A pretreatment method for improving the room temperature tensile strength of nickel-based single-crystal superalloys and its application
By using a high-temperature, low-stress creep pretreatment method, the microstructure evolution of nickel-based single-crystal superalloys is controlled, forming a structure that is conducive to room-temperature strengthening. This solves the problem of improving the room-temperature tensile strength of nickel-based single-crystal superalloys and achieves controllable adjustment of strength and plasticity.
Patent Information
- Application Number
- CN202611247657.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-18
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies are insufficient to effectively improve the room temperature tensile strength of nickel-based single-crystal superalloys. Traditional methods tend to lead to excessive coarsening of the γ′ phase and a decrease in microstructure stability, making it difficult to effectively control strength and plasticity.
By applying a constant tensile stress of 130-180 MPa at 1050-1120℃ and continuously loading for 30-80 h, the microstructure inside the alloy is induced to undergo controllable evolution, forming a raft-shaped γ′ phase and dislocation accumulation, thus optimizing the γ/γ′ interface structure.
Without changing the alloy composition, the room temperature tensile strength and plasticity of nickel-based single-crystal superalloys are significantly improved, and the strength and plasticity can be controlled and adjusted. The effect is significant within an appropriate time range, and plasticity is restored outside the range.
Smart Images

Figure CN123108451A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of high-temperature structural material performance regulation technology, and in particular relates to a pretreatment method for improving the room temperature tensile strength of nickel-based single-crystal high-temperature alloys and its application. Background Technology
[0002] Turbine blades and other hot-end components in advanced power equipment such as gas turbines and aero-engines endure prolonged exposure to high temperatures, high stresses, and complex cyclic loads during service. This places extremely high demands on the high-temperature strength, creep resistance, fatigue resistance, and microstructural stability of the materials used. To meet the demands of modern aerospace equipment for high thrust-to-weight ratios, high efficiency, and long service life, a series of high-temperature alloy materials with excellent high-temperature load-bearing capacity have been developed both domestically and internationally. High-temperature alloys are advanced metallic structural materials with elements such as iron, cobalt, and nickel as their matrix, capable of withstanding large loads for extended periods in high-temperature environments above 600 °C while maintaining good microstructural stability. They are currently irreplaceable core materials in the manufacture of key hot-end components for aero-engines and gas turbines. Among them, nickel-based high-temperature alloys are the most widely used and have the best overall performance due to their excellent high-temperature strength, good oxidation resistance, and high microstructural stability. With the continuous increase in the thrust-to-weight ratio and operating temperature of aero-engines, nickel-based high-temperature alloys have undergone a development process from traditional cast equiaxed crystal alloys and directionally solidified columnar crystal alloys to nickel-based single-crystal high-temperature alloys. Currently, nickel-based single-crystal superalloys are widely used in key hot-end components such as aero-engine and gas turbine blades. By employing directional solidification technology to eliminate transverse grain boundaries, the material avoids high-temperature failure mechanisms such as grain boundary slip and grain boundary diffusion, thus significantly improving the high-temperature mechanical properties along specific crystal orientations. Simultaneously, due to the elimination of grain boundaries, nickel-based single-crystal superalloys typically no longer require the addition of grain boundary strengthening elements such as boron and cadmium, effectively reducing problems such as element segregation during casting, eutectic structures, and localized melting during heat treatment. This results in a more stable microstructure and superior service performance.
[0003] Nickel-based single-crystal superalloys exhibit a typical γ / γ′ two-phase microstructure. The γ matrix phase is a Ni-rich solid solution with a face-centered cubic structure, while the γ′ strengthening phase is a Ni3Al-based intermetallic compound with an L12 ordered structure, dispersed in the γ matrix in a regular cubic morphology. As the primary strengthening phase, the γ′ phase hinders dislocation movement and increases the difficulty of dislocation cutting and bypassing, thus enabling the material to achieve excellent high-temperature load-bearing capacity. After standard heat treatment, nickel-based single-crystal superalloys typically possess uniformly sized γ′ strengthening phases and continuously distributed γ channel structures, with low internal dislocation density and good microstructural stability. However, in actual manufacturing and service, nickel-based single-crystal superalloys not only need to meet high-temperature long-term service performance requirements but also need sufficient room-temperature processing performance and resistance to external loads. Especially during blade manufacturing, assembly, and service maintenance, the material is inevitably subjected to room-temperature mechanical loads. Therefore, improving the room-temperature tensile strength of nickel-based single-crystal superalloys is of great significance for improving the reliability and service safety of blade structures.
[0004] Currently, methods to improve the mechanical properties of nickel-based single-crystal superalloys mainly include alloy composition optimization, heat treatment regime control, and surface strengthening treatment. Among these, adjusting the content of alloying elements such as Al, Ta, W, and Re can alter the stability of the γ′ phase and the matrix solid solution strengthening effect; optimizing the solid solution and aging heat treatment regimes can control the size, morphology, and spatial distribution of the γ′ phase, thereby improving the overall material properties. However, these methods typically require changing the alloy composition or redesigning the heat treatment process, primarily targeting high-temperature creep performance optimization, with limited effect on improving room-temperature tensile properties. Furthermore, nickel-based single-crystal superalloys undergo complex microstructure evolution processes during long-term high-temperature service, including γ′ phase morphology transformation, γ / γ′ interface adjustment, and dislocation structure evolution. Currently, the conventional view is that high-temperature creep leads to material damage and performance degradation; therefore, existing research mainly focuses on creep life prediction, damage mechanism analysis, and failure behavior studies, with less attention paid to using controlled creep processes to induce microstructure changes for material strengthening. Existing research has shown that under certain temperature and stress conditions, nickel-based single-crystal superalloys undergo phenomena such as γ′ phase directional coarsening, dislocation rearrangement, and interface structure adjustment during creep. These microstructural changes may affect subsequent room-temperature deformation behavior. However, current research mainly focuses on the microstructural damage evolution under long-term service conditions, with limited research on using short-time, high-temperature, low-stress creep processes as a pretreatment method to actively control the room-temperature tensile properties of materials. Furthermore, traditional high-temperature pretreatment methods often lead to excessive γ′ phase coarsening, decreased microstructural stability, and reduced plasticity, making it difficult to effectively control strength and plasticity. Therefore, developing a novel pretreatment method that is simple in process, has controllable parameters, and can utilize creep-induced microstructural evolution to improve the room-temperature tensile strength of nickel-based single-crystal superalloys is of great significance for expanding the avenues for performance control of nickel-based single-crystal superalloys. Summary of the Invention
[0005] To overcome the shortcomings of the prior art, the present invention provides a pretreatment method for improving the room temperature tensile strength of nickel-based single-crystal superalloys and its application. The method induces a controllable evolution of the internal microstructure of the alloy through a high-temperature, low-stress creep process, thereby improving the room temperature tensile strength of the nickel-based single-crystal superalloy without changing the alloy composition, while simultaneously achieving the regulation of material strength and plasticity.
[0006] The technical solution adopted by the present invention to solve its technical problem is: a pretreatment method for improving the room temperature tensile strength of nickel-based single crystal superalloys, wherein a constant tensile stress of 130-180 MPa is applied to the nickel-based single crystal superalloy at 1050-1120℃ and the loading is continued for 30-80 h, so that the nickel-based single crystal superalloy produces a raft-shaped γ′ phase perpendicular to the stress axis, resulting in anisotropic characteristics and dislocation accumulation.
[0007] Furthermore, a constant tensile stress of 140±3MPa was applied to the nickel-based single-crystal superalloy at 1100±5 ℃ for 50±2 h.
[0008] Furthermore, the matrix channel width is greater than or equal to 300 nm, and the volume fraction of the raft-shaped γ′ reinforcing phase is less than 60%.
[0009] Furthermore, the crystal orientation of the nickel-based single-crystal superalloy is as follows: <001> The direction, and the stretching axis is parallel to this orientation.
[0010] Furthermore, the nickel-based single-crystal superalloy is a second-generation nickel-based single-crystal superalloy.
[0011] Furthermore, the nickel-based single-crystal superalloy undergoes the following treatment:
[0012] Solution treatment was performed by heating to 1315℃ at a rate of 30℃ / min and holding for 6 hours, followed by air cooling.
[0013] One aging treatment involves heating to 1130℃ at a rate of 30℃ / min, holding at that temperature for 4 hours, and then air cooling.
[0014] The second aging treatment involves heating to 870℃ at a rate of 30℃ / min, holding at that temperature for 32 hours, and then air cooling.
[0015] Furthermore, the nickel-based single-crystal superalloy is derived from aero-engine turbine blade components.
[0016] Furthermore, this pretreatment is carried out in a high-temperature creep testing machine.
[0017] This invention also discloses an application of the pretreatment method for improving the room temperature tensile strength of the above-mentioned nickel-based single-crystal superalloy, which is applied to the performance optimization of nickel-based single-crystal turbine blades for aero-engines or gas turbines.
[0018] This invention addresses the need to improve the room-temperature tensile properties of nickel-based single-crystal superalloys by proposing a performance control method based on high-temperature, low-stress, short-time creep pretreatment. By controlling the creep temperature, applied stress, and treatment time, the room-temperature tensile strength of the alloy is improved without altering its composition through creep-induced γ′ strengthening phase morphology adjustment, γ / γ′ interface structure optimization, and dislocation redistribution. Compared to traditional heat treatment strengthening methods, this invention requires no complex equipment or special alloy design; it improves the material's room-temperature load-bearing capacity simply by adding a pretreatment process. Furthermore, this invention reveals a distinct time window characteristic for this strengthening effect: the material achieves high strength within an appropriate creep time range, while the strengthening effect gradually disappears with further extension of the treatment time, while plasticity is restored, achieving controllable adjustment of material strength and plasticity. Therefore, this invention provides a new technical route for optimizing the performance of nickel-based single-crystal superalloys and has significant application value in the manufacturing and service performance improvement of high-performance turbine blades for aero-engines and gas turbines.
[0019] This invention achieves active control of the microstructure of nickel-based single-crystal superalloys through a high-temperature, low-stress, short-time creep process. The method includes high-temperature loading, microstructure evolution, and performance optimization: First, by controlling the creep temperature and applying stress, the alloy undergoes limited plastic deformation and microstructure adjustment under high-temperature conditions. Subsequently, through dislocation movement, γ′ phase morphology adjustment, and γ / γ′ interface evolution generated during creep, a microstructure favorable for room-temperature strengthening is formed within the material. The raft-like structure causes stress redistribution, and the γ′ phase perpendicular to the stress axis hinders dislocation movement in the tensile direction, leading to dislocation accumulation and stress concentration, which contributes to tensile strength. Finally, cooling treatment yields a nickel-based single-crystal superalloy with high room-temperature tensile strength. When the pretreatment time is short, a stable strengthened microstructure is formed within the alloy, exhibiting high room-temperature yield strength and tensile strength. As the pretreatment time increases further, with prolonged high-temperature exposure, the microstructure further recovers and coarsens, and the strengthening effect gradually decreases, but the material's plasticity is restored. This invention achieves adjustable strength and plasticity of nickel-based single-crystal superalloys by controlling the high-temperature creep time window. Specifically, a 50-hour pre-creep treatment at 1100 °C and 140 MPa results in significant room-temperature strengthening; however, extending the treatment time to 150 hours reduces the strengthening effect while restoring the material's plasticity. This invention can be implemented using conventional high-temperature creep equipment, without altering the alloy's chemical composition or requiring complex surface treatments or special heat treatment equipment. It offers advantages such as simple process, low cost, high repeatability, and strong engineering applicability. This method can be applied to the manufacturing and performance optimization of nickel-based single-crystal turbine blades in advanced power equipment such as aero-engines and gas turbines.
[0020] The beneficial effects of this invention are: (1) This invention proposes a novel pretreatment method based on high-temperature low-stress creep-induced strengthening, which breaks through the traditional understanding that the creep process only leads to material damage and performance degradation, and realizes the active improvement of material performance by utilizing the evolution of creep structure; (2) This invention does not require changing the chemical composition of nickel-based single-crystal high-temperature alloys, and can improve the room temperature tensile strength of materials through pretreatment processes, which has the characteristics of simple process and convenient implementation; (3) This invention can achieve the control of γ′ strengthening phase morphology, γ / γ′ interface structure and dislocation state by controlling creep temperature, stress and time parameters, thereby improving the material's resistance to room temperature plasticity. (4) The present invention has discovered a time window for high temperature and low stress creep strengthening. Within an appropriate treatment time range, higher strength can be obtained. However, if the treatment time is extended further, the strengthening effect disappears but the plasticity of the material can be restored. (5) The equipment used in the present invention is a conventional high temperature creep test equipment. It is simple to operate and has strong adaptability to sample size and shape. It can be used for performance optimization of nickel-based single crystal high temperature alloy components with different structural forms. (6) This method is particularly suitable for the pre-service performance regulation of nickel-based single crystal turbine blades for aero-engines and gas turbines. It can improve the reliability and service life of key hot-end components and has high engineering application value and economic benefits. Attached Figure Description
[0021] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the embodiments are briefly described below. Obviously, the drawings described below are merely some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0022] Figure 1 a is an untreated nickel-based single-crystal superalloy subjected to room temperature along... <001> Stress-strain curves under uniaxial tension.
[0023] Figure 1 b is a nickel-based single-crystal superalloy that has undergone rafting treatment at 1100℃ / 140MPa / 50h and then subjected to room temperature rafting. <001> Stress-strain curves under uniaxial tension.
[0024] Figure 2 a is an SEM image of the two-phase microstructure of an untreated nickel-based single-crystal superalloy.
[0025] Figure 2 b is a SEM image of the two-phase microstructure of the nickel-based single-crystal superalloy after rafting treatment at 1100℃ / 140MPa / 50h.
[0026] Figure 3 a is a TEM image of the two-phase microstructure of an untreated nickel-based single-crystal superalloy.
[0027] Figure 3 b is a TEM image of the two-phase microstructure of a nickel-based single-crystal superalloy after rafting treatment at 1100℃ / 140MPa / 50h.
[0028] Figure 4 It is a rafting treatment at room temperature for 1100℃ / 140MPa / 120h followed by... <001> Stress-strain curves under uniaxial tension. Detailed Implementation
[0029] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0030] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, the present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments.
[0031] Example 1
[0032] Standard tensile specimens of nickel-based single-crystal superalloys were prepared (chemical composition: 4.4 parts Cr, 8.7 parts Co, 2.1 parts Mo, 7.1 parts Ta, 9.6 parts W, 2.0 parts Re, 5.2 parts Al, 0.7 parts Nb, and balance Ni). The crystal orientation of the specimens was as follows: <001> direction.
[0033] The nickel-based single-crystal superalloy underwent the following treatments: solution treatment, heating to 1315℃ at 30℃ / min, holding for 6 hours, followed by air cooling; first aging treatment, heating to 1130℃ at 30℃ / min, holding for 4 hours, followed by air cooling; and second aging treatment, heating to 870℃ at 30℃ / min, holding for 32 hours, followed by air cooling.
[0034] The processed samples were subjected to different pretreatments. One group of samples was not pretreated and was used directly as the initial state samples. The other group of samples was first subjected to high temperature and low stress creep pretreatment.
[0035] For the pretreated samples, they were placed in a high-temperature tensile creep testing apparatus and subjected to a constant tensile stress of 140 MPa at 1100 ℃ for 50 h. This temperature, below the alloy's melting temperature, ensured the alloy maintained its solid-state microstructure while promoting microstructural adjustment between the γ′ strengthening phase and the γ matrix. Specifically, the average width of the matrix channels was 400±50 nm, and the volume fraction of the strengthening phase was 57±2%. After creep treatment, the samples were cooled to room temperature and subjected to room-temperature tensile property tests simultaneously with untreated samples.
[0036] Figure 1 The figures show the room temperature tensile stress-strain curves of the untreated sample and the sample subjected to a high-temperature, low-stress creep pretreatment at 1100 ℃ / 140 MPa / 50 h. Figure 1 (a) is the room temperature tensile curve of an untreated nickel-based single-crystal superalloy. Figure 1 (b) is the room temperature tensile curve after high temperature and low stress creep pretreatment.
[0037] Depend on Figure 1 It can be seen that the room temperature tensile properties of nickel-based single-crystal superalloys were significantly improved after pre-creep treatment at 1100 ℃ / 140 MPa / 50 h. Compared with the untreated sample, the pretreated alloy exhibited higher yield strength and ultimate strength, with the yield strength increasing from 780 MPa to over 1000 MPa and the ultimate strength increasing from 908 MPa to over 1200 MPa. This indicates that the short-term high-temperature, low-stress creep process can effectively improve the material's room temperature load-bearing capacity, especially with a significant enhancement in tensile strength.
[0038] Simultaneously, it can be observed that the elongation after fracture of the pretreated sample is lower than that of the untreated sample, indicating that the pretreatment process, while improving the material strength, also has a certain impact on room temperature plasticity. This suggests that high-temperature, low-stress creep induces a high-strength microstructure, achieving the control of strength and plasticity of nickel-based single-crystal superalloys.
[0039] Furthermore, the microstructure of the samples before and after pretreatment was characterized to analyze the effect of high-temperature low-stress creep pretreatment on the material strengthening mechanism.
[0040] γ / γ′ two-phase microstructure of untreated samples, such as Figure 2 As shown in Figure a, the γ′ strengthening phase maintains a regular cubic morphology and is uniformly distributed in the γ matrix, with continuous γ channels.
[0041] The sample, after undergoing a high-temperature, low-stress creep pretreatment at 1100 ℃ / 140 MPa / 50 h, exhibits the following γ / γ′ two-phase microstructure: Figure 2As shown in b, it can be observed that after pretreatment, the alloy still maintains the typical two-phase microstructure of a single-crystal superalloy, the γ′ strengthening phase is not significantly damaged, and the γ / γ′ interface is adjusted to a certain extent.
[0042] The microstructure before and after pretreatment was further analyzed using transmission electron microscopy (TEM).
[0043] Further observation of dislocation structure changes before and after pretreatment was conducted using TEM. Figure 3 As shown in a, the number of dislocations inside the untreated sample is small, and the γ channel maintains a continuous structure.
[0044] TEM images of the sample after high-temperature, low-stress creep treatment at 1100 ℃ / 140 MPa / 50 h are shown below. Figure 3 As shown in b, it can be observed that dislocations generated during creep redistribute near the γ / γ′ interface, forming a stable interfacial dislocation structure. This structure enhances the ability to impede dislocation movement, resulting in higher yield strength of the material during room temperature tensile testing.
[0045] The results show that:
[0046] After a high-temperature, low-stress creep pretreatment at 1100 ℃ / 140 MPa / 50 h, the internal dislocation structure and interface state of the nickel-based single-crystal superalloy were significantly regulated. The anisotropic structural characteristics and stable interface dislocation structure induced by creep increased the resistance to dislocation movement during room temperature deformation, resulting in higher room temperature tensile strength of the alloy.
[0047] Therefore, this embodiment demonstrates that by controlling the high-temperature, low-stress creep pretreatment parameters, the room-temperature tensile properties of nickel-based single-crystal superalloys can be effectively improved.
[0048] Example 2
[0049] This embodiment uses the same nickel-based single-crystal high-temperature alloy sample as in Embodiment 1, the difference being the different high-temperature low-stress creep pretreatment time.
[0050] Nickel-based single-crystal superalloy specimens were placed in a high-temperature tensile creep testing apparatus and subjected to a constant tensile stress of 140 MPa at 1100 °C for 150 h. After the creep treatment, the specimens were cooled to room temperature and their room temperature tensile properties were tested.
[0051] Figure 4 The figure shows the room temperature tensile stress-strain curve of a nickel-based single-crystal superalloy after high-temperature low-stress creep pretreatment at 1100 ℃ / 140 MPa / 150 h.
[0052] Depend on Figure 4It can be seen that, compared with the sample pretreated at 1100 ℃ / 140 MPa / 50 h in Example 1, after extending the creep treatment time to 150 h, the improvement effect of room temperature tensile strength of the material is significantly reduced, and the yield strength and tensile strength gradually recover to the level of the untreated sample.
[0053] Meanwhile, the samples treated with 150 h of high temperature and low stress creep showed higher elongation after fracture, and the room temperature plasticity of the material was significantly restored. This indicates that as the high temperature treatment time is further extended, the strengthening structure formed in the early creep process gradually recovers and is adjusted, causing the material to transform from a high strength state to a high plasticity state.
[0054] Further analysis suggests that during the short-term high-temperature, low-stress creep process, the morphology of the γ′ strengthening phase, the γ / γ′ interface structure, and the dislocation configuration within the alloy undergo rapid adjustments, forming a stable microstructure that effectively hinders dislocation movement at room temperature, thereby improving the material's strength. However, when the creep time is extended to 150 hours, the sustained high temperature promotes dislocation recovery, interface relaxation, and the stabilization transformation of the strengthening structure, gradually reducing the original strengthening effect. Simultaneously, it lowers the internal deformation resistance of the material and improves its plastic deformation capacity.
[0055] The results show that:
[0056] Under conditions of 1100 ℃ / 140 MPa, the room temperature tensile properties of nickel-based single-crystal superalloys exhibit a significant time dependence with creep time. A 50 h pre-creep treatment can achieve high room temperature tensile strength, but after extending the treatment to 150 h, the strengthening effect disappears but the plasticity recovers.
[0057] The results demonstrate that the high-temperature, low-stress creep pretreatment method proposed in this invention has a reasonable time control window, and the room temperature strength and plasticity of nickel-based single-crystal superalloys can be controlled by controlling the creep time.
[0058] Example 3
[0059] The sample pre-deformation treatment method in this embodiment is consistent with that in Embodiment 1. Pre-treatment times were selected as 30h, 50h, 80h, 100h, and 120h, respectively, while other parameters (load stress, holding temperature) remained the same as in Embodiment 1. The different pre-treatment times will result in different driving forces and varying degrees of alloy control. Tensile tests were conducted on alloys with different treatment times to analyze the optimal treatment time. The results are shown in Table 1, which indicates whether strengthening occurred and the degree of strengthening.
[0060] Table 1
[0061]
[0062] Note: 0h represents the initial sample without pretreatment.
[0063] Example 4
[0064] The sample pre-deformation treatment method in this embodiment is consistent with that in Embodiment 1. The difference lies in the selection of the loading stress and the experimental temperature.
[0065] Table 2
[0066]
[0067] The results shown in Tables 1 and 2 indicate that pretreatment time, temperature, and applied stress have a significant impact on the room-temperature tensile strengthening effect of nickel-based single-crystal superalloys. The alloy achieves the best strengthening effect when the pretreatment conditions are 1100 ℃ / 140 MPa / 50 h; however, excessively long treatment times or unsuitable temperature-stress combinations lead to a decrease in the strengthening effect. For example... Figure 4 As shown, increasing the pretreatment time to 120 hours resulted in a decrease in both the yield strength and ultimate strength of the alloy, indicating the disappearance of the strengthening effect. This demonstrates that the high-temperature, low-stress creep pretreatment method proposed in this invention has a reasonable process window, and appropriate treatment parameters can effectively control the alloy microstructure, improve room temperature tensile strength, and optimize the material's strength and ductility.
[0068] It should be noted that, for those skilled in the art, it is obvious that the present invention is not limited to the details of the above exemplary embodiments, and that the present invention can be implemented in other specific forms without departing from the spirit or essential characteristics of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within the present invention, and no reference numerals in the claims should be construed as limiting the scope of the claims.
[0069] Specific examples have been used to illustrate the principles and implementation methods of this invention. The descriptions of the above embodiments are only for the purpose of helping to understand the method and core ideas of this invention. Furthermore, those skilled in the art will recognize that, based on the ideas of this invention, there will be changes in the specific implementation methods and application scope. Therefore, the content of this specification should not be construed as a limitation of this invention.
Claims
1. A pre-treatment method for improving room temperature tensile strength of a nickel-based single crystal superalloy, characterized in that: A constant tensile stress of 130-180 MPa is applied to the nickel-based single crystal superalloy at 1050-1120 °C for 30-80 h to produce rafted γ' phase perpendicular to the stress axis, anisotropic features and dislocation accumulation in the nickel-based single crystal superalloy.
2. The pretreatment method for improving the room temperature tensile strength of nickel-based single-crystal superalloys according to claim 1, characterized in that: A constant tensile stress of 140±3 MPa is applied to the nickel-based single crystal superalloy at 1100±5 °C for 50±2 h.
3. The pretreatment method for improving the room temperature tensile strength of nickel-based single-crystal superalloys according to claim 1, characterized in that: The substrate channel width is greater than or equal to 300 nm, and the volume fraction of the rafted γ' strengthening phase is less than 60%.
4. The pretreatment method for improving the room temperature tensile strength of nickel-based single-crystal superalloys according to claim 1, characterized in that: The nickel-based single crystal superalloy has a crystal orientation of <001> direction, and the tensile axis is parallel to the orientation.
5. The pretreatment method for improving the room temperature tensile strength of nickel-based single-crystal superalloys according to claim 1, characterized in that: The nickel-based single crystal superalloy is a second generation nickel-based single crystal superalloy.
6. The pretreatment method for improving the room temperature tensile strength of nickel-based single-crystal superalloys according to claim 1, characterized in that: The nickel-based single crystal superalloy is subjected to the following treatments, a solution treatment, heating at 30 °C / min to 1315 °C, holding for 6 h, and then air cooling; a first aging treatment, heating at 30 °C / min to 1130 °C, holding for 4 h, and then air cooling; a second aging treatment, heating at 30 °C / min to 870 °C, holding for 32 h, and then air cooling.
7. The method of claim 1, wherein the method is performed at a temperature of 600- 800°C. The nickel-based single crystal superalloy is taken from an aero-engine turbine blade component.
8. The method of claim 1, wherein the method is performed at a temperature of about 600 °C to about 800 °C. The pretreatment is carried out in a high-temperature creep testing machine.
9. Use of a pre-treatment method for increasing the room temperature tensile strength of a nickel-based single crystal superalloy according to any one of claims 1 to 8, characterized in that: It is applied to performance optimization of nickel-based single crystal turbine blades of aero-engines or gas turbines.