A method for solving the problem of dirty and dark film on TOPCon battery PL

By pre-regulating the pressure and gas flow to optimize the SiO2 content during the preparation of the tunneling layer and polycrystalline phosphorus-doped layer by PECVD, the problem of PL contamination and dark film caused by insufficient reaction at the bottom of the carrier plate was solved, and the A-grade rate and appearance quality of the battery were improved.

CN123108535APending Publication Date: 2026-11-17弘元新材料(徐州)有限公司 +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611278723.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

During the preparation of doped tunneling layers and polycrystalline phosphorus-doped layers using tubular PECVD, the SiO2 reaction at the bottom of the carrier plate is insufficient, leading to localized tunneling during subsequent high-temperature processes, resulting in dirty PL sheets and affecting battery quality.

Method used

In the process of preparing tunnel layers and polycrystalline phosphorus-doped layers by PECVD, the SiO2 content in the tubular PECVD preparation space is increased by pre-adjusting the pressure and gas flow to optimize the process, including process adjustments in steps S1 to S6.

Benefits of technology

It effectively reduced the generation of dirty and dark spots in PL, improved the A-grade rate and appearance quality of batteries, and increased the product yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108535A_ABST
    Figure CN123108535A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of solar cell fabrication technology, specifically relating to a method for solving the problem of dirty and dark PL wafers in TOPCon solar cells. The method involves introducing the silicon wafer into a furnace tube, heating it to 430°C, and then closing the tube for leak testing. After the temperature stabilizes at 430°C, nitrogen gas is introduced to purge the furnace tube. After nitrogen purging, pre-regulating the gas flow is performed to increase the SiO2 content in the fabrication space. Then, 13000W RF power is used for the first tunneling deposition layer. Next, 8000W RF power is used for the second tunneling deposition layer. Then, 15000W RF power is used, with RF on for 6ms and off for 60ms, and 3100 sccm of silane, 800 sccm of phosphine, and 10000 sccm of hydrogen gas are used for an 800-second phosphorus-doped layer deposition. Finally, after the film deposition is complete, 40000 sccm of nitrogen gas is introduced for backpressure purging. After backpressure purging, the wafer is removed from the furnace tube. This invention improves the SiO2 content in the tubular PECVD preparation space by pre-regulating the pressure and venting before the oxide layer is deposited, thereby increasing the SiO2 content in the preparation space and effectively reducing the generation of PL dirt films, thus improving the appearance quality and yield of the products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of solar cell fabrication technology, specifically relating to a method for reducing dirt and dark spots on the PL film of TOPCon cells. Background Technology

[0002] The full Chinese name for tubular PECVD is tubular plasma-enhanced chemical vapor deposition. This is a key thin-film preparation technology widely used in the manufacture of solar cells, especially TOPCon cells. Tubular PECVD is an important method for preparing tunneling oxide layers and polycrystalline phosphorus-doped layers. Specifically, it uses microwaves or radio frequency to locally form a plasma containing the atoms that make up the thin film. The plasma is highly chemically reactive and readily reacts, depositing the desired thin film on the substrate.

[0003] The process involves depositing a through-hole oxide layer. During the preparation of this layer, a difference in SiO2 concentration occurs between the substrate's support area and the normal area. This difference leads to localized penetration during subsequent high-temperature crystallization processes, resulting in localized contamination (PL) areas that reduce the A-grade yield of the production line. "PL" in PL stands for Photoluminescence. Photoluminescence (PL) is a non-destructive testing technique commonly used for quality control of solar cells. It involves irradiating the silicon wafer with light of a specific wavelength to excite it to emit infrared light, and then capturing the intensity of the light using a camera. Areas with stronger light emission indicate higher minority carrier lifetime and fewer defects; while areas with weaker light emission or dark areas / stains indicate the presence of defects or contamination.

[0004] In existing technical solutions, the mainstream methods currently used in the industry involve lowering the crystallization annealing temperature in subsequent high-temperature processes to reduce the risk of internal expansion, or optimizing the tunneling layer process time. While these solutions can reduce the output of PL contaminated films, they limit the window for improving efficiency and reducing costs in the later high-temperature crystallization process. Therefore, this invention provides a method for solving the problem of PL contaminated films in TOPCon batteries. In the process of preparing the tunneling layer and polycrystalline phosphorus-doped layer using PECVD, the tunneling process is optimized, and the bottom tunneling process is pre-regulated with pressure adjustment and gas venting to increase the SiO2 content within the tubular PECVD preparation space. Summary of the Invention

[0005] The purpose of this invention is to provide a method for solving the problem of dirty dark spots in PL imaging of TOPCon batteries. This method can solve the problem that "in the process of preparing doped tunneling layers and polycrystalline phosphorus-doped layers by tubular PECVD, the conventional process is to continuously prepare the tunneling layer and the polycrystalline phosphorus-doped oxide layer. This leads to insufficient local SiO2 reaction at the bottom of the carrier during oxide layer preparation, which causes local high-temperature propagation and penetration in the subsequent crystallization high-temperature preparation process, resulting in the generation of local dirty dark spots in PL imaging".

[0006] The specific technical solution adopted by this invention is as follows: A method for solving the problem of dirty and dark films in TOPCon batteries involves optimizing the tunneling process during the PECVD preparation of the tunneling layer and polycrystalline phosphorus-doped layer. This includes pre-regulating the pressure and venting the bottom tunneling process to increase the SiO2 content within the tubular PECVD preparation space. The method comprises the following steps: Step S1: Place the silicon wafer into the furnace tube, heat it to 430°C, and then close the tube to check for leaks; Step S2: After the temperature stabilizes at 430℃, purge the furnace tubes with 10000 sccm of nitrogen gas. Step S3: After the nitrogen purging is completed, pre-pressure purging is performed for 40 seconds to increase the SiO2 content in the preparation space. Then, 13000W radio frequency power is used, with radio frequency on for 20ms and off for 220ms, nitrous oxide flow rate of 10000sccm, and pressure of 1800motorr for the first layer of tunneling deposition in 30 seconds. Step S4: After the first tunneling layer is deposited, the second tunneling layer is deposited for 70 seconds using 8000W radio frequency power, RF on for 20ms, RF off for 250ms, nitrous oxide flow rate of 9000sccm, and pressure of 1800motorr. Step S5: After the tunneling layer deposition is completed, use 15000W RF power, RF on for 6ms, off for 60ms, 3100sccm of silane, 800sccm of phosphine, and 10000sccm of hydrogen to perform 800 seconds of phosphorus doping layer deposition. Step S6: After the film deposition is completed, nitrogen gas at 40000 sccm is introduced for back pressure and purging; after the back pressure purging is completed, the tube is removed and the wafer is taken out.

[0007] The technical effects achieved by this invention are as follows: This invention improves the SiO2 content in the tubular PECVD preparation space by pre-regulating the pressure and venting before the oxide layer is prepared and deposited, thereby effectively reducing the generation of PL dirty films and increasing the yield of A-grade films.

[0008] This invention successfully improves the problem of local darkening of polycrystalline silicon (PL) layers in the polycrystalline silicon deposition process of photovoltaic cells, especially TOPCon cells, thereby improving the appearance quality and yield of the products and providing strong support for the efficient production of photovoltaic cells. Attached Figure Description

[0009] Figure 1 This is a flowchart of a method for solving the problem of dirty and dark film on the TOPCon battery PL according to the present invention. Detailed Implementation

[0010] To make the objectives and advantages of this invention clearer, the invention will be specifically described below with reference to embodiments. It should be understood that the following text is merely used to describe one or more specific embodiments of the invention and does not strictly limit the scope of protection specifically claimed by the invention.

[0011] like Figure 1 As shown, a method for solving the problem of dirty dark film in TOPCon battery PL is to optimize the tunneling process during the preparation of tunneling layer and polycrystalline phosphorus-doped layer by PECVD, and to pre-regulate the pressure and ventilate the bottom tunneling process to increase the SiO2 content in the tubular PECVD preparation space. Specific Implementation Example 1: The tunneling oxide layer and polycrystalline phosphorus-doped layer of TOPCon cells were prepared using a tubular PECVD equipment. The silicon wafer was an N-type monocrystalline silicon wafer with a size of 182mm×182mm.

[0012] The specific process steps are as follows: S1: Place the silicon wafer on the carrier plate, send it into the furnace tube, heat it to 430℃, close the tube to check for leaks, and ensure that the reaction chamber is airtight.

[0013] S2: After the temperature stabilizes at 430℃, 10000 sccm of nitrogen is introduced to purge the furnace tubes for 60 seconds to remove residual gas.

[0014] S3: After purging, pre-pressure venting is performed for 40 seconds, with only nitrous oxide and nitrogen introduced and no radio frequency (RF) applied, to increase the initial proportion of SiO2 precursor in the preparation space; then RF is started with 13000W RF power, pulse mode, RF on for 20ms and off for 220ms, nitrous oxide flow rate of 10000sccm, and pressure of 1800mTorr to deposit the first tunnel oxide layer for 30 seconds.

[0015] S4: After the first layer deposition is completed, switch to the second layer deposition conditions: RF power 8000W, pulse mode, on for 20ms, off for 250ms, nitrous oxide flow rate 9000sccm, pressure 1800mTorr, deposition time 70s, forming a tunneling oxide layer with a total thickness of about 1.5nm.

[0016] S5: After the tunneling layer is deposited, a polycrystalline phosphorus-doped layer is deposited: RF power 15000W, pulse mode, 6ms on, 60ms off, silane flow rate 3100sccm, phosphine flow rate 800sccm, hydrogen flow rate 10000sccm, deposition time 800s, to obtain an in-situ doped polycrystalline silicon layer with a thickness of about 120nm.

[0017] S6: After deposition, nitrogen gas at 40,000 sccm is introduced for backpressure and purging, and then the tube is removed and the plate is taken out.

[0018] The silicon wafers were then subjected to subsequent crystallization high-temperature annealing, cleaning, passivation, and metallization processes to form TOPCon cells. The subsequent crystallization high-temperature annealing temperature was 920℃ for 30 minutes, and PL and EL tests were performed.

[0019] Comparative Example 1: Traditional process, without pre-pressure regulation ventilation; The only difference between Comparative Example 1 and Example 1 is that the pre-pressure regulation and venting for 40 seconds in step S3 is omitted; that is, the deposition of the first tunneling layer begins directly after nitrogen purging. All other process parameters are exactly the same as in Example 1.

[0020] Comparative Example 2: Traditional process + reduced crystallization annealing temperature; Comparative Example 2, based on the traditional process without pre-pressure regulation and ventilation, reduced the subsequent high-temperature crystallization annealing temperature from 920℃ to 880℃, while maintaining the annealing time at 30 minutes. All other parameters remained the same as in Comparative Example 1.

[0021] Each group of schemes produced 5000 silicon wafers, and the proportion of locally contaminated dark wafers in the PL test (i.e., PL defect rate) and the cell A-grade rate were statistically analyzed. Efficiency ≥23.8% was classified as A-grade, and the average conversion efficiency was measured. The results are shown in Table 1.

[0022] Table 1: Performance Comparison Table

[0023] From the comparison data in Table 1 above, we can see that: Comparative Example 1, using traditional processes and high-temperature crystallization, showed a PL (partially precipitated) black film ratio as high as 2.85%. This was due to insufficient SiO2 reaction at the bottom of the carrier plate during the tunnel oxide layer deposition process, resulting in a thinner local oxide layer. During subsequent high-temperature annealing at 920℃, excessive local diffusion and penetration of phosphorus occurred, forming PL black films. Although the average efficiency of 23.85% was acceptable, the A-grade rate of 92.4% was low.

[0024] In Comparative Example 2, lowering the crystallization temperature by reducing the annealing temperature to 880°C effectively suppressed the internal diffusion of phosphorus, reducing the proportion of dirty polycrystalline silicon (PL) wafers to 1.12% and increasing the grade A rate to 95.1%. However, due to insufficient annealing temperature, the crystallization quality and passivation effect of the polycrystalline silicon layer decreased, resulting in an average conversion efficiency of 23.72%, 0.4 percentage points lower than in Example 1. This indicates that while simply lowering the temperature improved the appearance, it sacrificed the window for improving battery efficiency.

[0025] Example 1, the present invention: While maintaining the optimal crystallization temperature of 920℃, by adding pre-pressure regulation and ventilation for 40 seconds before the deposition of the tunneling layer, the concentration of SiO2 precursor in the reaction chamber reaches a high and uniform distribution before plasma ignition, thereby improving the density and thickness uniformity of the oxide layer in areas difficult for airflow to reach, such as the bottom of the carrier plate. Ultimately, the proportion of contaminated PL films was reduced to 0.36%, the A-grade rate reached 97.8%, and the average conversion efficiency reached 24.12%, significantly better than the two comparative examples.

[0026] This invention addresses a common pain point in the industry: during the tubular PECVD fabrication of the tunneling oxide layer for TOPCon batteries, the difference in SiO2 concentration between the bottom of the carrier plate and the normal area leads to localized tunneling and PL contamination / darkening issues. Existing technologies, such as lowering the crystallization temperature or increasing the tunneling layer process time, have significant drawbacks: the former sacrifices efficiency gains, while the latter reduces production capacity and does not fundamentally solve the problem. This invention, for the first time, proposes a simple and effective method—"pre-pressure regulation and aeration"—to improve the initial uniformity of SiO2 within the reaction chamber from the source, fundamentally solving the problem of incomplete localized reactions.

[0027] Existing technologies focus on parameter adjustments during the deposition process, such as increasing RF power, extending deposition time, or compromising with subsequent annealing processes. When faced with the problem of thin SiO2 at the bottom of the substrate, those skilled in the art typically wouldn't consider simply introducing gas for pre-pressure regulation before plasma ignition, as this step doesn't involve a deposition reaction and is easily considered "meaningless" or a "waste of process time." Through extensive experiments, the inventors have discovered that pre-gasping for 40 seconds significantly improves the uniformity of oxygen source distribution in the initial atmosphere, thereby forming a more uniform oxide layer at the moment of ignition.

[0028] This invention requires no modification to equipment hardware; it can be implemented simply by adjusting the process formulation, resulting in extremely low implementation costs. It can be widely applied to existing tubular PECVD production lines. For a TOPCon battery factory with an annual capacity of 10GW, every 1 percentage point increase in the A-grade rate can bring direct economic benefits of tens of millions of yuan.

[0029] The above description is merely a preferred embodiment of the present invention. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention. Structures, devices, and operating methods not specifically described or explained in this invention are implemented according to conventional methods in the art unless otherwise specified or limited.

Claims

1. A method for solving the PL dirty negative of TOPCon cells, characterized in that: In the process of preparing tunneling layers and polycrystalline phosphorus-doped layers by PECVD, the tunneling process is optimized, and the bottom tunneling process is pre-pressurized and ventilated to increase the SiO2 content in the tubular PECVD preparation space.

2. The method for solving the PL dirty negative of the TOPCon cell according to claim 1, characterized in that: Specifically, the following steps are included: Step S1: Insert the silicon wafer into the furnace tube, heat it to 430℃, and then close the tube to check for leaks; Step S2: After the temperature stabilizes at 430℃, nitrogen gas is introduced to purge the furnace tubes; Step S3: After the nitrogen purging is completed, pre-pressure purging is performed to increase the SiO2 content in the preparation space, and then 13000W radio frequency power is used to perform the first layer of tunnel deposition. Step S4: After the first tunneling layer is deposited, the second tunneling layer is deposited using 8000W RF power. Step S5: After the tunneling layer deposition is completed, use 15000W RF power, RF on for 6ms, off for 60ms, 3100sccm of silane, 800sccm of phosphine, and 10000sccm of hydrogen to deposit a phosphorus-doped layer for 800 seconds. Step S6: After the film deposition is completed, nitrogen gas at 40000 sccm is introduced for back pressure and purging; after the back pressure purging is completed, the tube is removed and the wafer is taken out.

3. The method of claim 2, wherein the method is characterized by: In step S2, nitrogen gas at 10000 sccm is introduced to purge the furnace tubes.

4. The method of claim 3, wherein the method is characterized by: In step S3, the pre-pressure regulation ventilation time is 40 seconds.

5. The method of claim 4, wherein the method is characterized by: In step S3, the process conditions for the first layer of tunnel deposition are: RF power 13000W, RF on 20ms, RF off 220ms, nitrous oxide flow rate 10000sccm, pressure 1800mTorr, and deposition time 30 seconds.

6. The method of claim 5, wherein the method is characterized by: In step S4, the process conditions for the second tunnel deposition are: RF power 8000W, RF on 20ms, RF off 250ms, nitrous oxide flow rate 9000sccm, pressure 1800mTorr, and deposition time 70 seconds.