A low-remanence stainless steel pin bar, its preparation method and application

By employing a process of salt bath nitriding and acid leaching for demagnetization, combined with closed-loop detection control, a stainless steel pin bar with both high hardness and low remanence was prepared. This solves the problem of difficulty in achieving both hardness and remanence in existing technologies, making it suitable for precision equipment and weak magnetic environments.

CN123108472APending Publication Date: 2026-11-17杭州极弱磁场国家重大科技基础设施研究院
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611637050.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-22
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies cannot achieve both high hardness and low remanence on the surface of stainless steel pins, resulting in easy wear of the parts during friction, contact fatigue, and long-term use. Furthermore, ferromagnetic contamination introduced by oxide films or nitriding layers leads to increased remanence, failing to meet the requirements for weak magnetic environments.

Method used

The process route of salt bath nitriding combined with acid pickling and demagnetization is adopted. The magnetized surface layer formed during nitriding is removed by selective corrosion. The closed-loop control of surface hardness and remanence detection ensures that the remanence of the pin bar is less than 2nT at a hardness of 800 HV0.1.

Benefits of technology

This invention achieves a balance between high hardness and extremely low remanence in stainless steel pin bars, making them suitable for extremely weak magnetic field environments and precision equipment. It solves the problem of difficulty in achieving both hardness and remanence in traditional processes, and improves the wear resistance and service life of the parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108472A_ABST
    Figure CN123108472A_ABST
Patent Text Reader

Abstract

This invention relates to the field of surface strengthening and low-magnetic manufacturing technology for metallic materials, and discloses a low-remanence stainless steel pin bar, its preparation method, and its application. The preparation method includes the following steps: S1. Pretreatment of the low-magnetic stainless steel bar; the remanence of the low-magnetic stainless steel bar is <2nT when tested close to the surface, and <0.5nT when tested at a distance of 2cm from the surface; S2. First salt bath nitriding treatment; S3. First pickling, first rinsing, first neutralization, second rinsing, and first drying treatment; S4. Surface hardness and remanence testing of the pin bar workpiece. The salt bath nitriding treatment in this invention is not primarily aimed at forming an oxide protective layer, but rather at removing the magnetized surface layer generated after nitriding through pickling, and preventing secondary corrosion or secondary magnetic contamination caused by residual acid through the first rinsing, neutralization, second rinsing, and drying treatments. This process route is more suitable for the manufacture of extremely low-remanence stainless steel pin bars.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of surface strengthening and low-magnetic manufacturing technology of metallic materials, specifically to a low-remanence stainless steel pin rod, its preparation method, and its application. Background Technology

[0002] Low-magnetic stainless steel pins are widely used in precision equipment, low-magnetic structural components, special connection mechanisms, marine engineering equipment, medical devices, and instrument systems highly sensitive to magnetic environments. In these applications, stainless steel pins not only need high surface hardness but also extremely low remanence to avoid interference with surrounding precision sensors, magnetic measuring equipment, navigation systems, or weak magnetic environments. Generally, the raw material for these low-magnetic stainless steel pins (i.e., the rod-shaped raw material used to manufacture the pins) is required to have a remanence in the nT range, meaning a remanence of <2nT when tested close to the surface and <0.5nT when tested 2cm from the surface.

[0003] Low-magnetic austenitic stainless steel pins typically possess low magnetic permeability and low remanence. However, due to their relatively low surface hardness, pins manufactured from them are prone to wear, scratches, and premature failure under friction, contact fatigue, localized high stress, or long-term reciprocating mating conditions. Therefore, engineering applications often require improving the hardness and wear resistance of the stainless steel pin material. To address these issues, existing technologies improve the surface hardness of austenitic stainless steel pins by forming or retaining oxide films and nitrided layers with corrosion-resistant and oil-retaining properties. However, these oxide films or surface structures often contain free ferromagnetic contamination layers or locally magnetized structures, which can significantly increase the remanence of the workpiece, thus failing to meet the requirements for use in weak magnetic environments.

[0004] Therefore, there is an urgent need to develop a process that can form an effective hardening layer on the surface of low-magnetic austenitic stainless steel pins, so that the pins can maintain low remanence at the nT level even when the surface hardness is not less than 800 HV0.1. Summary of the Invention

[0005] This invention provides a low-remanence stainless steel pin bar, its preparation method, and its application, to solve the problem that existing technologies cannot simultaneously achieve high surface hardness and low remanence.

[0006] In a first aspect, the present invention provides a method for preparing a low-remanence stainless steel pin, comprising the following steps: S1. Obtain low-magnetic stainless steel bars, pre-treat the low-magnetic stainless steel bars to obtain pin bar blanks; The remanence of the low-magnetic stainless steel bar when tested close to the surface is <2nT, and the remanence at a distance of 2cm from the surface is <0.5nT. S2. The pin bar blank is subjected to a first salt bath nitriding treatment to obtain a first nitrided part; S3. The nitrided part is subjected to a first pickling, a first rinsing, a first neutralization, a second rinsing, and a first drying treatment to obtain the first pin bar workpiece; S4. Perform surface hardness and remanence testing on the first pin workpiece: When the test results simultaneously meet the requirements of surface hardness ≥ 800 HV0.1, remanence < 2nT when tested close to the surface and remanence < 0.5nT when tested 2cm from the surface, the preparation is complete and the stainless steel pin bar is obtained. If the surface hardness does not meet the requirements, perform steps S5 and S6 and then retest. If the surface remanence does not meet the conditions, perform step S5' and then retest. This process is repeated until the above conditions are met; S5. The first pin bar workpiece is subjected to a second salt bath nitriding treatment to obtain a second nitrided part; S6. The nitrided part is subjected to a second pickling, a third rinsing, a second neutralization, a fourth rinsing, and a second drying treatment to obtain the second pin bar workpiece; S5'. The first pin bar workpiece is subjected to a third pickling, a fifth rinsing, a third neutralization, a sixth rinsing, and a third drying process to obtain the third pin bar workpiece.

[0007] In one optional implementation, the residual magnetism detection employs a triaxial magnetic field measuring device with a residual magnetism of <2nT. The residual magnetism at close range is the maximum residual magnetism value measured when the sensor is 0cm away from the surface of the workpiece, and the residual magnetism at a distance of 2cm is the maximum residual magnetism value measured when the sensor is 2cm away from the surface of the workpiece. The maximum residual magnetism value refers to the residual magnetism detection result of the workpiece being measured, which is obtained by randomly selecting at least 6 detection positions on the surface of the workpiece.

[0008] In one optional embodiment, the method for preparing the low-remanence stainless steel pin bar satisfies at least one of the following conditions: (1) The low magnetic stainless steel bar in S1 includes austenitic stainless steel; (2) Before the first salt bath nitriding treatment and the second salt bath nitriding treatment, there are also separate washing and drying steps; the purpose of washing is to remove residual oil, particles, polishing wax and other contaminants on the surface of the pin; the purpose of drying is to keep the surface of the pin clean and dry so as to avoid surface residues affecting the subsequent salt bath nitriding effect; (3) The nitride salts used in the first salt bath nitriding treatment and the second salt bath nitriding treatment are independently composed of a mixed salt consisting of alkali metal cyanate and carbonate; the alkali metal cyanate provides an active nitrogen source, and the carbonate is used to adjust the reactivity and stability of the salt bath system. The active nitrogen atoms in the alkali metal cyanate diffuse to the surface of the pin bar blank during the heat preservation process, forming a nitriding hardened layer on the surface of the pin bar blank, thereby significantly improving the surface hardness and wear resistance of the pin bar blank. (4) The temperature of the first salt bath nitriding treatment in S2 is 400-600℃ and the holding time is 60-90min; the temperature and time of the salt bath nitriding are controlled within this range, which can ensure the formation of an effective hardened layer and avoid excessive generation of surface magnetized phase. (5) The temperature of the second salt bath nitriding treatment in S5 is 400-600℃ and the holding time is 20-40min.

[0009] In one optional embodiment, the method for preparing the low-remanence stainless steel pin bar satisfies at least one of the following conditions: (1) The austenitic stainless steel, by mass percentage, comprises the following components: C 0.01%-0.08%, Si 1.0%-1.5%, Mn 7.0%-8.0%, P 0.008%-0.05%, S 0.005%-0.04%, Cr 21.0%-24.0%, Ni 10.0%-15.0%, Mo 3.1%-4.0%, N 0.4%-0.6%, with the balance being Fe and unavoidable impurity components; (2) The alkali metal cyanate includes at least one of sodium cyanate and potassium cyanate; (3) The carbonate includes at least one of sodium carbonate and potassium carbonate; (4) The mass ratio of the alkali metal cyanate to the carbonate is (50-70): (30-50); the mass ratio of the alkali metal cyanate to the carbonate in the salt bath nitriding is controlled within this range, which can ensure the formation of an effective hardened layer and avoid excessive generation of surface magnetized phase.

[0010] In one optional embodiment, the method for preparing the low-remanence stainless steel pin bar satisfies at least one of the following conditions: (1) The reagents used for the first pickling, the second pickling and the third pickling are each independently a nitric acid-hydrofluoric acid compound pickling solution; (2) The first pickling time in S3 is 8-60 min; (3) The temperatures for the first drying, the second drying, and the third drying are each 60-100℃, and the time is 10-30 min. (4) The second pickling time in S6 is 10-30 min; (5) The third pickling time in S5' is 10-20 min.

[0011] In one optional embodiment, the first pickling time in S3 is 20-40 minutes.

[0012] In one optional embodiment, the nitric acid-hydrofluoric acid compound pickling solution comprises, by mass percentage, 10%-50% nitric acid, 5%-10% hydrofluoric acid, and 40%-85% deionized water.

[0013] In one optional embodiment, the method for preparing the low-remanence stainless steel pin bar satisfies at least one of the following conditions: (1) The washing media used in S2 and S5 each independently include one or more of anhydrous ethanol, isopropanol, and acetone; (2) The washing methods in S2 and S5 are independently ultrasonic washing; the ultrasonic washing is used to remove oil and particulate residues, ensure the surface of the pin is clean, and prevent the uniform penetration of active nitrogen atoms from being affected. (3) The drying temperatures in S2 and S5 are 60-100℃ and the drying time is 10-30min, respectively.

[0014] In one optional embodiment, the ultrasonic washing time is 30-50 minutes.

[0015] In one optional embodiment, the method for preparing the low-remanence stainless steel pin bar satisfies at least one of the following conditions: (1) The rinsing media used in the first rinsing, second rinsing, third rinsing, fourth rinsing, fifth rinsing and sixth rinsing are each independently one or more of deionized water, distilled water and ultrapure water; (2) The neutralizing agents used in the first neutralization treatment, the second neutralization treatment and the third neutralization treatment each independently include one or more of sodium carbonate, sodium bicarbonate and sodium hydroxide; (3) The time for the first rinse, the third rinse and the fifth rinse is 1-5 min each; (4) The second, fourth and sixth rinsings are performed independently until the pH of the residual liquid on the surface of the nitrided part is 6-7; (5) The soaking time for the first neutralization treatment, the second neutralization treatment and the third neutralization treatment is 1-5 min, respectively.

[0016] In one optional embodiment, the neutralizing agent has a mass fraction of 0.5-3 wt.%.

[0017] In one optional embodiment, the pretreatment step in S1 includes cutting, roughing, finishing and mechanical polishing. The surface of the low-magnetic stainless steel bar after mechanical polishing is flat and has fewer defects, which can reduce surface defects such as tool marks, microcracks and local pits, which is conducive to the uniform diffusion of active nitrogen atoms in the subsequent salt bath nitriding process and improves the uniformity and density of the nitrided layer.

[0018] In one alternative implementation, the cutting device includes one or more of water jet cutting, laser cutting, sawing, and wire cutting.

[0019] In one alternative implementation, the roughing step includes turning.

[0020] In one alternative implementation, the finishing step includes grinding.

[0021] In one alternative implementation, the roughing and finishing tools each independently include non-magnetic tools.

[0022] In one optional embodiment, the non-magnetic cutting tool includes one or more of ceramic cutting tools, diamond cutting tools, cubic boron nitride cutting tools, and non-magnetic tungsten carbide cutting tools.

[0023] In one optional embodiment, the surface roughness (Ra) of the blank after mechanical polishing is <0.1 μm. Controlling the surface roughness to Ra <0.1 μm through mechanical polishing can reduce tool marks, microcracks, and local defects, and improve the uniformity and density of the subsequent salt bath nitriding layer.

[0024] Secondly, the present invention provides a low remanent stainless steel pin rod, which is prepared according to the preparation method described above.

[0025] Thirdly, the present invention provides an application of the aforementioned low-remanence stainless steel pin in precision equipment, low-magnetic structural components, special connection mechanisms, marine engineering equipment, medical devices, or instrument systems that are highly sensitive to magnetic environments.

[0026] The technical solution of this invention has the following advantages: 1. The method for preparing a low-remanence stainless steel pin bar provided by the present invention includes the following steps: S1. Obtaining a low-magnetic stainless steel bar, pre-treating the low-magnetic stainless steel bar to obtain a pin bar blank; the remanence of the low-magnetic stainless steel bar is <2nT when tested close to the surface, and <0.5nT when tested at a distance of 2cm from the surface; S2. Performing a first salt bath nitriding treatment on the pin bar blank to obtain a first nitrided part; S3. Performing a first pickling, a first rinsing, a first neutralization, a second rinsing, and a first drying treatment on the nitrided part to obtain a first pin bar workpiece; S4. Performing surface hardness and remanence detection on the first pin bar workpiece: when the detection results simultaneously meet the surface hardness ≥800... When the remanence at close range is <2nT and the remanence at a distance of 2cm from the surface is <0.5nT, the preparation is complete, and the stainless steel pin is obtained. If the surface hardness does not meet the requirements, steps S5 and S6 are performed and the test is repeated. If the surface remanence does not meet the requirements, step S5' is performed and the test is repeated. This process is repeated until the above conditions are met. S5. The first pin workpiece is subjected to a second salt bath nitriding treatment to obtain a second nitrided part. S6. The nitrided part is subjected to a second pickling, a third rinsing, a second neutralization, a fourth rinsing, and a second drying treatment to obtain a second pin workpiece. S5'. The first pin workpiece is subjected to a third pickling, a fifth rinsing, a third neutralization, a sixth rinsing, and a third drying treatment to obtain a third pin workpiece.

[0027] In S1 of this invention, the remanence of the low-magnetic stainless steel bars tested close to the surface is <2nT, and the remanence at a distance of 2cm from the surface is <0.5nT. This limitation does not simply rely on the low magnetic properties of the base material, but rather establishes a low-magnetic benchmark for the manufacturing process. On one hand, this limitation excludes bars that have been contaminated or magnetized by ferromagnetism during feeding, transportation, processing, or storage, preventing the introduction of substandard base material into the subsequent nitriding process. On the other hand, this low-magnetic benchmark allows for a clear determination of whether salt bath nitriding has introduced a magnetized surface layer, and whether the pickling treatment has effectively removed this magnetized surface layer. Therefore, the low-magnetic detection in S1 is a prerequisite for achieving final nT-level remanence control and process closed-loop judgment.

[0028] The present invention provides a method for preparing low-remanence stainless steel pins, proposing a process route of salt bath nitriding followed by acid pickling for demagnetization. The key step of acid pickling has a dual function: on the one hand, it can effectively remove free iron, ferromagnetic deposits, and embedded metal impurities from the surface of the workpiece; on the other hand, it can significantly reduce the remanence of the stainless steel pin by selectively corroding and peeling off the surface oxide layer, reaction layer, and free ferromagnetic contamination layer formed during nitriding.

[0029] The salt bath nitriding treatment in the preparation method of this invention is not primarily aimed at forming an oxide protective layer. Instead, it removes the magnetized surface layer generated after nitriding by acid washing, and prevents secondary corrosion or secondary magnetic contamination caused by residual acid through rinsing, neutralization, rerinsing and drying. This process route is more suitable for the manufacture of stainless steel pins with extremely low remanence.

[0030] This invention sets up surface hardness and nT-level remanence detection steps, and performs supplementary nitriding and pickling and retesting when the hardness is unqualified, and supplementary pickling and retesting when the remanence is unqualified, forming a closed-loop control mechanism of "nitriding - pickling - hardness and remanence detection - supplementary nitriding and / or pickling - retesting", which can improve the stability of the surface hardness and extremely low remanence index of stainless steel pin bars in the batch production process.

[0031] The method for preparing low-remanence stainless steel pins provided by this invention enables the produced low-remanence stainless steel pins to have a surface hardness of not less than 800 HV0.1 while meeting the requirements of remanence less than 2nT when tested close to the surface and less than 0.5nT when tested at a distance of 2cm from the surface. This solves the problem of difficulty in achieving both high hardness and low remanence in traditional surface strengthening processes. It allows the parts to obtain high surface hardness and extremely low remanence while maintaining the low magnetic properties of the base material. It is suitable for manufacturing low-remanence stainless steel pin parts that have high requirements for wear resistance, service life and compatibility with weak magnetic environments. It can be applied to extremely weak magnetic field environments, precision equipment, low magnetic structural parts and instrument systems sensitive to magnetic interference. Attached Figure Description

[0032] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0033] Figure 1 This is a photograph of the nitrided part before pickling treatment in Embodiment 1 of the present invention; Figure 2 This is a photograph of the pin rod workpiece obtained after pickling treatment in Embodiment 1 of the present invention. Detailed Implementation

[0034] The following embodiments are provided to better understand the present invention, but the following embodiments do not constitute a limitation on the content and scope of protection of the present invention. Any product that is the same as or similar to the present invention, derived by any person under the guidance of the present invention or by combining the features of the present invention with other prior art, falls within the scope of protection of the present invention.

[0035] Unless otherwise specified, all experimental steps or conditions in the examples were performed according to conventional experimental procedures and conditions in the art. Reagents or instruments whose manufacturers are not specified are all commercially available products.

[0036] Example 1 This embodiment provides a method for preparing a low-remanence stainless steel pin, comprising the following steps: S1. Obtain low-magnetic stainless steel bars and pre-treat them. The pre-treatment steps are as follows: Cut the 20mm diameter bars into 120mm long samples using wire cutting. Then, remove the oxide scale from the surface of the bars using a CNC lathe and non-magnetic tools (ceramic cutters and ceramic fixtures). Grind away the deep scratches formed during the turning process, and then perform mechanical polishing to make the surface roughness Ra of the working surface of the low-magnetic stainless steel bars 0.08μm, thus obtaining the pin bar blank. Among them, the matrix structure of the low magnetic austenitic stainless steel bar is mainly stable austenite. The remanence of the low magnetic stainless steel bar is 1.0 nT when tested close to the surface and 0.2 nT when tested 2 cm from the surface. The material composition is shown in Table 1, with the balance being Fe and unavoidable impurity components.

[0037] Table 1 Material composition (mass ratio, %)

[0038] S2. Immerse the pin blank from S1 in anhydrous ethanol and clean it with an ultrasonic device for 40 minutes. Then, take out the pin and dry it with hot air at 60°C for 30 minutes. Place the dried pin blank in a salt bath nitriding furnace for salt bath nitriding treatment, which contains a mixed salt of potassium cyanate and potassium carbonate (the mass ratio of potassium cyanate to potassium carbonate is 70:30). Hold the solution at 520°C for 80 minutes to obtain the nitrided part.

[0039] S3. After removing residual salts from the nitrided parts in S2, immerse them in a nitric acid-hydrofluoric acid compound pickling solution (comprising 30% nitric acid, 6% hydrofluoric acid, and 64% deionized water by mass percentage) for pickling for 40 minutes. After pickling, rinse the nitrided parts with deionized water for 1 minute, then neutralize them with a 2 wt.% sodium bicarbonate solution for 5 minutes. Rinse again with deionized water to bring the pH of the residual solution on the surface of the nitrided parts to 6.8. Finally, dry them with hot air at 60°C for 30 minutes to obtain the pin rod workpiece. Figure 1 These are actual photos of the nitrided parts before pickling. Figure 2These are photographs of the pin workpieces after pickling. It can be seen that the surface color of the pin workpieces after pickling is significantly lighter and more uniform, indicating that the nitric acid-hydrofluoric acid composite pickling solution can remove the surface oxide layer, reaction layer, and other surface substances that may lead to increased remanence formed after nitriding. Combined with the following remanence test results, it can be seen that the remanence of the pin workpieces after pickling has recovered from the high remanence state after nitriding to a low remanence state in the nT range.

[0040] S4. Surface hardness and remanence of the pin bar workpiece from S3 were tested. Remanence values ​​were obtained from the workpiece surface and at a distance of 2 cm from the surface using a triaxial magnetic field measuring device with a remanence <2 nT. Six locations on the sample were randomly selected for remanence testing, and the results are shown in Table 2. After salt bath nitriding, the remanence of the pin bar blank increased significantly. After pickling, the remanence at close range was <2 nT, and the remanence at 2 cm from the surface was <0.5 nT. Surface microhardness was tested at three selected locations on the sample, and the results are shown in Table 3. The test showed that after salt bath nitriding and pickling, the surface hardness remained not less than 800 HV0.1. The test results indicate that this process satisfies the requirement of high hardness while also providing the sample with extremely low remanence.

[0041] Table 2. Remanence test results of samples before nitriding, after nitriding, and after acid washing in Example 1.

[0042] Table 3. Microhardness test results of the samples in Example 1 before nitriding, after nitriding, and after pickling.

[0043] Example 2 This embodiment provides a method for preparing a low-remanence stainless steel pin, comprising the following steps: S1. Obtain low-magnetic stainless steel bars and pre-treat them. The pre-treatment steps are as follows: Cut the 20mm diameter bars into 120mm long samples using wire cutting. Then, remove the oxide scale from the surface of the bars using a CNC lathe and non-magnetic tools (diamond tools and ceramic fixtures). Grind the deep scratches formed during the turning process to remove the oxide scale. Finally, perform mechanical polishing to make the surface roughness Ra of the working surface of the low-magnetic stainless steel bar 0.08μm, thus obtaining the pin bar blank. Among them, the matrix structure of the low magnetic austenitic stainless steel bar is mainly stable austenite. The remanence of the low magnetic stainless steel bar is 0.5 nT when tested close to the surface and 0 nT when tested 2 cm from the surface. The material composition is shown in Table 4, with the balance being Fe and unavoidable impurity components.

[0044] Table 4 Material composition (mass ratio, %)

[0045] S2. Immerse the pin blank from S1 in acetone and clean it with an ultrasonic device for 30 minutes. Then, take out the pin and dry it with hot air at 100°C for 10 minutes. Place the dried pin blank in a salt bath nitriding furnace for salt bath nitriding treatment, which contains a mixed salt of potassium cyanate and potassium carbonate (the mass ratio of potassium cyanate to potassium carbonate is 60:40). Keep it at 600°C for 60 minutes to obtain the nitrided part.

[0046] S3. After removing residual salts from the nitrided parts in S2, immerse them in a nitric acid-hydrofluoric acid compound pickling solution (comprising 50% nitric acid, 10% hydrofluoric acid, and 40% deionized water by mass percentage) for pickling for 20 minutes. After pickling, rinse the nitrided parts with distilled water for 5 minutes, then neutralize them with a 0.5 wt.% sodium carbonate solution for 5 minutes. Rinse again with distilled water to bring the pH of the residual solution on the surface of the nitrided parts to 6.7. Finally, dry them with hot air at 100°C for 10 minutes to obtain the pin rod workpiece.

[0047] S4. Surface hardness and remanence of the pin bar workpiece from S3 were tested. Remanence values ​​were obtained from the workpiece surface and at a distance of 2 cm using a triaxial magnetic field measuring device with a remanence <2 nT. Six locations on the sample were randomly selected for remanence testing. The results showed a maximum remanence of 1.4 nT when tested close to the surface and 0.2 nT at a distance of 2 cm. Surface microhardness was then tested at three selected locations on the sample. The surface hardness of the stainless steel pin bar was 836 HV0.1, 829 HV0.1, and 851 HV0.1, respectively.

[0048] Example 3 This embodiment provides a method for preparing a low-remanence stainless steel pin, comprising the following steps: S1. Obtain low-magnetic stainless steel bars and pre-treat them. The pre-treatment steps are as follows: Cut the 20mm diameter bars into 120mm long samples using wire cutting. Then, remove the oxide scale from the surface of the bars using a CNC lathe and non-magnetic tools (cubic boron nitride tools and ceramic fixtures). Grind the deep scratches formed during the turning process to remove the oxide scale. Finally, perform mechanical polishing to make the surface roughness Ra of the working surface of the low-magnetic stainless steel bar 0.08μm, thus obtaining the pin bar blank. Among them, the matrix structure of the low magnetic austenitic stainless steel bar is mainly stable austenite. The remanence of the low magnetic stainless steel bar was 1.4 nT when tested close to the surface and 0.2 nT when tested 2 cm from the surface. The material composition is shown in Table 5.

[0049] Table 5 Material composition (mass ratio, %)

[0050] S2. Immerse the pin blank from S1 in isopropanol and clean it with an ultrasonic device for 50 minutes. Then, take out the pin and dry it with hot air at 80°C for 20 minutes. Place the dried pin blank in a salt bath nitriding furnace for salt bath nitriding treatment, which contains a mixed salt of sodium cyanate and sodium carbonate (the mass ratio of sodium cyanate to sodium carbonate is 50:50). Keep it at 430°C for 90 minutes to obtain the nitrided part.

[0051] S3. After removing residual salts from the nitrided parts in S2, immerse them in a nitric acid-hydrofluoric acid compound pickling solution (comprising 10% nitric acid, 5% hydrofluoric acid, and 85% deionized water by mass percentage) for pickling for 40 minutes. After pickling, rinse the nitrided parts with deionized water for 3 minutes, then neutralize them with a 3 wt.% sodium hydroxide solution for 1 minute. Rinse again with deionized water to bring the pH of the residual solution on the surface of the nitrided parts to 6.6. Finally, dry them with hot air at 80°C for 20 minutes to obtain the pin rod workpiece.

[0052] S4. Surface hardness and remanence of the pin bar workpiece in S3 were tested. Remanence values ​​were obtained from the workpiece surface and at a distance of 2 cm using a triaxial magnetic field measuring device with a remanence <2 nT. Six locations on the sample were randomly selected for remanence testing. The results showed a maximum remanence of 1.6 nT when tested close to the surface and 0.3 nT at a distance of 2 cm. Surface microhardness was then tested at three selected locations on the sample. The surface hardness of the stainless steel pin bar was 882 HV0.1, 845 HV0.1, and 861 HV0.1, respectively.

[0053] Example 4 This embodiment provides a method for preparing a low-remanence stainless steel pin, comprising the following steps: S1. Obtain low-magnetic stainless steel bars and pre-treat them. The pre-treatment steps are as follows: Cut the 20mm diameter bars into 120mm long samples using wire cutting. Then, remove the oxide scale from the surface of the bars using a CNC lathe and non-magnetic tools (non-magnetic tungsten carbide tools and ceramic fixtures). Grind the deep scratches formed during the turning process to remove the oxide scale. Finally, perform mechanical polishing to make the surface roughness Ra of the working surface of the low-magnetic stainless steel bar 0.08μm, thus obtaining the pin bar blank. Among them, the matrix structure of the low magnetic austenitic stainless steel bar is mainly stable austenite. The remanence of the low magnetic stainless steel bar was 1.1 nT when tested close to the surface and 0.1 nT when tested 2 cm from the surface. The material composition is shown in Table 6.

[0054] Table 6 Material composition (mass ratio, %)

[0055] S2. Immerse the pin blank from S1 in anhydrous ethanol and clean it with an ultrasonic device for 40 minutes. Then, take out the pin and dry it with hot air at 60°C for 20 minutes. Place the dried pin blank in a salt bath nitriding furnace for salt bath nitriding treatment, which contains a mixed salt of potassium cyanate and potassium carbonate (the mass ratio of potassium cyanate to potassium carbonate is 70:30). Keep it at 520°C for 80 minutes to obtain the nitrided part.

[0056] S3. After removing residual salts from the nitrided parts in S2, immerse them in a nitric acid-hydrofluoric acid compound pickling solution (by mass percentage, including 30% nitric acid, 6% hydrofluoric acid, and 64% deionized water) for pickling treatment for 60 minutes. After pickling, rinse the nitrided parts with deionized water for 5 minutes, then neutralize them with a 2 wt.% sodium bicarbonate solution for 3 minutes. Rinse again with deionized water to make the pH of the residual solution on the surface of the nitrided parts 6.9. Finally, dry them at 60°C for 20 minutes to obtain the pin rod workpiece.

[0057] S4. Surface hardness and remanence of the pin bar workpiece from S3 are tested. Remanence values ​​at the workpiece surface and 2cm from the surface are obtained using a triaxial magnetic field measuring device with a remanence <2nT. Six locations on the sample are randomly selected for remanence testing. Due to excessive pickling, the finished product's remanence test results are as follows: maximum remanence 1.2nT close to the surface, and maximum remanence 0.2nT at 2cm from the surface. Surface microhardness is then tested at three selected locations on the sample. The results show that the surface hardness of the pin bar workpiece is 659 HV0.1, 617 HV0.1, and 602 HV0.1, respectively, indicating that the surface microhardness test is unqualified.

[0058] S5. The pin bar workpiece that fails the surface hardness test in S4 is immersed in anhydrous ethanol again and cleaned with ultrasonic equipment for 40 minutes. Then, the pin bar is taken out and dried with hot air at 60°C for 20 minutes. After drying, the pin bar is placed in a salt bath nitriding furnace for salt bath nitriding treatment, which contains a mixed salt of potassium cyanate and potassium carbonate (the mass ratio of potassium cyanate to potassium carbonate is 70:30). The temperature is maintained at 520°C for 30 minutes to obtain the nitrided part.

[0059] S6. After removing residual salts from the nitrided parts in S5, immerse them in a nitric acid-hydrofluoric acid compound pickling solution (by mass percentage, including 30% nitric acid, 6% hydrofluoric acid, and 64% deionized water) for pickling for 20 minutes. After pickling, rinse with deionized water for 5 minutes, then neutralize with a 2 wt.% sodium bicarbonate solution for 5 minutes. Rinse again with deionized water to bring the pH of the residual solution to 6.9. Finally, dry with hot air at 60°C for 20 minutes to obtain the pin rod workpiece.

[0060] S7. Surface hardness and remanence of the pin bar workpiece in S6 were tested. Remanence values ​​were obtained from the workpiece surface and at a distance of 2 cm using a triaxial magnetic field measuring device with a remanence <2 nT. Six locations on the sample were randomly selected for remanence testing. Results: Maximum remanence was 1.4 nT when tested close to the surface, and 0.2 nT at a distance of 2 cm. Surface microhardness was then tested at three selected locations on the sample. Results: The surface hardness of the stainless steel pin bar was 903 HV0.1, 884 HV0.1, and 915 HV0.1, respectively.

[0061] Example 5 This embodiment provides a method for preparing a low-remanence stainless steel pin, comprising the following steps: S1. Obtain low-magnetic stainless steel bars and pre-treat them. The pre-treatment steps are as follows: Cut the 20mm diameter bars into 120mm long samples using wire cutting. Then, remove the oxide scale from the surface of the bars using a CNC lathe and non-magnetic tools (non-magnetic tungsten carbide tools and ceramic fixtures). Grind the deep scratches formed during the turning process to remove the oxide scale. Finally, perform mechanical polishing to make the surface roughness Ra of the working surface of the low-magnetic stainless steel bar 0.08μm, thus obtaining the pin bar blank. Among them, the matrix structure of the low magnetic austenitic stainless steel bar is mainly stable austenite. The remanence of the low magnetic stainless steel bar was 1.1 nT when tested close to the surface and 0.1 nT when tested 2 cm from the surface. The material composition is shown in Table 7.

[0062] Table 7 Material composition (mass ratio, %)

[0063] S2. Immerse the pin blank from S1 in anhydrous ethanol and clean it with an ultrasonic device for 40 minutes. Then, take out the pin and dry it with hot air at 60°C for 20 minutes. Place the dried pin blank in a salt bath nitriding furnace for salt bath nitriding treatment, which contains a mixed salt of potassium cyanate and potassium carbonate (the mass ratio of potassium cyanate to potassium carbonate is 70:30). Keep it at 400°C for 80 minutes to obtain the nitrided part.

[0064] S3. After removing residual salts from the nitrided parts in S2, immerse them in a nitric acid-hydrofluoric acid compound pickling solution (by mass percentage, including 30% nitric acid, 6% hydrofluoric acid, and 64% deionized water) for pickling for 8 minutes. After pickling, rinse the nitrided parts with deionized water for 5 minutes, then neutralize them with a 2 wt.% sodium bicarbonate solution for 5 minutes. Rinse again with deionized water to bring the pH of the residual solution on the surface of the nitrided parts to 6.8. Finally, dry them with hot air at 60°C for 20 minutes to obtain the pin rod workpiece.

[0065] S4. Surface hardness and remanence of the pin bar workpiece from S3 are tested. Remanence values ​​are obtained from the workpiece surface and at a distance of 2 cm using a triaxial magnetic field measuring device with a remanence <2 nT. Six locations on the sample are randomly selected for remanence testing. Due to incomplete pickling, the remanence test results are as follows: maximum remanence close to the surface is 952.6 nT, and maximum remanence at a distance of 2 cm is 241.7 nT. Surface microhardness tests are performed at three selected locations on the sample: the surface hardness of the pin bar workpiece is 1209 HV0.1, 1154 HV0.1, and 1227 HV0.1 respectively, indicating that the remanence test is unqualified.

[0066] S5'. The defective pin bar workpiece obtained in S4 is immersed again in a nitric acid-hydrofluoric acid compound pickling solution (by mass percentage, including 30% nitric acid, 6% hydrofluoric acid, and 64% deionized water) for pickling treatment for 15 minutes. After pickling, the pin bar is rinsed with deionized water for 5 minutes, and then neutralized with a 2 wt.% sodium bicarbonate solution for 5 minutes. It is then rinsed again with deionized water to make the pH value of the residual liquid on the pin bar surface 6.8. Finally, it is dried with hot air at 60°C for 20 minutes to obtain the pin bar workpiece.

[0067] S6'. Surface hardness and remanence of the pin bar workpiece in S5' are tested. Remanence values ​​are obtained from the workpiece surface and at a distance of 2 cm using a triaxial magnetic field measuring device with a remanence <2 nT. Remanence tests are performed at six randomly selected locations on the sample. The results show a maximum remanence of 1.5 nT when tested close to the surface and a maximum remanence of 0.3 nT at a distance of 2 cm. Surface microhardness is then tested at three randomly selected locations on the sample. The surface hardness of the stainless steel pin bar is 827 HV0.1, 841 HV0.1, and 818 HV0.1, respectively.

[0068] Comparative Example 1 This comparative example provides a method for preparing a stainless steel pin bar. The only difference from Example 1 is that after salt bath nitriding, step S3 is not performed, and step S4 is performed directly for remanence and hardness testing. The remaining steps are the same as in Example 1.

[0069] Test results: After nitriding, the surface hardness was 1396 HV0.1 at position 1, 1436 HV0.1 at position 2, and 1423 HV0.1 at position 3, indicating that nitriding significantly improves surface hardness. However, the maximum remanence measured close to the surface was 2348.5 nT, and the maximum remanence measured 2 cm from the surface was 566.2 nT, clearly failing to meet the low remanence requirement. This comparative example illustrates that while salt bath nitriding alone can improve hardness, it leads to a significant increase in remanence, failing to meet the requirements for extremely low remanence applications.

[0070] Comparative Example 2 This comparative example provides a method for preparing a stainless steel pin bar. The only difference from Example 1 is that steps S2 and S3 are not performed, while the remaining steps are the same as in Example 1. The pin bar blank obtained after pretreatment of the low-magnetic stainless steel bar in step S1 is tested.

[0071] Test results: The maximum remanence near the surface was 1.0 nT, and the maximum remanence at 2 cm from the surface was 0.2 nT, meeting the low remanence requirement; however, the surface hardness was only 217 HV0.1 at position 1, 209 HV0.1 at position 2, and 221 HV0.1 at position 3, significantly lower than 800 HV0.1. This comparative example illustrates that although the low-magnetic base material meets the low remanence requirement, its surface hardness is insufficient and cannot meet the service requirements of high-hardness pins.

[0072] Comparative Example 3 This comparative example provides a method for preparing a stainless steel pin rod, which differs from Example 1 only in that the raw material does not meet the requirements of a remanence of less than 2nT when tested close to the surface and less than 0.5nT when tested at a distance of 2cm from the surface of the low-magnetic stainless steel rod. The remanence of the low-magnetic stainless steel rod is 20.6nT when tested close to the surface and 4.1nT when tested at a distance of 2cm from the surface. The material composition is shown in Table 8, with the balance being Fe and unavoidable impurity components.

[0073] Table 8 Material composition (mass ratio, %)

[0074] Results: The maximum remanence measured close to the surface was 28.2 nT, and the maximum remanence measured 2 cm from the surface was 5.8 nT, which does not meet the low remanence requirement. The surface hardness was only 849 HV0.1 at position 1, 806 HV0.1 at position 2, and 825 HV0.1 at position 3, while the microhardness met the requirement of being higher than 800 HV0.1. This comparative example illustrates that the low-magnetic base material does not meet the low remanence requirement. Although the surface hardness of the specimen meets the requirement after nitriding, it does not meet the service requirements of the extremely low remanence pin.

[0075] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.

Claims

1. A method for preparing a low-remanence stainless steel pin, characterized in that, Includes the following steps: S1. Obtain low-magnetic stainless steel bars, pre-treat the low-magnetic stainless steel bars to obtain pin bar blanks; The remanence of the low-magnetic stainless steel bar when tested close to the surface is <2nT, and the remanence at a distance of 2cm from the surface is <0.5nT. S2. The pin bar blank is subjected to a first salt bath nitriding treatment to obtain a first nitrided part; S3. The nitrided part is subjected to a first pickling, a first rinsing, a first neutralization, a second rinsing, and a first drying treatment to obtain the first pin bar workpiece; S4. Perform surface hardness and remanence testing on the first pin workpiece: When the test results simultaneously meet the requirements of surface hardness ≥ 800 HV0.1, remanence < 2nT when tested close to the surface and remanence < 0.5nT when tested 2cm from the surface, the preparation is complete and the stainless steel pin bar is obtained. If the surface hardness does not meet the requirements, perform steps S5 and S6 and then retest. If the surface remanence does not meet the conditions, perform step S5' and then retest. This process is repeated until the above conditions are met; S5. The first pin bar workpiece is subjected to a second salt bath nitriding treatment to obtain a second nitrided part; S6. The nitrided part is subjected to a second pickling, a third rinsing, a second neutralization, a fourth rinsing, and a second drying treatment to obtain the second pin bar workpiece; S5'. The first pin bar workpiece is subjected to a third pickling, a fifth rinsing, a third neutralization, a sixth rinsing, and a third drying process to obtain the third pin bar workpiece.

2. The method for preparing a low-remanence stainless steel pin according to claim 1, characterized in that, At least one of the following conditions must be met: (1) The low magnetic stainless steel bar in S1 includes austenitic stainless steel; (2) Before the first salt bath nitriding treatment and the second salt bath nitriding treatment, there are also separate washing and drying steps; (3) The nitriding salts used in the first salt bath nitriding treatment and the second salt bath nitriding treatment each independently include a mixed salt composed of alkali metal cyanate and carbonate; (4) The temperature of the first salt bath nitriding treatment in S2 is 400-600℃, and the holding time is 60-90min; (5) The temperature of the second salt bath nitriding treatment in S5 is 400-600℃ and the holding time is 20-40min.

3. The method for preparing a low-remanence stainless steel pin rod according to claim 2, characterized in that, At least one of the following conditions must be met: (1) The austenitic stainless steel, by mass percentage, comprises the following components: C 0.01%-0.08%, Si 1.0%-1.5%, Mn 7.0%-8.0%, P 0.008%-0.05%, S 0.005%-0.04%, Cr 21.0%-24.0%, Ni 10.0%-15.0%, Mo 3.1%-4.0%, N 0.4%-0.6%, with the balance being Fe and unavoidable impurity components; (2) The alkali metal cyanate includes at least one of sodium cyanate and potassium cyanate; (3) The carbonate includes at least one of sodium carbonate and potassium carbonate; (4) The mass ratio of the alkali metal cyanate to the carbonate is (50-70): (30-50).

4. The method for preparing a low-remanence stainless steel pin according to claim 1, characterized in that, At least one of the following conditions must be met: (1) The reagents used for the first pickling, the second pickling and the third pickling are each independently a nitric acid-hydrofluoric acid compound pickling solution; (2) The first pickling time in S3 is 8-60 min; (3) The temperatures for the first drying, the second drying, and the third drying are each 60-100℃, and the time is 10-30 min. (4) The second pickling time in S6 is 10-30 min; (5) The third pickling time in S5' is 10-20 min.

5. The method for preparing a low-remanence stainless steel pin according to claim 4, characterized in that, The first pickling time in S3 is 20-40 minutes.

6. The method for preparing a low-remanence stainless steel pin according to claim 4, characterized in that, The nitric acid-hydrofluoric acid compound pickling solution comprises, by mass percentage, 10%-50% nitric acid, 5%-10% hydrofluoric acid, and 40%-85% deionized water.

7. The method for preparing a low-remanence stainless steel pin according to claim 2, characterized in that, At least one of the following conditions must be met: (1) The washing media used in S2 and S5 each independently include one or more of anhydrous ethanol, isopropanol, and acetone; (2) The washing methods in S2 and S5 each independently include ultrasonic washing; (3) The drying temperatures in S2 and S5 are 60-100℃ and the drying time is 10-30min, respectively.

8. The method for preparing a low-remanence stainless steel pin according to claim 1, characterized in that, At least one of the following conditions must be met: (1) The rinsing media used in the first rinsing, second rinsing, third rinsing, fourth rinsing, fifth rinsing and sixth rinsing are each independently one or more of deionized water, distilled water and ultrapure water; (2) The neutralizing agents used in the first neutralization treatment, the second neutralization treatment and the third neutralization treatment each independently include one or more of sodium carbonate, sodium bicarbonate and sodium hydroxide; (3) The time for the first rinse, the third rinse and the fifth rinse is 1-5 min each; (4) The second, fourth and sixth rinsings are performed independently until the pH of the residual liquid on the surface of the nitrided part is 6-7; (5) The soaking time for the first neutralization treatment, the second neutralization treatment and the third neutralization treatment is 1-5 min, respectively.

9. A low-remanence stainless steel pin bar, characterized in that, Prepared by the preparation method according to any one of claims 1-8.

10. The application of the low remanent magnet stainless steel pin bar of claim 9 in precision equipment, low magnetic structural components, special connection mechanisms, marine engineering equipment, medical devices, or instrument systems that are highly sensitive to magnetic environments.