A low-temperature preparation process for plasma spraying yttrium oxide onto a carbon-carbon substrate surface
By spraying yttrium oxide onto the surface of a carbon-carbon substrate and implementing active temperature control throughout the process, the problems of substrate oxidation and coating cracking caused by excessively high temperatures during plasma spraying of carbon-carbon substrates were solved, achieving a low-temperature preparation process and improving coating adhesion and wafer cleanliness.
Patent Information
- Application Number
- CN202611601553.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-16
- Publication Date
- 2026-11-17
AI Technical Summary
In the existing plasma spraying process for yttrium oxide onto carbon-carbon substrates, the spraying flame causes excessively high temperatures in the carbon-carbon substrate, leading to substrate oxidation, high thermal stress at the coating interface, coating cracking and peeling, and particulate contamination.
A yttrium oxide protective ceramic coating is applied to the surface of a carbon-carbon composite substrate using plasma spraying. The substrate temperature is controlled within a low-temperature range of 20℃ to 150℃ by an active temperature control system throughout the process. Combined with a SiC transition layer and low-temperature annealing, thermal stress and particulate contamination are reduced.
It effectively inhibits carbon-carbon substrate oxidation, reduces thermal stress at the coating-substrate interface, enhances coating adhesion, reduces particulate contamination, and improves coating service reliability and wafer yield.
Smart Images

Figure CN123108467A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of coating preparation technology, and specifically discloses a low-temperature preparation process for plasma spraying yttrium oxide onto the surface of a carbon-carbon substrate. Background Technology
[0002] In semiconductor dry etching equipment, carbon-carbon composite substrates have advantages such as low density, high thermal conductivity, and low coefficient of thermal expansion, making them suitable as wafer carriers. However, carbon-carbon substrates are easily corroded by plasma bombardment in fluorine and chloride plasma etching environments, resulting in particulate contamination. Therefore, a yttrium oxide (Y₂O₃) ceramic protective coating is typically prepared on the surface of the carbon-carbon substrate. This coating utilizes yttrium oxide's excellent resistance to plasma corrosion to protect the substrate and reduce wafer contamination.
[0003] Current technologies typically employ atmospheric plasma spraying to prepare yttrium oxide coatings on carbon-carbon composite materials. Plasma spraying involves extremely high flame temperatures, causing a significant temperature increase in the substrate during the spraying process due to continuous heating. Carbon-carbon composite materials are prone to oxidation damage under high-temperature environments. Furthermore, the large difference in thermal expansion coefficients between yttrium oxide ceramic and the carbon-carbon substrate leads to substantial thermal stress at the coating-substrate interface due to the high spraying temperatures. This can cause coating cracking and interface delamination, resulting in coating peeling and particle shedding during semiconductor etching operations, thus affecting wafer yield.
[0004] Currently, most methods for improving carbon-carbon matrix yttrium oxide coatings focus on introducing a SiC transition layer, optimizing the composition of sprayed powder, and using suspension plasma spraying to enhance coating adhesion through interface modification or coating microstructure optimization.
[0005] For example, Chinese invention patent application publication number CN121293017A discloses a high-resistance yttrium oxide coating for semiconductor devices and its preparation method. The above scheme uses SPPS solution precursor plasma spraying to set a SiC transition layer and a yttrium oxide (Y2O3) surface layer; it is applied to semiconductor plasma etching cavity components.
[0006] For example, Chinese invention patent application publication number CN120231032A discloses a method for preparing a yttrium oxide insulating coating for a carbon fiber carrier plate used in a PECVD chamber. This method includes the following steps: Step 1: Cleaning the carbon fiber carrier plate; Step 2: Drying the carbon fiber carrier plate; Step 3: Spraying the carbon fiber carrier plate; Step 4: Polishing the carbon fiber carrier plate. In this method, the high-temperature stability of the yttrium oxide coating protects the carbon fiber carrier plate from high-temperature damage during the PECVD process, extending its service life. The yttrium oxide coating has excellent corrosion resistance, protecting the carbon fiber carrier plate from corrosive gases. The yttrium oxide coating has high hardness and wear resistance, improving the surface strength of the carbon fiber carrier plate and reducing wear and damage. Plasma spraying technology optimizes the bonding strength between the coating and the carbon fiber substrate, ensuring the stability and reliability of the coating during the PECVD process.
[0007] For example, Chinese invention patent application publication number CN122212218A discloses a yttrium oxide-based coating material, a composite carrier, and a method for preparing the same. The yttrium oxide-based coating material has a core-shell structure, including a yttrium oxide core and a silicon outer shell layer covering the yttrium oxide core. The composite carrier prepared using the yttrium oxide-based coating material as a raw material overcomes the defect of insufficient coating bonding strength in the prior art and solves the technical problem that the poor bonding effect between the existing yttrium oxide coating and carbon / carbon composite materials makes it difficult for the carrier to meet the process requirements of photovoltaic cells.
[0008] Chinese invention patent application publication number CN122128654A discloses a yttrium oxide gradient protective coating for a graphite substrate, its preparation method, and its application. The yttrium oxide gradient protective coating comprises a silicon carbide layer, a transition layer, and a yttrium oxide layer sequentially stacked on a graphite substrate. The silicon carbide layer is formed by atmospheric plasma spraying of silicon carbide powder and graphite powder. The transition layer is formed by atmospheric plasma spraying of silicon carbide powder, graphite powder, and yttrium oxide powder. The yttrium oxide layer is formed by atmospheric plasma spraying of yttrium oxide powder. Furthermore, along the direction from the silicon carbide layer to the yttrium oxide layer, the content of silicon carbide and graphite in the yttrium oxide gradient protective coating gradually decreases. This invention, by introducing graphite powder to protect silicon carbide and combining the gradient structure design with atmospheric plasma spraying technology, significantly improves the interfacial bonding strength between the protective coating and the graphite substrate, and effectively reduces the risk of thermal cycling cracking of the coating.
[0009] The above-mentioned solutions alleviate thermal stress through composition gradients, but do not alleviate matrix oxidation and interfacial thermal stress by suppressing the temperature rise of the matrix. The defects of high-temperature oxidation of the matrix and thermal stress cracking of the coating in the carbon-carbon carrier plate during the spraying preparation stage have not been effectively solved. None of the above-mentioned existing technologies implement active low-temperature control of the carbon-carbon composite carrier plate matrix during the spraying process. Summary of the Invention
[0010] The purpose of this invention is to overcome the defects in the existing plasma spraying process for yttrium oxide on carbon-carbon substrates, which causes excessively high temperatures in the carbon-carbon substrate due to the spraying flame, leading to substrate oxidation, high thermal stress at the coating interface, coating cracking and peeling, and particulate contamination. This invention provides a low-temperature preparation process for plasma spraying yttrium oxide onto carbon-carbon substrates, which actively controls the carbon-carbon composite substrate to maintain a low temperature during plasma spraying, inhibiting carbon-carbon substrate oxidation, reducing thermal stress at the coating-substrate interface, improving coating adhesion, and reducing particulate contamination.
[0011] To achieve the above objectives, the present invention provides the following basic solution: a low-temperature preparation process for plasma spraying yttrium oxide onto a carbon-carbon substrate surface, comprising the following steps:
[0012] Step S1: Perform surface pretreatment on the carbon-carbon composite material carrier substrate to remove oil stains and surface impurities and complete roughening and activation;
[0013] Step S2: Fix the pretreated carbon-carbon composite material carrier plate substrate to a spraying and cooling fixture system with real-time active temperature control;
[0014] Step S3: Apply a yttrium oxide protective ceramic coating to the surface of the carbon-carbon composite substrate using a plasma spraying process;
[0015] Throughout the plasma spraying process, continuous active temperature control is implemented on the carbon-carbon composite substrate to regulate and stabilize the substrate temperature within the low-temperature process range of 20℃ to 150℃.
[0016] The system implements a zoned control strategy based on the real-time temperature of the substrate:
[0017] When the temperature of the carbon-carbon composite material carrier substrate is in the range of 20℃ to 150℃, maintain constant temperature steady-state spraying.
[0018] When the temperature of the carbon-carbon composite carrier substrate exceeds the 150℃ over-temperature threshold, an over-temperature treatment strategy is initiated to suppress the temperature rise of the carbon-carbon composite carrier substrate.
[0019] When the temperature of the carbon-carbon composite substrate is below the low temperature threshold of 20°C due to the initial temperature of the cooling medium being too low, or during non-continuous spraying conditions such as the gap between spray gun sweeps or restarting after a shutdown, a low temperature treatment strategy is initiated to reduce heat dissipation intensity and perform temperature correction.
[0020] Furthermore, the carbon-carbon composite material carrier obtained through steps S1-S3 is used as a wafer carrier in semiconductor dry etching equipment or PECVD equipment.
[0021] Furthermore, the active temperature control is achieved by a full-area bonding low-temperature spraying fixture system, which includes a back-side full-area bonding cooling fixture, a high-frequency temperature acquisition module, a variable frequency flow regulation module, and a temperature control computing terminal.
[0022] The cooling fixture fits seamlessly with the back of the carrier plate, and a uniform cooling channel is provided inside the cooling fixture. A high-frequency temperature acquisition module is embedded in the side of the carbon-carbon composite carrier plate substrate to collect the body temperature of the carbon-carbon composite carrier plate substrate. The sampling frequency of the high-frequency temperature acquisition module is ≥100Hz, and the response time of the temperature sensor used is ≤10ms (the temperature sensor uses a thin-film thermocouple). The high-frequency temperature acquisition module is electrically connected to the frequency conversion flow regulation module and the temperature control calculation terminal.
[0023] Furthermore, throughout the plasma spraying process, a combined feedforward compensation and PID feedback temperature control algorithm is employed to regulate the temperature at the substrate measurement points. This combined feedforward compensation and PID feedback temperature control algorithm includes the following steps:
[0024] Step A1: Establish a steady-state PID feedback model for matrix temperature:
[0025] ;
[0026] Wherein, ΔQ is the cooling medium flow rate adjustment (control output, ΔQ positive indicates decreasing the cooling medium flow rate, ΔQ negative indicates increasing the cooling medium flow rate), and the substrate temperature is measured in real time. Acquired through a high-frequency temperature acquisition module. To preset the target low temperature, For real-time temperature deviation, = , , , These are the proportional, integral, and differential coefficients, respectively. The feedforward compensation amount (with the same dimensions as the control output) is the real-time heat input of the plasma flame after conversion by equivalent heat capacity and flow rate.
[0027] Step A2: Establish an empirical feedforward compensation model for the heat input of the spraying process, and dynamically calculate the real-time heat input feedforward compensation amount of the plasma flame after normalization by the substrate heated area, equivalent heat capacity, and flow rate equivalent. :
[0028] ;
[0029] Where P is the real-time spraying power, L is the spraying distance, v is the spray gun moving speed, and α is the process-related comprehensive calibration coefficient (including the heated area, the equivalent heat capacity of the substrate, and the flow equivalent conversion); the thermal shock is predicted in advance by the process-calibrated spraying heat input experience feedforward compensation model, and the cooling amount is compensated in advance to reduce the lag deviation of the substrate temperature control.
[0030] Step A3: Set the PID parameters: proportional coefficient Kp = 0.8~1.5, integral coefficient Ki = 0.02~0.1, and derivative coefficient Kd = 0.05~0.2; the control deviation of the substrate measuring point temperature relative to the target temperature shall not exceed ±3℃, that is, the temperature fluctuation of a single point on the substrate under the target temperature in each spraying stage shall not exceed ±3℃; the substrate temperature range given in the following examples is the target temperature range set for different spraying stages.
[0031] Furthermore, the over-temperature handling strategy is as follows: when the substrate temperature is greater than 150°C, the spraying cooling fixture system immediately and dynamically increases the flow rate of the cooling medium and reduces the heat input of the spray gun to lower the substrate temperature. After the temperature drops back to the range of 20°C to 150°C, the steady-state spraying parameters are restored. The low-temperature handling strategy is as follows: when the substrate temperature is lower than 20°C due to the initial temperature of the cooling medium being too low, the spray gun sweeping gap, or the instantaneous temperature drop after shutdown and restart, the system reduces the flow rate of the cooling medium to reduce the heat dissipation intensity and maintain the substrate temperature within the process window.
[0032] Furthermore, the back-side full-area bonding cooling fixture is cooled by either water cooling or air cooling.
[0033] When water cooling is used, the cooling water temperature is controlled between 10 and 30°C, and the flow rate is dynamically adjusted to between 2 and 15 L / min.
[0034] When air cooling is used: the outlet air temperature is controlled at ≤25℃ and the air speed is controlled at ≥15m / s to achieve rapid and uniform heat dissipation with high heat flux.
[0035] Furthermore, in step S1: the surface is roughened by sandblasting with 80# to 120# SiC sand, with a surface roughness Ra=2.0 to 6.0μm; then it is ultrasonically cleaned with organic solvent, rinsed with deionized water, and finally dried at a low temperature of 100 to 120℃.
[0036] Furthermore, in step S3, the plasma spraying parameters in the plasma process include: argon as the main gas 35-55 L / min, hydrogen as the auxiliary gas 3-8 L / min, spraying power 35-55 kW, spraying distance 80-120 mm, powder feeding rate 15-35 g / min, and spray gun moving speed 300-600 mm / s; yttrium oxide powder purity ≥99.9% and particle size 10-45 μm.
[0037] Furthermore, before spraying the yttrium oxide protective ceramic coating, a SiC transition layer, a pure silicon transition layer, or a silicon-yttrium composite transition layer is pre-placed, with a transition layer thickness of 10–40 μm.
[0038] Furthermore, it also includes step S4, after the spraying is completed, low-temperature annealing at 120-180℃ is carried out, and the temperature is maintained for 1-3 hours, followed by natural cooling in the furnace.
[0039] The principle and effect of this solution are as follows:
[0040] Compared with existing technologies, this invention continuously removes heat from the carbon-carbon composite substrate throughout the plasma spraying process using a feedforward compensation and PID feedback composite temperature control system, stably maintaining the substrate temperature within a low-temperature range of 20℃ to 150℃. The oxidation rate of the carbon-carbon matrix is affected by factors such as material composition, atmosphere, temperature, and exposure time. Lowering the substrate temperature helps reduce the risk of thermal oxidation, protecting the carbon-carbon matrix skeleton structure and its mechanical properties and dimensional accuracy. Simultaneously, a zoned temperature control strategy is implemented; once the substrate temperature exceeds the 150℃ threshold, the system immediately activates an enhanced heat dissipation compensation mechanism to rapidly lower the substrate temperature, reducing the risk of continuous temperature rise and localized overheating damage.
[0041] Compared with existing technologies, the thermal expansion coefficients of carbon-carbon substrates and yttrium oxide ceramics differ significantly. Under spraying conditions lacking effective temperature control, substrate temperature fluctuations and thermal expansion mismatch between the coating and the substrate may increase the risk of cracking and interface delamination. This invention helps reduce thermal expansion mismatch strain during the overall cooling stage after deposition by controlling substrate temperature rise and fluctuations. The total residual stress of the coating is also affected by droplet solidification, temperature gradient, coating structure, and constraint conditions; its changes should be judged in conjunction with measurement results. Simultaneously, the combination of SiC, pure silicon, or silicon-yttrium composite transition layers, through reasonable material composition and layer structure design, helps alleviate the thermal expansion mismatch problem. Experimental results show that the crack rate of the coating using this invention can be as low as 0.4%, far lower than the 7.3% crack level of existing processes, significantly improving the coating's service reliability.
[0042] Compared to existing technologies, a continuous and well-covered silicon-based transition layer helps to seal open pores on the carbon-carbon matrix surface. This reduces the risk of uneven local deposition caused by molten yttrium oxide droplets entering the pores. Furthermore, suitable transition layer morphology and interface structure improve coating adhesion. Whether interfacial chemical bonding forms should be determined based on the transition layer preparation conditions and interface characterization results. With a low-temperature spraying environment, the damage to the nascent interface from high-temperature thermal shock is reduced, and the interfacial bonding strength can reach up to 24.2 MPa, higher than the comparative experiments conducted in this group where back-side cooling or the SiC transition layer was omitted.
[0043] Compared to existing technologies, the porosity and microcracks in sprayed coatings are influenced by factors such as particle state, substrate temperature, etching method, and coating thickness. Fluorine-chlorine plasma etching media easily penetrate along pores and cracks to the interface, continuously corroding it and causing coating peeling, resulting in a large number of particles that contaminate the semiconductor wafer. The low-temperature controlled process of this invention produces a coating with a porosity as low as 2.1%, higher coating density, enhanced resistance to plasma erosion, and significantly reduced etching weight loss. The coating is less prone to fragmentation and peeling, and the number of particles larger than 0.2 μm on the wafer surface is significantly reduced, helping to lower the risk of particle contamination during semiconductor dry etching and PECVD equipment use.
[0044] Compared with existing technologies, this invention sets a lower limit temperature protection logic. When the substrate temperature is below 20°C, the system automatically reduces heat dissipation intensity and performs temperature correction. It also sets a low-temperature control lower limit based on the real-time dew point of the spraying environment to reduce the risk of condensation on the substrate surface. Condensation on the substrate surface can cause poor adhesion of yttrium oxide powder, abnormally increased coating porosity, and localized peeling defects. This zoned control strategy takes into account both high-temperature oxidation risks and low-temperature condensation risks, broadens the process window, and improves the process stability and yield of the spraying process. Attached Figure Description
[0045] To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0046] Figure 1 A schematic flowchart of a low-temperature preparation process for plasma spraying yttrium oxide onto a carbon-carbon substrate surface, as proposed in an embodiment of this application, is shown. Detailed Implementation
[0047] To further illustrate the technical means and effects of the present invention in achieving its intended purpose, the following detailed description of the specific implementation methods, structures, features, and effects of the present invention, in conjunction with the accompanying drawings and preferred embodiments, is provided below.
[0048] Implementation, for example Figure 1 As shown:
[0049] A low-temperature preparation process for plasma spraying yttrium oxide onto a carbon-carbon substrate includes the following steps: Step S1: The carbon-carbon composite substrate is pretreated to remove oil and surface impurities and to roughen and activate it. In step S1: 80# to 120# SiC abrasive is used for sandblasting to roughen the surface, with a surface roughness Ra = 2.0 to 6.0 μm; the substrate is then ultrasonically cleaned with an organic solvent, rinsed with deionized water, and finally dried at a low temperature of 100 to 120°C.
[0050] Finally, a carbon-carbon composite material carrier substrate that meets the requirements is obtained.
[0051] Step S2: Fix the pretreated carbon-carbon composite material carrier substrate to a spraying and cooling fixture system with real-time active temperature control. Specifically, active temperature control is achieved through a full-area bonding low-temperature spraying fixture system. This fixture system includes a back-side full-area bonding cooling fixture, a high-frequency temperature acquisition module, a variable frequency flow regulation module, and a temperature control computing terminal. The cooling fixture is bonded to the back of the carrier substrate without gaps, and a uniform cooling channel is provided inside the cooling fixture. The high-frequency temperature acquisition module is embedded in the side of the carbon-carbon composite material carrier substrate to acquire the body temperature of the carbon-carbon composite material carrier substrate. The sampling frequency of the high-frequency temperature acquisition module is ≥100Hz, and the response time of the temperature sensor used is ≤10ms (the temperature sensor uses a thin-film thermocouple). The high-frequency temperature acquisition module is electrically connected to the variable frequency flow regulation module and the temperature control computing terminal.
[0052] Step S3: A yttrium oxide protective ceramic coating is sprayed onto the surface of the carbon-carbon composite material carrier substrate using a plasma spraying process. During the entire plasma spraying process, continuous active temperature control is implemented on the carbon-carbon composite material carrier substrate to regulate and stabilize the substrate temperature within the low-temperature process range of 20℃ to 150℃.
[0053] The aforementioned 20℃ is a nominal low-temperature threshold. The actual lower limit for low-temperature control should be higher than the real-time dew point of the spraying environment, with an appropriate margin, to reduce the risk of condensation on the substrate surface. The oxidation behavior of carbon-carbon composite materials is affected by factors such as temperature, atmosphere, material composition, and exposure time. Controlling the substrate temperature rise helps reduce the risk of oxidation damage, but side-mounted body temperature measurement cannot directly represent the instantaneous temperature of the sprayed surface. Under the same incident droplet temperature, the higher the substrate temperature, the smaller the initial temperature difference between the droplet and the substrate. Controlling the substrate temperature rise can reduce the temperature drop and corresponding thermal expansion mismatch strain during the overall cooling stage after deposition. The total residual stress of the coating is also related to droplet solidification, temperature gradient, and structural constraints, and cannot be judged solely by the substrate temperature.
[0054] The system implements a zoned control strategy based on the real-time temperature of the substrate: when the temperature of the carbon-carbon composite substrate is between 20℃ and 150℃, it maintains constant temperature steady-state spraying; when the temperature of the carbon-carbon composite substrate exceeds the 150℃ over-temperature threshold, it initiates an over-temperature treatment strategy to suppress the temperature rise of the carbon-carbon composite substrate; when the temperature of the carbon-carbon composite substrate is below the 20℃ low-temperature threshold due to the initial temperature of the cooling medium being too low, or during non-continuous spraying conditions such as the spray gun sweeping gap or restarting after a shutdown, it initiates a low-temperature treatment strategy to reduce heat dissipation intensity and perform temperature correction.
[0055] Specifically: The over-temperature handling strategy is as follows: when the substrate temperature is greater than 150℃, the spraying cooling fixture system immediately and dynamically increases the flow rate of the cooling medium and reduces the heat input of the spray gun to lower the substrate temperature. After the temperature drops back to the range of 20℃ to 150℃, the steady-state spraying parameters are restored. The low-temperature handling strategy is as follows: when the substrate temperature is momentarily lower than 20℃, the system reduces the flow rate of the cooling medium to reduce the heat dissipation intensity and maintain the substrate temperature within the process window.
[0056] Specifically: Throughout the plasma spraying process, a combined feedforward compensation and PID feedback temperature control algorithm is used to regulate the temperature of the substrate measuring points. This combined feedforward compensation and PID feedback temperature control algorithm includes the following steps: Step A1: Establish a steady-state PID feedback model for the substrate temperature:
[0057] ;
[0058] Wherein, ΔQ is the cooling medium flow rate adjustment (control output, ΔQ positive indicates decreasing the cooling medium flow rate, ΔQ negative indicates increasing the cooling medium flow rate), and the substrate temperature is measured in real time. Acquired through a high-frequency temperature acquisition module. To preset the target low temperature, For real-time temperature deviation, = , , , These are the proportional, integral, and differential coefficients, respectively. The feedforward compensation amount (with the same dimensions as the control output) is the real-time heat input of the plasma flame after conversion by equivalent heat capacity and flow rate.
[0059] Step A2: Establish an empirical feedforward compensation model for the heat input of the spraying process, and dynamically calculate the real-time heat input feedforward compensation amount of the plasma flame after normalization by the substrate heated area, equivalent heat capacity, and flow rate equivalent. : Where P is the real-time spraying power, L is the spraying distance, v is the spray gun moving speed, and α is the process-related comprehensive calibration coefficient (including the heated area, the equivalent heat capacity of the substrate, and the flow equivalent conversion); the thermal shock is predicted in advance by the process-calibrated spraying heat input experience feedforward compensation model, and the cooling amount is compensated in advance to reduce the lag deviation of the substrate temperature control.
[0060] Step A3: Set the PID parameters, where the proportional coefficient Kp = 0.8~1.5, the integral coefficient Ki = 0.02~0.1, and the derivative coefficient Kd = 0.05~0.2; the control deviation of the substrate measuring point temperature relative to the target temperature shall not exceed ±3℃, that is, the temperature fluctuation of a single point on the substrate under the target temperature in each spraying stage shall not exceed ±3℃; the substrate temperature range given in the following examples is the target temperature range set for different spraying stages.
[0061] The carbon-carbon composite material carrier obtained through steps S1-S3 is used as a wafer carrier for semiconductor dry etching equipment or PECVD equipment.
[0062] In step S2, the back-side full-area bonding cooling fixture is cooled by either water cooling or air cooling. Specifically: when water cooling is used, the cooling water temperature is controlled at 10-30℃ and the flow rate is dynamically adjusted to 2-15L / min; when air cooling is used, the outlet air temperature is controlled at ≤25℃ and the air velocity is controlled at ≥15m / s, so as to achieve rapid and uniform heat dissipation with high heat flux.
[0063] In step S3, the plasma spraying parameters in the plasma process include: argon as the main gas 35-55 L / min, hydrogen as the auxiliary gas 3-8 L / min, spraying power 35-55 kW, spraying distance 80-120 mm, powder feeding rate 15-35 g / min, and spray gun moving speed 300-600 mm / s; yttrium oxide powder purity ≥99.9% and particle size 10-45 μm.
[0064] In this embodiment, before spraying the yttrium oxide protective ceramic coating, a SiC transition layer, a pure silicon transition layer, or a silicon-yttrium composite transition layer is pre-placed. The thickness of the transition layer is 10–40 μm. Specifically, a suitable transition layer composition is selected based on the thermal expansion properties of the carbon-carbon matrix and yttrium oxide to alleviate interfacial thermal expansion mismatch. The actual thermal expansion properties of each candidate transition layer need to be determined in conjunction with the composition and temperature range. At the same time, the transition layer can seal the open pores on the surface of the carbon-carbon matrix, preventing fluorine-chlorine plasma from penetrating the matrix along the pores, and improving the interfacial compatibility between the carbon matrix and the yttrium oxide ceramic, thereby enhancing the interfacial bonding strength of the coating. If the transition layer is too thin, it may lead to insufficient coverage; if it is too thick, it may change the stress state and heat transfer conditions. The specific impact depends on factors such as pore size, layer structure, thermal conductivity, and interfacial thermal resistance.
[0065] It also includes step S4, after the spraying is completed, low-temperature annealing at 120-180℃ is carried out, the temperature is held for 1-3 hours, and the furnace is naturally cooled to obtain a carbon-carbon composite material carrier plate with a yttrium oxide coating on the surface by plasma spraying.
[0066] To demonstrate the effectiveness of this method, multiple sets of examples and comparative examples are prepared in this embodiment, as follows: Uniform substrate: carbon-carbon composite carrier substrate from the same batch (density 1.75 g / cm³). 3 The coefficient of thermal expansion is 1.8 × 10⁻⁶. -6 / K); Yttrium oxide powder uniformity: purity 99.95%, particle size 10~45μm; transition layer uniformly selected SiC, thickness 25μm; performance test items and methods: interface bonding strength is tested by tensile method, coating crack rate and porosity are statistically analyzed by metallographic cross-sectional image method, plasma etching unit area weight loss is calculated by dividing the mass difference before and after etching by the etched area, particle contamination number is counted by wafer surface particle detector for particles larger than 0.2μm; spraying equipment: atmospheric plasma spraying APS; test environment: fluorine-based plasma etching environment (CF4 / O2), etching time 2h.
[0067] Example 1: A low-temperature preparation process for plasma spraying yttrium oxide onto the surface of a carbon-carbon substrate, step S1: 80# SiC sandblasting, Ra 3.2μm; ultrasonic cleaning + deionized water rinsing, drying at 110℃.
[0068] Step S2: Install the water-cooled bonding fixture on the back of the carrier plate, pre-embed a thin-film thermocouple, and use a temperature sensor with a response time ≤10ms and a sampling frequency of 100Hz; use a combination of feedforward compensation and PID feedback for temperature control, Kp=1.0, Ki=0.05, Kd=0.1; use cooling water at 18℃ with dynamic flow adjustment.
[0069] Step S3: First, spray a 25μm SiC transition layer; then spray a Y2O3 topcoat. The substrate temperature is kept stable at 60-120℃ throughout the spraying process. Spraying parameters: Ar 45L / min, H 25L / min, power 42kW, spraying distance 100mm, powder feeding rate 22g / min, and spray gun moving speed 450mm / s.
[0070] Step S4: Low-temperature annealing at 150℃, holding for 2 hours, then cooling in the furnace.
[0071] The test results are as follows: Coating interfacial bonding strength: 24.2 MPa; Coating crack rate: 0.4%; Coating porosity: 2.1%; Plasma etching weight loss: 0.28 mg / cm³. 2 Number of particles larger than 0.2μm (on wafer surface): 12.
[0072] Example 2: The process is the same as in Example 1, but the cooling method is changed to forced air cooling. By increasing the bonding heat dissipation area and air velocity, the heat dissipation is balanced with the heat input to the substrate, and the substrate temperature is stably maintained between 25 and 55°C throughout the spraying process. Specifically, the air cooling system outlet air temperature is ≤25°C, the air velocity is ≥15m / s, and the effective heat exchange area of the heat dissipation fins is approximately 0.12m². 2 The convective heat transfer coefficient is approximately 50–80 W / (m²). 2•K); It should be noted that 42kW is the total power of the plasma power supply. Under high-speed sweeping conditions, the actual net heat absorption per unit time of the thin substrate is only a small proportion of this. The heat capacity of the bonding fixture is used to mitigate the transient temperature rise, while the continuous heat dissipation capacity depends on the effective heat transfer area, heat transfer coefficient, and the temperature difference between the heat dissipation surface and the cooling air (control: the substrate rises to 265℃ without cooling in Comparative Example 1). The test results are as follows: Coating interface bonding strength: 22.7MPa; Coating crack rate: 0.6%; Coating porosity: 2.4%; Plasma etching weight loss: 0.31mg / cm³ 2 Number of particles larger than 0.2μm: 15.
[0073] Example 3: The process is the same as in Example 1, but the target temperature is increased, and the substrate temperature is 120-148℃ throughout the spraying process, which is close to the upper limit threshold.
[0074] The test results are as follows: Coating interfacial bonding strength: 21.5 MPa; Coating crack rate: 1.1%; Coating porosity: 2.6%; Plasma etching weight loss: 0.34 mg / cm³. 2 Number of particles larger than 0.2μm: 18.
[0075] Comparative Example 1: The substrate, pretreatment, SiC transition layer, spraying parameters, powder, and annealing process were completely consistent with Example 1; the back cooling fixture was removed, there was no active temperature control, and the substrate naturally heated up during the spraying process, with the highest substrate temperature measured at 265℃.
[0076] The test results are as follows: Coating interfacial bonding strength: 14.6 MPa; Coating crack rate: 7.3%; Coating porosity: 4.8%; Plasma etching weight loss: 0.79 mg / cm³. 2 Number of particles larger than 0.2μm: 56.
[0077] Comparative Example 2: The hardware is consistent with Example 1, and has certain temperature control measures, but continuous active temperature control is cancelled, and the substrate temperature naturally rises to 180-210℃ throughout the spraying process.
[0078] The test results are as follows: Coating interfacial bonding strength: 16.1 MPa; Coating crack rate: 5.8%; Coating porosity: 4.2%; Plasma etching weight loss: 0.68 mg / cm³ 2 Number of particles larger than 0.2μm: 47.
[0079] Comparative Example 3: Temperature control, spraying parameters, cooling, and annealing were the same as in Example 1; the SiC transition layer was removed, and a yttrium oxide coating was directly sprayed onto the substrate.
[0080] The test results are as follows: Coating interfacial bonding strength: 13.2 MPa; Coating crack rate: 8.5%; Coating porosity: 5.1%; Plasma etching weight loss: 0.87 mg / cm³.2 Number of particles larger than 0.2μm: 63.
[0081] Comparative Example 4: The remaining conditions are the same as in Example 1, but the SiC transition layer thickness is only 5 μm.
[0082] The test results are as follows: Coating interfacial bonding strength: 16.8 MPa; Coating crack rate: 4.9%; Coating porosity: 4.0%; Plasma etching weight loss: 0.62 mg / cm³ 2 Number of particles larger than 0.2μm: 41.
[0083] Comparative Example 5: The remaining conditions are the same as in Example 1, with a SiC transition layer thickness of 50 μm.
[0084] The test results are as follows: Coating interfacial bond strength: 17.4 MPa; Coating crack rate: 4.3%;
[0085] Coating porosity: 3.7%; Plasma etching weight loss: 0.54 mg / cm³ 2 Number of particles larger than 0.2μm: 35.
[0086] The conclusions are as follows: As can be seen from the comparison between Examples 1-3 and Comparative Examples 1-5, by adopting the feedforward compensation and PID feedback composite temperature control of the entire spraying process of the present invention, the carbon-carbon composite substrate is stably controlled within the range of 20℃ to 150℃. Combined with the zoned temperature control strategy, under the listed test conditions, the coating crack rate is reduced, the interface bonding strength is improved, and the weight loss per unit area of plasma etching and the number of wafer particles are reduced.
[0087] Compared with Comparative Example 2, under the conditions of 180-210℃ described in Comparative Example 2, even with cooling fixtures, the test results for bonding strength, crack rate, etc., were still inferior to those of Example 1.
[0088] Compared with Comparative Example 3, under the listed process conditions, the removal of the SiC transition layer resulted in a decrease in bonding strength, an increase in crack rate and particle number, indicating that the SiC transition layer helps to improve coating performance.
[0089] Comparing Comparative Examples 4 and 5, among the three thicknesses tested (5μm, 25μm, and 50μm), the 25μm transition layer showed better overall test results. These results indicate that the thickness of the transition layer affects the coating performance, but it is not sufficient to determine 10μm and 40μm as the applicable window boundaries.
[0090] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.
Claims
1. A low-temperature preparation process for plasma spraying yttrium oxide onto a carbon-carbon substrate surface, characterized in that, Includes the following steps: Step S1: Perform surface pretreatment on the carbon-carbon composite material carrier substrate to remove oil stains and surface impurities and complete roughening and activation; Step S2: Fix the pretreated carbon-carbon composite material carrier plate substrate to a spraying and cooling fixture system with real-time active temperature control; Step S3: Apply a yttrium oxide protective ceramic coating to the surface of the carbon-carbon composite substrate using a plasma spraying process; Throughout the plasma spraying process, continuous active temperature control is implemented on the carbon-carbon composite substrate to regulate and stabilize the substrate temperature within the low-temperature process range of 20℃ to 150℃. The system implements a zoned control strategy based on the real-time temperature of the substrate: When the temperature of the carbon-carbon composite material carrier substrate is in the range of 20℃ to 150℃, maintain constant temperature steady-state spraying. When the temperature of the carbon-carbon composite carrier substrate exceeds the 150℃ over-temperature threshold, an over-temperature treatment strategy is initiated to suppress the temperature rise of the carbon-carbon composite carrier substrate. When the temperature of the carbon-carbon composite substrate is too low at the initial temperature of the cooling medium, during the spray gun sweeping interval, during non-continuous spraying conditions of stopping and restarting, or below the low temperature threshold of 20°C, a low temperature treatment strategy is initiated to reduce heat dissipation intensity and perform temperature correction.
2. The method for preparing yttrium oxide by plasma spraying on a carbon-carbon carrier plate at low temperature according to claim 1, characterized in that, The active temperature control is achieved by a full-area bonding low-temperature spraying fixture system, which includes a back full-area bonding cooling fixture, a high-frequency temperature acquisition module, a variable frequency flow regulation module, and a temperature control computing terminal. The cooling fixture fits seamlessly with the back of the carrier plate, and the interior of the cooling fixture is equipped with uniform cooling channels. A high-frequency temperature acquisition module is embedded in the side of the carbon-carbon composite carrier plate substrate to collect the body temperature of the carbon-carbon composite carrier plate substrate. The sampling frequency is ≥100Hz and the response time of the temperature sensor used is ≤10ms. The high-frequency temperature acquisition module is electrically connected to the frequency conversion flow regulation module and the temperature control calculation terminal.
3. The method for preparing yttrium oxide by plasma spraying on a carbon-carbon carrier plate at low temperature according to claim 2, characterized in that, Throughout the plasma spraying process, a combined temperature control algorithm of feedforward compensation and PID feedback is used to regulate the temperature of the substrate measuring points. This combined temperature control algorithm includes the following steps: Step A1: Establish a steady-state PID feedback model for matrix temperature: ; Where ΔQ is the cooling medium flow rate adjustment amount, and the substrate temperature is measured in real time. Acquired through a high-frequency temperature acquisition module. To preset the target low temperature, For real-time temperature deviation, = , , , These are the proportional, integral, and differential coefficients, respectively. The feedforward compensation amount is the real-time heat input of the plasma flame after conversion by equivalent heat capacity and flow rate equivalent. Step A2: Establish an empirical feedforward compensation model for the heat input of the spraying process, and dynamically calculate the real-time heat input feedforward compensation amount of the plasma flame after normalization by the substrate heated area, equivalent heat capacity, and flow rate equivalent. : ; Where P is the real-time spraying power, L is the spraying distance, v is the spray gun moving speed, and α is the process-related comprehensive calibration coefficient; the thermal shock is predicted in advance by the process-calibrated spraying heat input experience feedforward compensation model, and the cooling amount is compensated in advance to reduce the lag deviation of substrate temperature control. Step A3: Set the PID parameters: proportional coefficient Kp = 0.8~1.5, integral coefficient Ki = 0.02~0.1, derivative coefficient Kd = 0.05~0.2; the control deviation of the substrate measuring point temperature relative to the target temperature shall not exceed ±3℃.
4. The method for preparing yttrium oxide by plasma spraying on a carbon-carbon carrier plate at low temperature according to claim 3, characterized in that, The over-temperature handling strategy is as follows: when the substrate temperature is greater than 150℃, the spraying cooling fixture system immediately and dynamically increases the flow rate of the cooling medium and reduces the heat input of the spray gun to lower the substrate temperature. After the temperature drops back to the range of 20℃ to 150℃, the steady-state spraying parameters are restored. The low-temperature handling strategy is as follows: when the substrate temperature is lower than 20℃ due to the initial temperature of the cooling medium being too low, the spray gun sweeping gap, or the instantaneous temperature drop after shutdown and restart, the system reduces the flow rate of the cooling medium to reduce the heat dissipation intensity and maintain the substrate temperature within the process window.
5. The method for preparing yttrium oxide by plasma spraying on a carbon-carbon substrate at low temperature according to claim 4, characterized in that, The back-side full-area bonding cooling fixture is cooled by either water cooling or air cooling. When water cooling is used, the cooling water temperature is controlled between 10 and 30°C, and the flow rate is dynamically adjusted to between 2 and 15 L / min. When air cooling is used: the outlet air temperature is controlled at ≤25℃ and the air speed is controlled at ≥15m / s to achieve rapid and uniform heat dissipation with high heat flux.
6. A low-temperature preparation process for plasma spraying yttrium oxide onto a carbon-carbon substrate surface according to any one of claims 1-5, characterized in that, In step S1: the surface is roughened by sandblasting with 80# to 120# SiC sand, with a surface roughness Ra of 2.0 to 6.0 μm; it is then ultrasonically cleaned with organic solvent, rinsed with deionized water, and finally dried at a low temperature of 100 to 120°C.
7. The method for preparing yttrium oxide by plasma spraying on a carbon-carbon carrier plate at low temperature according to claim 6, characterized in that, In step S3, the plasma spraying parameters in the plasma process include: argon as the main gas 35-55 L / min, hydrogen as the auxiliary gas 3-8 L / min, spraying power 35-55 kW, spraying distance 80-120 mm, powder feeding rate 15-35 g / min, and spray gun moving speed 300-600 mm / s; yttrium oxide powder purity ≥99.9% and particle size 10-45 μm.
8. The method for preparing yttrium oxide by plasma spraying on a carbon-carbon carrier plate at low temperature according to claim 7, characterized in that, Before spraying the yttrium oxide protective ceramic coating, a SiC transition layer, a pure silicon transition layer, or a silicon-yttrium composite transition layer is pre-placed, with a transition layer thickness of 10–40 μm.
9. The method for preparing yttrium oxide by plasma spraying on a carbon-carbon carrier plate at low temperature according to claim 8, characterized in that, It also includes step S4, after the spraying is completed, low-temperature annealing at 120-180℃ is carried out, the temperature is held for 1-3 hours, and then the furnace is naturally cooled.
10. The application of the carbon-carbon composite material carrier prepared by the method according to any one of claims 1, 2, 3, 4, 5, 7, 8 or 9 in wafer support in semiconductor dry etching equipment or PECVD equipment.
Citation Information
Patent Citations
Preparation method of yttrium oxide insulating coating applied to carbon fiber support plate in PECVD (Plasma Enhanced Chemical Vapor Deposition) cavity
CN120231032A
High-corrosion-resistance yttrium oxide coating for semiconductor equipment and preparation method of high-corrosion-resistance yttrium oxide coating
CN121293017A
Yttrium oxide gradient protective coating for graphite matrix as well as preparation method and application of yttrium oxide gradient protective coating
CN122128654A
Yttrium oxide-based coating material, composite support plate and preparation method of yttrium oxide-based coating material
CN122212218A