilize the matrix and hinder plastic deformation, thereby improving the alloy's creep resistance. However, existing AFA steel patent technologies and composition ratios mostly focus on static oxidation resistance or high-temperature lead-bismuth environments. Due to the stress concentration at the crack tip during dynamic tension, which causes the local protective film to continuously rupture, and the limited diffusion rate of Al, conventional AFA steel cannot achieve efficient passivation of the crack tip during deformation, thus failing to effectively block the rapid propagation of stress corrosion cracks along grain boundaries.

[0005] In view of this, and in response to the problem that traditional austenitic stainless steel and existing modified steel are prone to grain boundary oxidation and intergranular stress corrosion cracking in a 600℃, 20 MPa SC-CO2 environment, this invention provides an austenitic stainless steel resistant to supercritical carbon dioxide intergranular stress corrosion cracking and its preparation method. Summary of the Invention

[0006] The purpose of this section is to outline some aspects of embodiments of the present invention and to briefly describe some preferred embodiments. Simplifications or omissions may be made in this section, as well as in the abstract and title of this application, to avoid obscuring the purpose of these documents; however, such simplifications or omissions should not be construed as limiting the scope of the invention.

[0007] In view of the problems existing in the above and / or prior art, the present invention is proposed.

[0008] Therefore, the purpose of this invention is to overcome the shortcomings of the prior art and provide an austenitic stainless steel resistant to intergranular stress corrosion cracking of supercritical carbon dioxide, its preparation method, and its application.

[0009] The composition, by mass percentage of raw materials, includes 25.5-26.5% nickel, 18.5-19.5% chromium, 2-3% aluminum, 1.8-2.2% manganese, 0.5-0.7% silicon, 0.3-0.5% niobium, 0.05-0.08% carbon, 0.8-1.2% copper, 0.2-0.5% titanium, 1.5-2.2% molybdenum, with the balance being Fe.

[0010] As a preferred embodiment of the austenitic stainless steel resistant to supercritical carbon dioxide intergranular stress corrosion cracking described in this invention, the following is a preferred embodiment based on the mass percentage of raw materials: nickel 26%, chromium 19%, aluminum 2.5%, manganese 2.0%, silicon 0.6%, niobium 0.4%, carbon 0.07%, copper 1.0%, titanium 0.4%, molybdenum 2.0%, with the balance being Fe.

[0011] As a preferred embodiment of the austenitic stainless steel resistant to intergranular stress corrosion cracking by supercritical carbon dioxide as described in this invention, wherein: in a 600℃, 20 MPa SC-CO2 environment, with 10 -7 s -1 Constant strain rate tension has the following characteristics: (i) When stretched to a strain of 14%, the average oxide film thickness on the surface is less than 1 μm.

[0012] (ii) When stretched to a strain of 10%, the average intergranular oxidation depth of the cross section is less than 4 μm.

[0013] (iii) When stretched to fracture, the fracture surface morphology shows transgranular fracture characteristics dominated by dimples, with no obvious intergranular cracks.

[0014] Another objective of this invention is to overcome the shortcomings of the prior art and provide a method for preparing austenitic stainless steel resistant to intergranular stress corrosion cracking caused by supercritical carbon dioxide.

[0015] As a preferred embodiment of the preparation method described in this invention, the pure metal raw materials Fe, Cr, Ni, Mo, Nb and Cu are mixed and then vacuum-smelted by electric current. C is added while maintaining the vacuum, and vacuum carbon-oxygen degassing and refining are completed by heat preservation and stirring. Subsequently, metal Al is added, and the mixture is fully melted, stirred and pre-deoxidized for refining. After refining, argon gas is introduced, and metallic Mn and metallic Si are added in sequence. After they are completely melted and stirred evenly, metallic Ti is added last, and stirring is continued until all alloying elements are fully and evenly dissolved. The smelted steel ingot is forged into shape, and after forging, it is air-cooled to obtain a stainless steel forging billet, and the oxide scale on the surface of the forging billet is removed. Austenitic stainless steel resistant to intergranular stress corrosion cracking caused by supercritical carbon dioxide is obtained by heat treatment of stainless steel forging billets after removing oxide scale.

[0016] As a preferred embodiment of the preparation method described in this invention, the steel ingot is placed in a heating furnace during the forging process and heated to 1200°C at a heating rate of 150°C / h, and held at that temperature for 1-2 h; then cooled to 1100-1180°C and held at that temperature for 1 h; the initial forging temperature is controlled at 1100-1180°C, and the final forging temperature is controlled at 950-1050°C; after forging, the steel ingot is air-cooled.

[0017] As a preferred embodiment of the preparation method described in this invention, the vacuum power supply melting conditions are: melting temperature 1420~1520℃, power supply power 5~40 kW.

[0018] As a preferred embodiment of the preparation method described in this invention, the refining conditions are a vacuum degree of less than 1×10⁻⁶. - 2 Pa, keep warm at 1480~1520℃ for no less than 10 min.

[0019] As a preferred embodiment of the preparation method described in this invention, the heat treatment conditions are as follows: the stainless steel forging billet is solution treated at 1100~1200℃ for 60~120 min and then water-cooled, followed by aging treatment at 800~850℃ for 10 h, and then air-cooled after being taken out of the furnace.

[0020] Another objective of this invention is to overcome the shortcomings of the prior art and provide an application of austenitic stainless steel resistant to intergranular stress corrosion cracking of supercritical carbon dioxide in heat exchanger components of SC-CO2 Brayton cycle power systems.

[0021] Beneficial effects of this invention: (1) This invention addresses the corrosion-resistant service material requirements of SC-CO2 Brayton cycle heat exchange systems by rationally designing the composition, adjusting the content and ratio of each element in the alloy, and supplementing with heat treatment and other processes to obtain IGSCC-resistant austenitic stainless steel.

[0022] (2) This invention possesses excellent resistance to IGSCC: under conditions of 600℃, 20 MPa SC-CO2 environment, and 10 -7 s -1 Under constant strain rate conditions, when the specimen is stretched to 14% strain, the average oxide film thickness on the surface is less than 1 μm; when stretched to 10% strain, the intergranular oxide depth is less than 4 μm. Simultaneously, no intergranular cracks are generated in the tensile fracture section of the specimen, fully meeting the requirements for the material's resistance to IGSCC under 600℃ and 20 MPa SC-CO2 conditions. Attached Figure Description

[0023] To more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings used in the following description of the embodiments will be briefly introduced. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort. Wherein: Figure 1 The IGSCC-resistant austenitic stainless steels of Examples 1-4, the 20Cr25NiNb type austenitic stainless steels of Comparative Examples 1-3, the 316LN stainless steels of Comparative Examples 4-5, and the aluminum-containing austenitic stainless steels of Comparative Examples 6-10 were subjected to an IGSCC-resistant austenitic stainless steel at 600°C and 20 MPa SC-CO2 environment, with a concentration of 10... -7 s -1 Comparison of average oxide film thicknesses obtained after stretching to different strain rates.

[0024] Figure 2 The IGSCC-resistant austenitic stainless steels of Examples 1-4, the 20Cr25NiNb type austenitic stainless steels of Comparative Examples 1-3, the 316LN stainless steels of Comparative Examples 4-5, and the aluminum-containing austenitic stainless steels of Comparative Examples 6-10 were subjected to an IGSCC-resistant austenitic stainless steel at 600°C and 20 MPa SC-CO2 environment, with a concentration of 10... -7 s -1 Comparison of intergranular oxidation morphology of cross sections obtained after straining to 10% strain rate.

[0025] Figure 3 The IGSCC-resistant austenitic stainless steel of Example 1 and the 20Cr25NiNb type austenitic stainless steel of Comparative Example 1 were subjected to a 10-year reaction in a 600°C, 20 MPa SC-CO2 environment. -7 s -1 Comparison of EBSD characterization and fracture morphology of cross-section cracks after strain rate stretching to fracture.

[0026] Figure 4 The IGSCC-resistant austenitic stainless steel of Example 1 and the 20Cr25NiNb type austenitic stainless steel of Comparative Example 1 were subjected to a 10-year reaction in a 600°C, 20 MPa SC-CO2 environment. -7 s -1 SEM characterization of cross-sectional cracks after strain rate stretching to fracture.

[0027] Figure 5 This is a conceptual diagram of the SC-CO2 stress corrosion testing device in Embodiment 1 of the present invention.

[0028] Figure 6 This is a physical image of the SC-CO2 stress corrosion testing device in Embodiment 1 of the present invention. Detailed Implementation

[0029] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, the specific embodiments of the present invention will be described in detail below with reference to the examples in the specification.

[0030] Many specific details are set forth in the following description in order to provide a full understanding of the invention. However, the invention may also be practiced in other ways different from those described herein, and those skilled in the art can make similar extensions without departing from the spirit of the invention. Therefore, the invention is not limited to the specific embodiments disclosed below.

[0031] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The phrase "in one embodiment" appearing in different places in this specification does not necessarily refer to the same embodiment, nor is it a single or selective embodiment that is mutually exclusive with other embodiments.

[0032] Unless otherwise specified, all raw materials used in the embodiments of this invention are commercially available.

[0033] Example 1 This invention provides a method for preparing austenitic stainless steel resistant to supercritical carbon dioxide intergranular stress corrosion cracking in heat exchanger components of SC-CO2 Brayton cycle power systems: (1) Weigh the following raw materials by mass fraction: 26% Ni, 2.5% Al, 19% Cr, 2% Mn, 0.6% Si, 0.4% Nb, 0.07% C, 1% Cu, 0.4% Ti, 2% Mo, with the balance being Fe.

[0034] (2) The pure metal matrix raw materials Fe, Cr, Ni, Mo, Nb, and Cu are mixed and placed in a crucible of a vacuum induction furnace. After being evacuated to a high vacuum, the furnace is smelted by electricity. The power supply during the heating and melting stage is 15 kW, and the power supply during the melting and refining stage is 30 kW. The furnace charge is heated to 1480℃ to fully melt the various metal raw materials and form a uniformly composed molten steel. The temperature of the molten steel is controlled at 1480℃. The vacuum degree in the furnace is maintained at less than 1×10⁻⁶. -2 Under Pa conditions, carbon material is first added to the molten steel, and vacuum carbon-oxygen degassing and refining are completed by keeping it warm and stirring. Then, metallic Al is added, fully melted and stirred for pre-deoxidation, and then refined at a constant temperature of 1480℃ for 10 min.

[0035] (3) After refining, 0.04 MPa argon gas is introduced, and metallic Mn and metallic Si are added sequentially. After complete melting and uniform stirring, metallic Ti is added last, and stirring is continued until all alloying elements are fully melted and uniformly mixed. (4) The smelted steel ingot is forged. During the forging process, the steel ingot is placed in a heating furnace and heated to 1200°C at a heating rate of 150°C / h, and held at that temperature for 1 hour; then cooled to 1100°C and held at that temperature for 1 hour. The initial forging temperature is controlled at 1100°C and the final forging temperature is controlled at 1000°C. After forging, the ingot is air-cooled to obtain a stainless steel forging billet, and the oxide scale on the surface of the stainless steel forging billet is removed.

[0036] (5) Heat treatment of stainless steel forging billets after descaling: first, solution treatment at 1140℃ for 60 min, then water cooling after removal from the furnace; then aging treatment at 800℃ for 10 h, then air cooling after removal from the furnace.

[0037] Example 2 The difference from Example 1 is that the raw material composition is adjusted. Specifically, the following raw materials are weighed out by mass fraction: 26% Ni, 2.5% Al, 19% Cr, 2% Mn, 0.6% Si, 0.3% Nb, 0.07% C, 1% Cu, 0.4% Ti, 2% Mo, with the balance being Fe.

[0038] Example 3 The difference from Example 1 is that the raw material composition is adjusted. Specifically, the following raw materials are weighed out by mass fraction: 26% Ni, 2.5% Al, 19% Cr, 2% Mn, 0.6% Si, 0.4% Nb, 0.07% C, 1% Cu, 0.2% Ti, 2% Mo, with the balance being Fe.

[0039] Example 4 The difference from Example 1 is that the raw material composition is adjusted. Specifically, the following raw materials are weighed out by mass fraction: 26% Ni, 2.5% Al, 19% Cr, 2% Mn, 0.6% Si, 0.4% Nb, 0.07% C, 1% Cu, 0.4% Ti, 1.5% Mo, with the balance being Fe.

[0040] Comparative Example 1 The difference from Example 1 is that the raw material composition is adjusted. Specifically, the following raw materials are weighed out by mass fraction: 25% Ni, 20% Cr, 0.7% Mn, 0.6% Si, 0.6% Nb, 0.04% C, and the balance is Fe.

[0041] Comparative Example 2 The difference from Example 1 is that the raw material composition is adjusted. Specifically, the following raw materials are weighed out by mass fraction: 25% Ni, 20% Cr, 0.6% Mn, 0.6% Si, 0.6% Nb, 0.04% C, and the balance is Fe.

[0042] Comparative Example 3 The difference from Example 1 is that the raw material composition is adjusted. Specifically, the following raw materials are weighed out by mass fraction: 25% Ni, 20% Cr, 0.7% Mn, 0.5% Si, 0.6% Nb, 0.04% C, and the balance is Fe.

[0043] Comparative Example 4 The difference from Example 1 is that the raw material composition is adjusted. Specifically, the following raw materials are weighed out by mass fraction: 12% Ni, 16% Cr, 1.5% Mn, 0.6% Si, 2% Mo, 0.03% C, 0.12% N, and the balance is Fe.

[0044] Comparative Example 5 The difference from Example 1 is that the raw material composition is adjusted. Specifically, the following raw materials are weighed in by mass fraction: 12% Ni, 16% Cr, 2% Mn, 0.7% Si, 2% Mo, 0.03% C, 0.14% N, and the balance is Fe.

[0045] Comparative Example 6 The difference from Example 1 is that the raw material composition is adjusted. Specifically, the following raw materials are weighed out by mass fraction: 26% Ni, 2.5% Al, 19% Cr, 2% Mn, 0.6% Si, 0.4% Nb, 0.07% C, 1% Cu, 2% Mo, with the balance being Fe.

[0046] Comparative Example 7 The difference from Example 1 is that in step (5), the stainless steel forging billet after removing the oxide scale is subjected to heat treatment: first, it is solution treated at 1140℃ for 60 min, then water-cooled after being taken out of the furnace; then it is aged at 700℃ for 10 h, and air-cooled after being taken out of the furnace.

[0047] Comparative Example 8 The difference from Example 1 is that in step (5), the stainless steel forging billet after removing the oxide scale is subjected to heat treatment: first, it is solution treated at 1140℃ for 60 min, then water-cooled after being taken out of the furnace; then it is aged at 800℃ for 100 h, and air-cooled after being taken out of the furnace.

[0048] Comparative Example 9 The preparation method described in Example 2 of patent CN114318169A differs from Example 1 of this invention in that, by mass fraction, the composition is: 26% Ni, 2.5% Al, 19% Cr, 2% Mn, 1% Si, 1% Nb, 0.08% C, 1.5% Cu, 4% Mo, with the balance being Fe. The mixture was aged at 700°C for 100 hours.

[0049] Comparative Example 10 The preparation method described in Example 1 of patent CN118345314A differs from Example 1 of this invention in that, by mass fraction, the composition is: 26% Ni, 2.5% Al, 19% Cr, 2% Mn, 1.5% Si, 0.6% Nb, 0.04% C, 1.5% Cu, 4% Mo, with the balance being Fe. The mixture was aged at 700°C for 100 hours.

[0050] The ingredients are shown in Table 1.

[0051] Table 1 (Unit: Percentage by Mass)

[0052] Corrosion tests were conducted on Examples 1-4 and Comparative Examples 1-10 in SC-CO2 (600℃, 20 MPa). The IGSCC resistance of the design scheme was evaluated by the average intergranular oxidation depth, average oxide film thickness, and the type of crack generated at tensile fracture. The results are as follows.

[0053] use Figure 5 , Figure 6 The SC-CO2 stress corrosion testing apparatus shown is divided into three main systems: gas supply, high-temperature experiment, and data acquisition and control. Each system has its own dedicated components and performs corresponding functions: the gas supply system supplies high-purity CO2 to achieve dynamic circulation of the corrosive medium and establish the required experimental pressure; the high-temperature experiment system includes an Inconel 625 alloy autoclave, heating device, pressure balancing components, and a tensile tester. Stress corrosion cracking tests are all completed in this module, and a single gas supply and control system can be equipped with four parallel high-temperature units, significantly improving experimental efficiency; the data acquisition and control system integrates temperature, pressure, tensile tester control, and DCPD signal acquisition functions, monitoring and recording environmental temperature and pressure, as well as mechanical parameters such as sample load and strain in real time throughout the process. The example and comparative sample specimens were fixed in the fixture inside the autoclave and subjected to constant strain rate tensile tests in a 600℃, 20 MPa SC-CO2 environment. After the system temperature and pressure reached the preset values, the tensile tester was started: first, the sample was loaded to 0.8 times its yield strength, then the constant strain rate control mode was switched, and the strain rate was increased to 10 MPa. -7 s -1 The strain rates were measured, and the samples were stretched to 10%, 14% strain, and fracture state, respectively. The material properties were evaluated by testing the average oxide film thickness, intergranular oxide depth, and crack initiation type. The numerical results are shown in Table 2. Crack types are listed below. Figure 3 and Figure 4 .

[0054] Table 2 (Unit: μm)

[0055] As shown in Table 2, among all samples prepared with different element ratios and heat treatment processes, Example 1 exhibited the best IGSCC resistance in a 600℃, 20 MPa SC-CO2 environment. Figure 1 It can be seen that the sample at 10 -7 s -1 The oxide film formed under constant strain rate test conditions has the smallest thickness and dense structure, which can effectively reduce the interfacial corrosion rate and improve the corrosion resistance stability of the material; at the same time, under all test strain conditions, its intergranular oxidation depth is lower than that of all other samples. Figure 2 The comparison results show the intergranular oxidation morphology of the samples after being stretched to 10% strain. In Example 1, the intergranular oxidation depth was only 2.783 μm, far smaller than the 13.786 μm of Comparative Example 1. In the alloy composition system described in this invention, the appropriate addition of Al promotes the formation of NiAl phase near the grain boundaries. The NiAl phase at the grain boundaries acts as an Al "reservoir," continuously supplying Al, allowing a continuous Al2O3 passivation film to form at the oxidation tip of the material. This effectively blocks the diffusion of corrosive media along the grain boundaries and inhibits creep crack propagation, improving the material's resistance to IGSCC. Furthermore, the addition of an appropriate amount of Al to the alloy precipitates a large amount of dispersed NiAl phase within the grains. This phase can pin dislocations, hinder intragranular slip, alleviate grain boundary stress concentration, and thus protect the grain boundaries and inhibit intergranular crack initiation. Figure 3 EBSD and SEM morphology analysis of the fracture surface showed that after tensile fracture, Example 1 had only about 8 μm transgranular cracks, and the fracture surface exhibited dimple-type transgranular fracture characteristics; while Comparative Example 1 showed a large number of intergranular cracks and grain boundary creep cracks exceeding 100 μm, and the fracture surface exhibited typical candy-like intergranular fracture, with severe corrosion damage. Figure 4 Further analysis shows that the cross-section of Example 1 is dominated by transgranular cracks, while the cross-section of the comparative sample is covered with long-scale intergranular cracks, and a large number of creep damage cracks are also distributed in the matrix. Based on the above characterization results, Example 1 exhibits excellent resistance to IGSCC in an SC-CO2 environment.

[0056] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the present invention.

Claims

1. An austenitic stainless steel resistant to intergranular stress corrosion cracking caused by supercritical carbon dioxide, characterized in that: The austenitic stainless steel resistant to supercritical carbon dioxide intergranular stress corrosion cracking contains nickel, chromium, aluminum, manganese, silicon, niobium, carbon, copper, titanium, molybdenum, and the balance is iron. The composition, by mass percentage of raw materials, includes 25.5-26.5% nickel, 18.5-19.5% chromium, 2-3% aluminum, 1.8-2.2% manganese, 0.5-0.7% silicon, 0.3-0.5% niobium, 0.05-0.08% carbon, 0.8-1.2% copper, 0.2-0.5% titanium, 1.5-2.2% molybdenum, with the balance being Fe.

2. The austenitic stainless steel resistant to intergranular stress corrosion cracking of supercritical carbon dioxide as described in claim 1, characterized in that: The raw materials, by mass percentage, contain 25.8-26% nickel, 18.8-19% chromium, 2.3-2.5% aluminum, 1.8-2.0% manganese, 0.5-0.6% silicon, 0.3-0.4% niobium, 0.06-0.07% carbon, 0.9-1.0% copper, 0.3-0.4% titanium, 1.8-2.0% molybdenum, with the balance being Fe.

3. The austenitic stainless steel resistant to intergranular stress corrosion cracking of supercritical carbon dioxide as described in claim 1 or 2, characterized in that: It also possesses the following characteristics: Under a supercritical carbon dioxide environment of 600℃ and 20 MPa, with a yield of 10... -7 s -1 Constant strain rate stretching; (i) Stretched to a strain of 14%, the average oxide film thickness on the surface is less than 1 μm; (ii) Stretched to a strain of 10%, the average intergranular oxidation depth of the cross section is less than 4 μm; (iii) When stretched to fracture, the fracture surface morphology shows transgranular fracture characteristics dominated by dimples, with no obvious intergranular cracks.

4. The method for preparing austenitic stainless steel resistant to intergranular stress corrosion cracking of supercritical carbon dioxide as described in any one of claims 1 to 3, characterized in that: Pure metal raw materials Fe, Cr, Ni, Mo, Nb and Cu are mixed and then smelted under vacuum until they are melted into a homogeneous molten steel. C is added while maintaining the vacuum, and the mixture is kept warm and stirred to complete the vacuum carbon and oxygen degassing refining. Then, metallic Al is added, and the mixture is fully melted, stirred and pre-deoxidized for refining. After refining, argon gas is introduced, and metallic Mn and metallic Si are added in sequence. After they are completely melted and stirred evenly, metallic Ti is added last, and stirring is continued until all alloying elements are fully and evenly dissolved. The smelted steel ingot is forged into shape, and after forging, it is air-cooled to obtain a stainless steel forging billet, and the oxide scale on the surface of the forging billet is removed. Austenitic stainless steel resistant to intergranular stress corrosion cracking caused by supercritical carbon dioxide is obtained by heat treatment of stainless steel forging billets after removing oxide scale.

5. The preparation method according to claim 4, characterized in that: During the forging process, the steel ingot is placed in a heating furnace and heated to 1200℃ at a heating rate of 150℃ / h, and held at that temperature for 1~2 h; then cooled to 1100~1180℃ and held at that temperature for 1 h; the initial forging temperature during forging is controlled at 1100~1180℃, and the final forging temperature is controlled at 950~1050℃; after forging is completed, it is air-cooled.

6. The preparation method according to claim 4, characterized in that: The vacuum power supply melting conditions are a melting temperature of 1420~1520℃ and a power supply of 5~40 kW.

7. The preparation method according to claim 4, characterized in that: The refining conditions are a vacuum degree of less than 1×10⁻⁶. -2 Pa, keep warm at 1480~1520℃ for no less than 10 min.

8. The preparation method according to claim 4, characterized in that: The heat treatment conditions are as follows: the stainless steel forging billet is solution treated at 1100~1200℃ for 60~120 min and then water-cooled, followed by aging treatment at 800~850℃ for 10 h, and then air-cooled after being taken out of the furnace.

9. The application of the austenitic stainless steel resistant to intergranular stress corrosion cracking of supercritical carbon dioxide as described in claim 1 in the preparation of components for supercritical carbon dioxide Brayton cycle high temperature and high pressure heat exchangers.

Citation Information

Patent Citations

  • Supercritical water / supercritical carbon dioxide corrosion resistant aluminum-containing austenitic stainless steel

    CN114318169A

  • High-strength corrosion-resistant austenitic stainless steel for supercritical carbon dioxide environment and preparation method of high-strength corrosion-resistant austenitic stainless steel

    CN118345314A