A PCB gold bonding agent, its preparation method and application method
By constructing a molecular bridging structure with multiple branched anthracene derivatives and other components on the gold surface of the PCB, the problem of insufficient bonding strength caused by the chemical inertness of the gold surface is solved, achieving highly reliable bonding performance and resistance to damp heat, making it suitable for high-end PCB packaging.
Patent Information
- Application Number
- CN202611640637.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-22
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies struggle to overcome the chemical inertness of the PCB gold surface at the molecular level, making it impossible to construct a complete chemical bridging layer between the gold surface and the epoxy encapsulation material. This results in insufficient bonding strength, leading to problems such as insufficient bond pull, debonding, poor soldering, and bond cracking. Furthermore, the gold surface easily adsorbs contaminants, affecting packaging yield and reliability.
A PCB gold-side bonding agent composed of multi-branched anthracene derivatives, multi-branched isocyanate silanes, multi-branched cycloboroxane derivatives, multi-branched ether ester compounds, and multi-branched bridging derivatives is used to form a gold-π coordination anchor with the gold surface through an electron-rich large π conjugated system, thereby constructing a complete molecular bridging structure and improving interfacial bonding strength and thermal stability.
It significantly improves wire bonding strength and interfacial shear strength, with no damage to the gold plating, is suitable for ultra-fine lines, meets the high reliability requirements of high-density and ultra-thin plating, has excellent resistance to damp heat aging, and is suitable for automotive and 5G high-reliability packaging.
Smart Images

Figure CN123108546A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of printed circuit board packaging technology, specifically to a PCB gold bonding agent and its preparation and application methods. Background Technology
[0002] With the rapid development of consumer electronics, new energy vehicles, 5G communications, and artificial intelligence chips, printed circuit boards (PCBs) are gradually iterating towards high density, ultra-fine lines, ultra-thin plating, high reliability, and long lifespan. Currently, the line width and spacing of high-end PCBs have generally decreased to below 35μm, placing stringent requirements on the bonding performance of gold-plated packaging. As the core process for electrical interconnection between PCBs and chips, the bonding strength, consistency, and temperature and humidity resistance stability of PCBs directly determine the packaging yield and lifespan of electronic products.
[0003] The gold surface of PCBs mainly employs three mainstream processes: chemical immersion gold, electroplating soft gold, and chemical nickel-palladium-gold plating. The gold layer thickness is generally controlled between 0.05 and 0.3 μm. However, the plating layer suffers from inherent micropore defects, uneven surface crystallization, a loose nickel-gold diffusion layer, and low surface energy. During subsequent ultrasonic thermoforming bonding of gold and aluminum wires, defects such as insufficient bond pull, bond debonding, poor soldering, and bond cracking are highly likely to occur. Furthermore, the gold surface easily absorbs moisture, oil, and sulfides and oxides from the air during storage and process transfer, further reducing the bonding activity and leading to a decrease in batch packaging yield.
[0004] In traditional processes, the industry mainly relies on physical treatments such as post-gold surface polishing, plasma cleaning, and high-temperature activation to improve bonding performance. However, these processes can only remove surface contaminants and cannot repair micropores in the gold layer or optimize the surface crystallization state. Furthermore, high-temperature and high-energy treatments can easily cause burns and oxidation of the ultra-thin gold layer, damaging the flatness of the gold surface and resulting in extremely poor adaptability to high-end PCBs with ultra-fine lines. At the same time, existing commercial gold surface treatment agents are mostly single degreasing and antioxidant sealing agents, which can only achieve surface protection and cannot improve the interfacial bonding force between the gold wire and the gold surface at the molecular level, making it difficult to meet the long-term stability requirements of high-density, ultra-fine lines, and high-reliability packaging.
[0005] The main solutions and their shortcomings in existing technologies for addressing low adhesion of PCB gold surfaces are as follows: Physical cleaning methods (such as patent document CN115119414A) disclose processes for removing contaminants from the gold surface using sodium carbonate solution cleaning, ultrasonic water washing, and deionized water washing. However, this method only physically removes contaminants and does not change the chemical inertness of the gold surface, resulting in limited improvement in chemical bonding strength. Surface treatment methods containing thiol compounds (such as patent document CN116607136B) disclose water-based bonding agents composed of thiol molecules, nitrogen-containing heterocyclic molecules, and coupling agents to treat copper surfaces. However, these methods are designed for copper surfaces, and the nitrogen-containing heterocyclic chelating of copper ions is not applicable to gold surfaces, making it difficult to form an effective chemical bridge on the gold surface. The physical roughening method uses plasma treatment or mechanical polishing to increase the roughness of the gold surface, but it is easy to damage the ultra-thin gold layer, expose the palladium or nickel layer and cause corrosion, and it is difficult to guarantee the uniformity over a large area. The aminosilane adhesive method (such as patent document CN102412166A) discloses 3-aminopropylsilanetriol as an adhesive, but its silanol is difficult to bond with the chemically inert gold surface, and the gold surface does not have metal hydroxyl groups that can be condensed, which has an essential limitation on the applicability to the gold surface. The sulfur-containing silane direct addition method directly adds sulfur-containing silane coupling agent to epoxy resin, but the silane is unevenly dispersed and its migration is uncontrollable. The hydrolysis condensation and epoxy curing compete with each other, making it difficult to form a uniform and complete chemical bridging layer.
[0006] In summary, current technologies lack a bonding agent that can overcome the chemical inertness of the gold surface at the molecular level and construct a complete chemical bridging layer between the gold surface and the epoxy encapsulation material. Summary of the Invention
[0007] The purpose of this invention is to overcome the shortcomings of the prior art and provide a PCB gold surface bonding agent, its preparation method and application method, so as to improve the adhesion of the packaging material to the PCB gold surface, avoid delamination and peeling of the chip bonding interface and wire bonding area under temperature cycling, damp heat aging and mechanical bending conditions, thereby ensuring the long-term reliability of the packaged device.
[0008] To achieve the above objectives, the technical solution adopted by the present invention is as follows: A PCB gold-side bonding agent, by mass percentage, comprises the following components: 1.0%–2.0% of a multi-branched anthracene derivative; 0.2%–1.0% of a multi-branched isocyanate silane; 0.2%–1.0% of a multi-branched cycloboroxane derivative; 1.0%–2.0% of a multi-branched ether ester compound; 0.2%–1.0% of a multi-branched bridging derivative; and the balance being water.
[0009] Further, the multibranched anthracene derivative is selected from one or more of 1,4,5,8-tetramethoxyanthracene (CAS No.: 60767-87-1), 2,3,6,7-tetramethoxy-9,10-dimethylanthracene (CAS No.: 13985154), and 2,6-di-tert-butyl-9,10-dimethoxyanthracene (CAS No.: 22433290).
[0010] Further, the multi-branched isocyanate silane is selected from one or more of 3-isocyanatepropyltriethoxysilane (CAS No.: 24801885), 3-isocyanatepropyltrimethoxysilane (CAS No.: 15396-00-6), and tris[3(trimethoxysilyl)propyl]isocyanurate (CAS No.: 26115708).
[0011] Furthermore, the multi-branched cyclic triboroxane derivative is selected from one or more of 2,4,6-tritert-butylcyclotriboroxane (CAS No.: 13155005), 2,4,6-tri-n-butylcyclotriboroxane (CAS No.: 7359980), and 2,4,6-triphenylcyclotriboroxane (CAS No.: 3262893).
[0012] Further, the multi-branched ether ester compound is selected from one or more of dipropylene glycol methyl ether acetate (CAS No.: 88917220), 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate (CAS No.: 25265774), and dipropylene glycol diacetate (CAS No.: 58125943).
[0013] Furthermore, the multi-branched bridging derivative is selected from one or more of bis(3-triethoxysilylpropyl)amine (CAS No.: 13497-18-2), 3-[tris(trimethylsiloxane)silyl]propylamine (CAS No.: 25357-81-7), and bis(3-trimethoxysilylpropyl)amine (CAS No.: 82985-35-1).
[0014] Furthermore, the water is deionized water or tap water.
[0015] Preferably, the PCB gold bonding agent comprises the following components by weight percentage: 1,4,5,8-Tetramethoxyanthracene 1.5%; 3. Propyltriethoxysilane isocyanate 0.5%; 0.5% of 2,4,6-tert-butylcyclotriboroxane; Dipropylene glycol methyl ether acetate 1.5%; 0.5% bis(3-triethoxysilylpropyl)amine; The remainder is water.
[0016] The multi-branched anthracene derivative of this invention serves as the gold-surface anchoring host. It achieves effective anchoring of the bonding agent on the inert gold surface through a gold-π coordination interaction with the gold surface via an electron-rich large π-conjugated system. Its large-volume branches can regulate the thickness of the self-assembled film layer, preventing excessive film thickness from interfering with wire bonding. The active groups on the multi-branched isocyanate silane can add to the active sites of the anthracene ring, covalently incorporating π-adsorbed anthracene into the silicon-oxygen network, enhancing the bonding strength. The multi-branched cyclotriboroxane derivative participates in silicon-oxygen crosslinking, buffering interfacial thermal stress and improving the system's thermal stability. The multi-branched ether ester compounds improve film continuity, reduce film brittleness, and regulate the volatilization rate. The multi-branched bridging derivative, through co-condensation reactions between its molecular branches and other components in the formulation, constructs a multi-node crosslinked network in the interfacial region. Simultaneously, it utilizes polar functional groups to form hydrogen bonds and chemical interactions with the epoxy encapsulation material, enhancing the interfacial anchoring density and network stability between the bonding agent layer and the epoxy matrix. The above components work synergistically to construct a molecular bridging structure of gold surface-gold π site-organic intermediate layer-covalent bond-epoxy encapsulation material, achieving high bonding strength, temperature and humidity resistance, without damaging the ultra-thin gold layer, and without interfering with wire bonding.
[0017] The present invention also provides a method for preparing the above-mentioned PCB gold bonding agent, comprising the following steps: mixing a multi-branched anthracene derivative, a multi-branched isocyanate silane, a multi-branched cycloboroxane derivative, a multi-branched ether ester compound, a multi-branched bridging derivative, and the remainder water, and stirring and mixing at room temperature for 20 to 40 minutes to obtain the PCB gold bonding agent.
[0018] The present invention also provides a method for using the above-mentioned PCB gold bonding agent, including a gold bonding step: immersing the degreased and washed PCB gold panel in a treatment solution containing the PCB gold bonding agent for gold bonding treatment.
[0019] Preferably, the mass concentration of the PCB gold bonding agent in the treatment solution is 3% to 8%.
[0020] Preferably, the gold bonding treatment is performed by immersion for a time of (60±6) s; the temperature of the treatment solution is 25±2℃.
[0021] In some specific embodiments, the method of using the PCB gold bonding agent of the present invention includes the following steps: S1. Degreasing: Degreasing treatment of the gold-plated PCB panel; S2. Water washing: Wash the gold-plated PCB panel after degreasing treatment with water; S3, Gold bonding: The washed PCB gold panel is immersed in a treatment solution containing the PCB gold bonding agent for gold bonding treatment. S4. Water washing: Wash the PCB gold panel after gold bonding treatment with water. S5. Drying: Dry the gold-plated PCB panel after washing. S6. Hot pressing: The dried PCB gold panel is hot-pressed and bonded to the epoxy prepreg to form a chemical bridging layer between the PCB gold surface and the organic resin.
[0022] Preferably, in step S6, the temperature of the hot-press bonding is 160–200°C, and the pressure is 120–180 N / cm. 2 The time is 30 to 60 minutes.
[0023] Compared with the prior art, the present invention has the following beneficial effects: (1) This invention uses the electron-rich large π conjugated system of multi-branched anthracene derivatives to form gold-π coordination anchoring with the gold surface, fundamentally overcoming the chemical inertness of the gold surface and realizing the effective anchoring of the bonding agent on the inert gold surface; (2) This invention uses multi-component synergistic construction of a complete molecular bridging structure, which significantly improves the lead bonding strength and interfacial shear strength. After testing, the lead bonding pull failure mode reaches level A, and the interfacial shear strength reaches level 1 (shear strength ≥ 12 MPa, no delamination at the interface); (3) The bonding agent of this invention does not damage the gold surface coating, the gold layer thickness loss is ≤ 0.01 μm, the microstructure of the gold surface is complete, and there are no corrosion pinholes; (4) The bonding agent of this invention has excellent resistance to humid heat aging. After aging at 85℃ / 85%RH for 1000h, the shear strength retention rate is ≥ 90%, and the interfacial delamination rate is 0; (5) The bonding agent of this invention does not damage the ultra-thin gold layer, does not interfere with lead bonding, is suitable for ultra-fine lines, and is suitable for automotive and 5G high reliability sulfur-free requirements. Attached Figure Description
[0024] To more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings used in the following description of the embodiments will be briefly introduced. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0025] Figure 1 The microstructure of the gold layer is shown in the scanning electron microscope (1000x) for testing the protective performance of the gold coating in Example 1. Figure 2 The microstructure of the gold coating is shown in the scanning electron microscope (1000x) for testing the protective performance of the gold coating in Comparative Example 16. Detailed Implementation
[0026] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. In the following embodiments and comparative examples, the amount of each component is by mass percentage, and the water mentioned is deionized water.
[0027] Example 1 Weigh out the following components in sequence: multi-branched anthracene derivative, multi-branched isocyanate silane, multi-branched cycloboroxane derivative, multi-branched ether ester compound, multi-branched bridging derivative, and the remaining water, and add them to the reaction vessel. Stir and mix at room temperature for 30 minutes to obtain the gold bonding agent. Seal and store the solution for later use.
[0028] The content of multi-branched anthracene derivatives is 1.5%, specifically: 1,4,5,8-tetramethoxyanthracene; The content of the multi-branched isocyanate silane is 0.5%, specifically: 3-isocyanate propyltriethoxysilane; The content of the multi-branched cyclic triboroxane derivative is 0.5%, specifically 2,4,6-tritert-butylcyclotriboroxane; The content of multi-branched ether ester compounds is 1.5%, specifically dipropylene glycol methyl ether acetate; The content of the multi-branched bridging derivative is 0.5%, specifically bis(3-triethoxysilylpropyl)amine; The remainder is water.
[0029] Example 2 Weigh out the following components in sequence: multi-branched anthracene derivative, multi-branched isocyanate silane, multi-branched cycloboroxane derivative, multi-branched ether ester compound, multi-branched bridging derivative, and the remaining water, and add them to the reaction vessel. Stir and mix at room temperature for 30 minutes to obtain the gold bonding agent. Seal and store the solution for later use.
[0030] The content of multi-branched anthracene derivatives is 1.5%, specifically: 2,3,6,7-tetramethoxy-9,10-dimethylanthracene; The content of the multi-branched isocyanate silane is 0.5%, specifically: 3-isocyanatopropyltrimethoxysilane; The content of the multi-branched cyclic triboroxane derivative is 0.5%, specifically 2,4,6-tributylcyclotriboroxane; The content of multi-branched ether ester compounds is 1.5%, specifically 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate; The content of the multi-branched bridging derivative is 0.5%, specifically 3-[tris(trimethylsiloxane)silyl]propylamine; The remainder is water.
[0031] Example 3 Weigh out the following components in sequence: multi-branched anthracene derivative, multi-branched isocyanate silane, multi-branched cycloboroxane derivative, multi-branched ether ester compound, multi-branched bridging derivative, and the remaining water, and add them to the reaction vessel. Stir and mix at room temperature for 30 minutes to obtain the gold bonding agent. Seal and store the solution for later use.
[0032] The content of multi-branched anthracene derivatives is 1.5%, specifically: 2,6-di-tert-butyl-9,10-dimethoxyanthracene; The content of the multi-branched isocyanate silane is 0.5%, specifically: tris[3(trimethoxysilyl)propyl]isocyanurate; The content of the multi-branched cyclic triboroxane derivative is 0.5%, specifically 2,4,6-triphenylcyclotriboroxane; The content of multi-branched ether ester compounds is 1.5%, specifically dipropylene glycol diacetate; The content of the multi-branched bridging derivative is 0.5%, specifically bis(3-trimethoxysilylpropyl)amine; The remainder is water.
[0033] Example 4 Weigh out the following components in sequence: multi-branched anthracene derivative, multi-branched isocyanate silane, multi-branched cycloboroxane derivative, multi-branched ether ester compound, multi-branched bridging derivative, and the remaining water, and add them to the reaction vessel. Stir and mix at room temperature for 30 minutes to obtain the gold bonding agent. Seal and store the solution for later use.
[0034] The content of multi-branched anthracene derivatives is 1.0%, specifically: 1,4,5,8-tetramethoxyanthracene; The content of the multi-branched isocyanate silane is 0.2%, specifically: 3-isocyanate propyltriethoxysilane; The content of the multi-branched cyclic triboroxane derivative is 0.2%, specifically 2,4,6-tritert-butylcyclotriboroxane; The content of multi-branched ether ester compounds is 1.0%, specifically dipropylene glycol methyl ether acetate; The content of the multi-branched bridging derivative is 0.2%, specifically bis(3-triethoxysilylpropyl)amine; The remainder is water.
[0035] Example 5 Weigh out the following components in sequence: multi-branched anthracene derivative, multi-branched isocyanate silane, multi-branched cycloboroxane derivative, multi-branched ether ester compound, multi-branched bridging derivative, and the remaining water, and add them to the reaction vessel. Stir and mix at room temperature for 30 minutes to obtain the gold bonding agent. Seal and store the solution for later use.
[0036] The content of multi-branched anthracene derivatives is 2.0%, specifically: 1,4,5,8-tetramethoxyanthracene; The content of multi-branched isocyanate silane is 1.0%, specifically: 3-isocyanate propyltriethoxysilane; The content of the multi-branched cyclic triboroxane derivative is 1.0%, specifically 2,4,6-tritert-butylcyclotriboroxane; The content of multi-branched ether ester compounds is 2.0%, specifically dipropylene glycol methyl ether acetate; The content of the multi-branched bridging derivative is 1.0%, specifically bis(3-triethoxysilylpropyl)amine; The remainder is water.
[0037] In the course of this invention research, gold bonding agents for comparative examples 1-15 were prepared based on Example 1, and gold bonding agent for comparative example 16 was prepared with reference to the prior art.
[0038] Comparative Example 1 The only difference between Comparative Example 1 and Example 1 is that the components do not contain multi-branched anthracene derivatives.
[0039] Comparative Example 2 The only difference between Comparative Example 2 and Example 1 is that the components do not contain multi-branched isocyanate silanes.
[0040] Comparative Example 3 The only difference between Comparative Example 3 and Example 1 is that the components do not contain multi-branched cyclic triboroxane derivatives.
[0041] Comparative Example 4 The only difference between Comparative Example 4 and Example 1 is that the components do not contain multi-branched ether ester compounds.
[0042] Comparative Example 5 The only difference between Comparative Example 5 and Example 1 is that the components do not contain multi-branched bridging derivatives.
[0043] Comparative Example 6 The only difference between Comparative Example 6 and Example 1 is that the concentration of the multibranched anthracene derivative in the component is 4.0%.
[0044] Comparative Example 7 The only difference between Comparative Example 7 and Example 1 is that the concentration of the multi-branched isocyanate silane in the component is 2.0%.
[0045] Comparative Example 8 The only difference between Comparative Example 8 and Example 1 is that the concentration of the multi-branched cyclic triboroxane derivative in the component is 2.0%.
[0046] Comparative Example 9 The only difference between Comparative Example 9 and Example 1 is that the concentration of the multi-branched ether ester compound in the component is 4.0%.
[0047] Comparative Example 10 The only difference between Comparative Example 10 and Example 1 is that the concentration of the multi-branched bridging derivative in the component is 2.0%.
[0048] Comparative Example 11 The only difference between Comparative Example 11 and Example 1 is that the multi-branched anthracene derivative component 1,4,5,8 tetramethoxyanthracene was replaced with an equal mass of anthracene (CAS No.: 120-12-7).
[0049] Comparative Example 12 The only difference between Comparative Example 12 and Example 1 is that the multi-branched isocyanate silane component 3, isocyanate propyltriethoxysilane, is replaced with an equal mass of trimethylethoxysilane (CAS No.: 1825-62-3).
[0050] Comparative Example 13 The only difference between Comparative Example 13 and Example 1 is that the multi-branched cyclic triboroxane derivative component 2,4,6-tert-butylcyclotriboroxane was replaced with an equal mass of trimethylcyclotriboroxane (CAS No.: 823-96-1).
[0051] Comparative Example 14 The only difference between Comparative Example 14 and Example 1 is that the dipropylene glycol methyl ether acetate component of the multi-branched ether ester compound was replaced with an equal mass of 2-methylcyclohexyl acetate (CAS No.: 5726-19-2).
[0052] Comparative Example 15 The only difference between Comparative Example 15 and Example 1 is that the multi-branched bridging derivative component, bis(3-triethoxysilylpropyl)amine, is replaced with an equal mass of methyltriethoxysilane (CAS No.: 2031-67-6).
[0053] Comparative Example 16 Comparative Example 16 uses a bonding agent based on existing technology (patent document CN116607136B), the specific components of which include: The specific preparation method of the 20 g / L composition of thiol-containing molecules and nitrogen-containing heterocyclic molecules includes the following steps: (1) Prepare an aqueous solution of arginine with a mass concentration of 10%, then add 13 g of γ-mercaptopropyltrimethoxysilane to 100 g of aqueous solution of arginine, add 5% dilute hydrochloric acid to adjust the pH to 5, stir at 75°C for 3 h to obtain a mixture; (2) Add 1,3-bis(1H-benzotriazolyl)propane to anhydrous ethanol to prepare a solution A with a mass concentration of 8%, then add 50 g of solution A to 120 g of the mixture in step (1), and add 8 g of 3,5-dimethyl-2-mercaptobenzimidazole, mix evenly to obtain the composition of thiol-containing molecules and nitrogen-containing heterocyclic molecules; The coupling agent content is 20 g / L, specifically: γ-aminopropyltriethoxysilane; The dispersant content is 5g / L, specifically: polyvinylpyrrolidone; The penetrant content is 7g / L, specifically: a mixture of sodium fatty alcohol polyoxyethylene ether sulfate and polyether silicone oil in a mass ratio of 1:1; The additive content is 3g / L, specifically a mixture of sodium benzoate and Tween-80 in a mass ratio of 4:1. The solvent is deionized water, which is used to make up the balance.
[0054] The method of using the gold-face bonding agent of this invention (for the following performance tests) includes the following steps: S1 degreasing; S2 water washing; S3 gold-face bonding; S4 water washing; S5 drying; S6 hot pressing; specifically: The S1 degreasing section is used to degrease the gold-plated PCB panel and remove surface impurities. The process parameters for this section are as follows: This section is a spray type; the sulfuric acid concentration in the degreasing tank is 1.0%, with the remainder being deionized water; the temperature is 25±0.5 ℃; the length of the degreasing section is 2.0 m; the linear velocity is 4.0±0.2 m / min; and the pressure is 1.5±0.5 kg / cm². 2 ; The S2 water washing section is used to wash the gold-plated PCB panel after the S1 degreasing section with deionized water. The process parameters for the water washing section are as follows: this section is a spray type, temperature 25±0.5 ℃, length of the water washing section is 2.0 m; linear speed 4.0±0.2 m / min, pressure 1.0±0.5 kg / cm 2 ; The S3 gold bonding section is used for surface treatment of the PCB gold panel after the S2 water washing section. The gold bonding agent prepared according to the embodiments or comparative proportions of this invention is added to the gold bonding tank at a mass concentration of 5%, with the remainder being deionized water. The process parameters for the gold bonding section are: immersion type, temperature 25±2 ℃, length 2.0 m, linear speed 2.0±0.2 m / min. In step S4, the washing section is to wash the PCB gold panel that has passed through the gold surface bonding section S3 with deionized water. The process parameters of the washing section are as follows: this section adopts a spray type, the temperature is 25±2 °C, the length of the washing section is 1.0 m, the line speed is 2.0±0.2 m / min, and the pressure is 1.5±0.5 kg / cm 2 ; In step S5, the drying section is to dry the PCB gold panel after the washing section S4 process. The process parameters of drying are as follows: the temperature is 70±2 °C, the length of the drying section is 1.0 m, and the line speed is 1.0±0.2 m / min.
[0055] In step S6, the hot pressing section performs hot press bonding on the PCB gold panel that has passed through the drying section S5 and the epoxy prepreg, so as to form a chemical bridging layer between the PCB gold surface and the organic resin. The process parameters of the hot press bonding section are as follows: the lamination temperature is 180 °C, and the lamination pressure is 150 N / cm 2 , and the lamination time is 40 min.
[0056] The performance of the gold surface bonding agent of the present invention is mainly tested from the following four aspects.
[0057] (1) Wire bonding pull performance: With reference to the MIL-STD-883 Method 2011 standard, a bonding pull tester is used, and a 25 μm diameter gold wire is used to complete ball bonding on the PCB gold pad treated with the gold surface bonding agent; the pull test hook is placed at the mid-span position of the lead, and a pull force is applied upward at a constant speed until the bonding point fails, and the bonding pull value and failure mode of each group of samples are recorded.
[0058] Failure mode classification: Class A: The lead body is broken, the fracture position is far away from the bonding ball, no pad peeling occurs, which is an ideal failure mode; Class B: The neck of the bonding ball is broken, and the bonding ball is completely retained on the gold pad; Class C: The bonding ball peels off from the gold pad interface, and less than 25% of the metal remains on the pad surface; Class D: The pad peels off and damages together with the underlying metal.
[0059] The requirements for this test result are that Class A or Class B is qualified, and the gold wire bonding pull force is ≥ 12g.
[0060] (2) Interfacial shear strength performance: With reference to the JEDEC JESD22-B116B standard, a standard chip is mounted on the surface of the gold pad treated with the bonding agent to complete epoxy curing; using a shear thrust tester, the shear punch is aligned with the side edge of the chip, the height of the punch is lower than the bottom surface of the chip, the chip is pushed laterally at a test speed of 0.5 mm / min, the maximum shear force when the chip is separated from the gold surface is recorded, and the shear strength is calculated.
[0061] Intensity level classification: Level 1: Shear strength ≥12MPa, no delamination at the interface, chip breakage; Level 2: Shear strength 812 MPa, with minor localized peeling at the interface; Level 3: Shear strength 48MPa, large-area peeling at the interface; Level 4: Shear strength < 4 MPa, complete debonding at the interface.
[0062] The requirement for passing this test is a Level 1 score.
[0063] (3) Gold plating protective performance (gold layer loss): Using an X-ray fluorescence thickness gauge (XRF), the gold layer thickness was measured at multiple gold pads on the same PCB before and after treatment. No less than 6 test points were selected for each sample. The difference in gold layer thickness before and after treatment was compared, and the gold layer thickness loss value was statistically analyzed. At the same time, the microstructure of the gold layer was observed with a scanning electron microscope to observe whether corrosion, pinholes, or cracks appeared.
[0064] Level determination: Grade 0: Gold layer thickness loss ≤ 0.01μm, intact microstructure of gold surface, no corrosion pinholes; Level 1: Gold layer thickness loss 0.01-0.03 μm, a few tiny spots on the gold surface, no obvious corrosion; Level 2: Gold layer thickness loss of 0.03-0.05 μm, with localized corrosion marks on the gold surface; Level 3: Gold layer thickness loss > 0.05 μm, with obvious pinholes and damage in the gold layer.
[0065] A score of 0 is required to pass this test.
[0066] (4) Reliability performance of damp heat aging: In accordance with the JEDEC JESD22A101 standard, the bonded PCB samples were placed in an 85 ℃ / 85% RH constant temperature and humidity test chamber and aged continuously for 1000h. After aging, the samples were taken out and cooled to room temperature, and the chip shear strength test was carried out again. The shear strength before and after aging was compared and the strength retention rate was calculated.
[0067] Level determination: Grade I: Shear strength retention ≥90%, SAM interface delamination rate 0%; Grade II: Shear strength retention rate 80%-90%, with localized minor delamination at the interface; Grade III: Shear strength retention rate 60%-80%, with obvious delamination at the interface; Grade IV: Shear strength retention rate <60%, large-area delamination at the interface.
[0068] The requirement for passing this test is to achieve Level I.
[0069] The performance test results of each embodiment and comparative example are shown in Table 1 below.
[0070] Table 1 Performance Test Results
[0071] Example 1: Scanning electron microscopy (1000x) for testing the protective performance of gold plating. The microstructure of the gold layer is shown in the image. Figure 1 As shown; the scanning electron microscope (SEM) microscopy (1000x) morphology of the gold coating used to test the protective performance of the gold coating in Comparative Example 16 is shown below. Figure 2 As shown.
[0072] As can be seen from the test results of Examples 1-5 in Table 1, the PCB gold-side bonding agent of the present invention has excellent comprehensive performance: the lead bonding pull failure mode reaches Class A, and the bonding point is mainly due to lead body fracture; the interface shear strength performance reaches Class 1, with no interface delamination and chip body fracture; the gold plating protective performance is Class 0, with gold layer thickness loss ≤0.01μm, and the gold surface microstructure is complete without corrosion pinholes; the damp heat aging reliability performance reaches Class I, with shear strength retention rate ≥90%, and the SAM detection interface delamination rate is 0, which can meet the process requirements of automotive and 5G high-reliability PCB gold-side packaging bonding.
[0073] The difference between Comparative Examples 1-5 and Example 1 is that the gold-face bonding agent of this invention lacks single components of multi-branched anthracene derivatives, multi-branched isocyanate silanes, multi-branched cycloboroxane derivatives, multi-branched ether ester compounds, and multi-branched bridging derivatives, respectively. The test results show that the multi-branched anthracene derivative, as the main body for gold-face anchoring, relies on an electron-rich large π-conjugated system to generate gold-π coordination, and is a key component for achieving effective anchoring of the bonding agent on inert gold surfaces; the multi-branched isocyanate silane can covalently integrate π-adsorbed anthracene into the silicon-oxygen network, improving the overall bonding strength; the multi-branched cycloboroxane derivative participates in silicon-oxygen crosslinking, buffering interfacial thermal stress and improving the thermal stability of the system; the multi-branched ether ester compounds improve film continuity, reduce film brittleness, and regulate the agent volatilization rate; the multi-branched bridging derivative can construct a multi-node crosslinked network, enhancing the anchoring density between the bonding agent layer and the epoxy matrix. The five components described above work synergistically to construct a complete molecular bridging structure of the gold surface, gold π-site, organic intermediate layer, covalent bond, and epoxy encapsulation material. When any of these components is missing, the wire bonding failure mode deteriorates, the interfacial shear strength decreases significantly, some samples show slight damage to the gold surface, and the interface is prone to delamination after damp heat aging. Therefore, the overall bonding effect of the PCB gold surface bonding agent of this invention is achieved through the synergistic interaction of its functional components; each component is indispensable and works in harmony with the others.
[0074] The difference between Comparative Examples 6-10 and Example 1 is that the concentrations of multi-branched anthracene derivatives, multi-branched isocyanate silanes, multi-branched cycloboroxane derivatives, multi-branched ether ester compounds, and multi-branched bridging derivatives in the single component of the gold-face bonding agent of this invention are all higher than the upper limit of the concentration of the bonding agent of this invention. Test results show that, compared with Example 15, further increasing the concentration of the above functional components does not further improve wire bonding, shear strength, gold-face protection, and wet heat aging reliability, and cannot bring about any performance gain of the bonding agent. On the contrary, it will significantly increase the cost of chemical preparation. Excessively high concentrations also pose a risk of causing excessively thick film layers that interfere with wire bonding. Therefore, the functional components of the gold-face bonding agent of this invention do not need to be added in excessively high amounts. Controlling the content of each component within the numerical range defined in the examples of this invention is sufficient to achieve excellent bonding process performance of the gold-face bonding agent.
[0075] Comparative Examples 11-15, compared to Example 1, involved replacing multi-branched anthracene derivatives, multi-branched isocyanate silanes, multi-branched cycloboroxane derivatives, multi-branched ether ester compounds, and multi-branched bridging derivatives with similar compounds of the same structure in equal mass. The test results confirmed that differences in the molecular branches and substituents of the functional components directly alter the gold π coordination effect, the degree of silicon-oxygen crosslinking, and the film quality. Using the aforementioned substitute compounds resulted in deterioration of the wire bonding failure mode, decreased interfacial shear strength, partial damage to the gold plating, and easy delamination of the interface after damp heat aging, making it difficult to meet the process requirements for high-reliability PCB gold-plated packaging bonding.
[0076] Comparative Example 16 is a prior art solution (patent document CN116607136B), which is compared and verified with the gold-face bonding agent of Example 1 of this invention. The test results show that compared with the prior art developed for copper surfaces, the gold-face bonding agent of this invention has superior comprehensive performance in key performance indicators such as wire bonding failure mode, interfacial shear strength, gold coating protection, and wet heat aging reliability. Existing copper-face bonding agents cannot build effective molecular bridging structures on inert gold surfaces, resulting in poor overall gold-face bonding performance.
[0077] In summary, the PCB gold bonding agent provided by this invention comprises functional components such as multi-branched anthracene derivatives, multi-branched isocyanate silanes, multi-branched cycloboroxane derivatives, multi-branched ether ester compounds, and multi-branched bridging derivatives. Through synergistic compounding of multiple components, a complete molecular bridging structure can be constructed on an inert gold surface, taking into account excellent wire bonding performance, high interfacial shear strength, zero damage to the gold plating layer, and excellent resistance to damp heat aging. At the same time, it does not interfere with wire bonding, is suitable for ultra-fine lines, and can meet the large-scale production application requirements of high-reliability PCB packaging such as automotive electronics and 5G RF modules.
[0078] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.
Claims
1. A PCB gold-side bonding agent, characterized in that, By mass percentage, it comprises the following components: 1.0%–2.0% of multi-branched anthracene derivatives; 0.2%–1.0% of multi-branched isocyanate silanes; 0.2%–1.0% of multi-branched cycloboroxane derivatives; 1.0%–2.0% of multi-branched ether esters; 0.2%–1.0% of multi-branched bridging derivatives; the balance being water. The multibranched anthracene derivative is selected from one or more of 1,4,5,8-tetramethoxyanthracene, 2,3,6,7-tetramethoxy-9,10-dimethylanthracene, and 2,6-di-tert-butyl-9,10-dimethoxyanthracene. The multi-branched isocyanate silane is selected from one or more of 3-isocyanatepropyltriethoxysilane, 3-isocyanatepropyltrimethoxysilane, and tris[3-(trimethoxysilyl)propyl]isocyanurate; The multi-branched cyclic triboroxane derivative is selected from one or more of 2,4,6-tritert-butylcyclotriboroxane, 2,4,6-tri-n-butylcyclotriboroxane, and 2,4,6-triphenylcyclotriboroxane; The multi-branched ether ester compound is selected from one or more of dipropylene glycol methyl ether acetate, 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate, and dipropylene glycol diacetate. The multi-branched bridging derivative is selected from one or more of bis(3-triethoxysilylpropyl)amine, 3-[tris(trimethylsiloxane)silyl]propylamine, and di(3-trimethoxysilylpropyl)amine.
2. The PCB gold bonding agent according to claim 1, characterized in that, The water is either deionized water or tap water.
3. The PCB gold bonding agent according to claim 1, characterized in that, By mass percentage, it includes the following components: 1,4,5,8-Tetramethoxyanthracene 1.5%; 3. Propyltriethoxysilane isocyanate 0.5%; 0.5% of 2,4,6-tert-butylcyclotriboroxane; Dipropylene glycol methyl ether acetate 1.5%; 0.5% bis(3-triethoxysilylpropyl)amine; The remainder is water.
4. A method for preparing the PCB gold bonding agent according to any one of claims 1 to 3, characterized in that, Includes the following steps: The multi-branched anthracene derivative, multi-branched isocyanate silane, multi-branched cycloboroxane derivative, multi-branched ether ester compound, multi-branched bridging derivative, and the balance water are mixed and stirred at room temperature for 20-40 minutes to obtain the PCB gold surface bonding agent.
5. A method for using a PCB gold-side bonding agent, characterized in that, The process includes a gold bonding step: immersing the degreased and washed PCB gold panel in a treatment solution containing the PCB gold bonding agent described in any one of claims 1 to 3 for gold bonding treatment.
6. The method of using the PCB gold-surface bonding agent according to claim 5, characterized in that, The mass concentration of PCB gold bonding agent in the treatment solution is 3% to 8%.
7. The method of using the PCB gold-surface bonding agent according to claim 5, characterized in that, The gold bonding treatment is performed by immersion for a time of (60±6) s; the temperature of the treatment solution is 25±2℃.
8. A method for using a PCB gold-side bonding agent, characterized in that, Includes the following steps: S1. Degreasing: Degreasing treatment of the gold-plated PCB panel; S2. Water washing: Wash the gold-plated PCB panel after degreasing treatment with water; S3, Gold bonding: The washed PCB gold panel is immersed in a treatment solution containing the PCB gold bonding agent according to any one of claims 1 to 3 for gold bonding treatment; S4. Water washing: Wash the PCB gold panel after gold bonding treatment with water. S5. Drying: Dry the gold-plated PCB panel after washing. S6. Hot pressing: The dried PCB gold panel is hot-pressed and bonded to the epoxy encapsulation material to form a chemical bridging layer between the PCB gold surface and the organic resin.
9. The method of using the PCB gold-side bonding agent according to claim 8, characterized in that, In step S3, the mass concentration of the PCB gold bonding agent in the treatment solution is 3% to 8%.
10. The method of using the PCB gold-face bonding agent according to claim 8, characterized in that, In step S6, the temperature for hot-press bonding is 160–200°C, and the pressure is 120–180 N / cm. 2 The time is 30 to 60 minutes.
Citation Information
Patent Citations
Surface nanofilm processing method prior to plastic packaging in semiconductor packaging
CN102412166A
PCB processing technology capable of improving lead bonding tension
CN115119414A
A bonding agent for circuit board surface treatment and preparation method thereof
CN116607136B