A high-speed laser repair method for locomotive axles
By employing a high-speed laser repair method, using spiral gradient scanning and composite stress control, the problems of limited repair depth, low bonding strength, and high residual stress in locomotive axles have been solved, achieving efficient and stable remanufacturing results.
Patent Information
- Application Number
- CN202611586169.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-14
- Publication Date
- 2026-11-17
AI Technical Summary
Existing locomotive axle repair technologies suffer from limited repair depth, low bonding strength, high residual stress, and low repair efficiency, making it difficult to meet the high safety standards required by the rail transit industry.
A high-speed laser repair method is adopted, in which alloy powder is delivered to the damaged area through coaxial powder feeding. Combined with a spiral gradient scanning path and composite stress control, a dense metallurgical bond is achieved at the damaged site, and the surface and internal stress of the cladding layer are optimized.
It achieves strong deep repair capability, high bonding strength, low residual stress, and high repair efficiency, meeting the long-term, high-strength, and high-stability remanufacturing requirements of locomotive axles.
Smart Images

Figure CN123108554A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of remanufacturing technology for key components of rail transit vehicles, and in particular relates to a high-speed laser repair method for locomotive axles. Background Technology
[0002] As the core load-bearing component of the running gear of rail transit vehicles, the axle has been in service for a long time in complex and harsh working conditions. Specifically, on the one hand, it continuously bears the high-frequency vibration alternating load brought about by wheel-rail coupling and the friction and wear of the wheel-axle mating surface. On the other hand, it is susceptible to surface scratches or dents caused by collisions with foreign objects on the track and impacts from sand and gravel. In addition, during the wheel replacement and axle removal process, uneven clamping and disassembly forces of the tooling may cause accidental strain on the axle. These damages can quickly induce fatigue crack propagation, directly threatening driving safety. Therefore, it is necessary to repair and remanufacture damaged axles.
[0003] Currently, the most commonly used repair process for locomotive axle surface damage is thermal spraying with molybdenum. This process relies on the wear and corrosion resistance of the molybdenum coating to repair the surface, and is especially suitable for shallow scratches, dents and other damage with a depth of no more than 0.5 mm. However, this process still has the following technical limitations: First, the bonding between the molybdenum sprayed coating and the substrate is mainly mechanical, and the bonding strength is usually less than 200 MPa. Within its applicable repair thickness range, the coating is still at risk of peeling, flaking, or even detachment under long-term heavy-load alternating stress, affecting the long-term operational reliability of the repaired axle. Second, due to the limitations of the coating's cohesive strength and residual stress, the effective repair depth of molybdenum spraying is usually only below 0.5 mm. For deep scratches, wear pits, and other damages exceeding 0.5 mm, current processes typically do not use molybdenum spraying for repair. Instead, the axle is scrapped directly because the axle diameter cannot be restored to its design size through molybdenum spraying, resulting in a large number of axles being unusable, causing resource waste and increased maintenance costs. Third, the control of the heat-affected zone and the stability of the interface structure in the molybdenum spraying process still need improvement, which may adversely affect the metallographic structure of the substrate and the fatigue strength of the axle.
[0004] While existing conventional laser additive repair technologies can achieve metallurgical bonding between the repair layer and the substrate, they still suffer from the following problems: First, conventional laser cladding often employs Gaussian-distributed spot sizes and reciprocating scanning paths, resulting in uneven spot energy distribution and unidirectional heat accumulation. This leads to high heat input, a wide heat-affected zone, and stress concentration in the cladding layer, along with low scanning speed and low repair efficiency. Second, conventional processes rely heavily on post-processing stress relief for residual stress control. This is not only cumbersome and time-consuming, but also fails to differentiate between the surface and interior of the cladding layer. Simultaneously addressing the introduction of residual compressive stress on the surface and the elimination of residual tensile stress in the interior is difficult, resulting in generally high residual stress in the cladding layer. Furthermore, post-processing can easily cause overall axle deformation, making it difficult to guarantee the dimensional accuracy of the repaired axle. Third, conventional laser cladding methods lack specific process optimization for the axisymmetric rotating structure and heavy-load fatigue characteristics of locomotive axles. They cannot simultaneously meet the requirements of deep repair, structural stability, and long-term service, making them unsuitable for the high safety standards of the rail transit industry.
[0005] Therefore, there is an urgent need to develop a locomotive axle repair method that combines deep repair capability, high bonding strength, low residual stress, and high efficiency to achieve high-quality remanufacturing of heavy-duty locomotive axles. Summary of the Invention
[0006] To address the aforementioned issues, this invention provides a high-speed laser repair method for locomotive axles, which enables deep repair of damaged axle areas through dense metallurgical bonding. Simultaneously, it optimizes the stress on the surface and inside of the cladding layer, taking into account repair depth, bonding strength, structural stability, and repair efficiency, thus meeting the long-term, high-strength, and high-stability remanufacturing requirements of locomotive axles.
[0007] This invention provides a high-speed laser repair method for locomotive axles, comprising: S1. Perform damage detection on the locomotive axle, determine the damaged area and remove the fatigue layer of the damaged area. When the depth of the damaged area reaches the preset depth, perform stepped grooving treatment on the damaged defects to form a multi-level stepped groove that rises step by step from the bottom layer to the top layer. S2. Alloy powder is fed to the damaged area using a coaxial powder feeding method. The axle is clamped in a CNC rotary fixture and rotates around its own axis. The laser cladding head is fed along the axial direction of the axle, so that the circumferential rotation of the axle and the axial feed of the laser cladding head are linked to form a spiral gradient scanning path. A ring-shaped laser beam is used to perform high-speed laser cladding on the damaged area along the spiral gradient scanning path. The spiral gradient scanning path extends from the position corresponding to the deepest point of the defect in the coordinate system of the axle cylindrical surface to the edge of the repair area, and the axial feed per revolution increases along the extension direction. S3. Behind the laser cladding spot, a composite stress control of ultrasonic rolling and pulsed laser shock is performed synchronously with the high-speed laser cladding. Compressive stress is introduced on the surface of the cladding layer by ultrasonic rolling, and residual stress inside the cladding layer is reduced by pulsed laser shock.
[0008] Preferably, in the above-mentioned high-speed laser repair method for locomotive axles, in step S1, the number of steps N of the stepped grooving process is determined by N=ceil(D1 / 0.5), where D1 is the depth value of the damage defect in mm, and ceil means rounding up; the depth of each step is 0.2mm to 0.7mm, and D1≥0.3mm.
[0009] Preferably, in the above-mentioned high-speed laser repair method for locomotive axles, the horizontal width W of each step surface is... i =max[4×(d i +d i+1 ), 4.0mm], where d i d represents the depth of the i-th step; i+1 Let d be the depth of the (i+1)th step. When i=N, let d N+1 =0; The bottom and sidewalls of each step are connected by a curved surface.
[0010] Preferably, in the above-mentioned high-speed laser repair method for locomotive axles, in step S1, the surface of the stepped groove is activated by an atmospheric pressure dielectric barrier discharge plasma jet before cladding, and the working gas is argon; the activation process is carried out under the protection of argon atmosphere and shares the same gas source as the argon protection gas path of the high-speed laser cladding.
[0011] Preferably, in the above-mentioned high-speed laser repair method for locomotive axles, in step S2, the alloy powder is an Fe-based Ni-Cr-Mo pre-alloyed powder, comprising, by mass percentage: Ni: 10.5% to 16.0%, Cr: 17.5% to 20.0%, Mo: 2.0% to 4.5%, C: ≤0.10%, Ti: 0.10% to 0.30%, Nb: 0.05% to 0.20%, with the balance being Fe and unavoidable impurities; the absolute difference between the coefficient of thermal expansion of the alloy powder and the average coefficient of linear expansion of the axle matrix is ≤1.5×10⁻⁶. -6 / ℃.
[0012] Preferably, in the above-mentioned high-speed laser repair method for locomotive axles, the scanning rate of the high-speed laser cladding is 30 m / min to 50 m / min, and the scanning rate is the linear velocity of the laser spot relative to the axle surface; the annular spot is a hollow annular spot with an inner diameter of 0.30 to 0.40 times the outer diameter and an outer diameter of 1.2 mm to 2.0 mm; the spiral gradient scanning path extends from the deepest point of the defect to the edge in the coordinate system of the axle cylindrical surface, and the axle rotation speed n and the scanning rate V satisfy V=πD2n, where D2 is the actual diameter of the area to be repaired.
[0013] Preferably, in the above-mentioned high-speed laser repair method for locomotive axles, the journal diameter of the axle is 140mm to 260mm; in step S2, the cladding parameters are matched segmentally according to the actual diameter of the area to be repaired, and the larger the diameter, the higher the scanning rate and laser power, and the lower the axial feed per revolution; the axial feed per revolution is 0.20mm / r to 0.40mm / r, and is consistent with the pitch of the spiral gradient scanning path.
[0014] Preferably, in the above-mentioned high-speed laser repair method for locomotive axles, in step S2, the temperature of the molten pool is monitored in real time and the laser power is adjusted in a closed loop to control the temperature of the molten pool at 1600℃ to 1800℃. At the same time, the substrate is preheated and interlayer insulation is performed to stabilize the substrate temperature at 180℃ to 250℃.
[0015] Preferably, in the above-mentioned high-speed laser repair method for locomotive axles, in step S3, both the ultrasonic rolling head and the pulsed laser impact head are located 5mm to 10mm behind the laser cladding spot. The two are arranged at a circumferential angle of 45° to 60° in the cross section perpendicular to the axle axis. Along the axle axis, the ultrasonic rolling head is closer to the laser cladding spot than the pulsed laser impact head. During the continuous rotation of the axle, the same cladding layer area first introduces surface compressive stress through the ultrasonic rolling head, and then the internal residual stress is reduced by the pulsed laser impact head.
[0016] Preferably, in the above-mentioned high-speed laser repair method for locomotive axles, a precision post-processing step is included after step S3: after CNC precision grinding of the cladding repair area, flexible polishing is performed using a nylon bristle brush containing abrasive. The flexible polishing is performed in two steps: coarse polishing and fine polishing. The polishing pressure is provided by the centrifugal force of the brush body rotation and natural contact. Finally, low-temperature aging treatment is performed.
[0017] As described above, the high-speed laser repair method for locomotive axles provided by this invention includes: damage detection of the locomotive axle, determination of the damaged area and removal of the fatigue layer in the damaged area; when the depth of the damaged area reaches a preset depth, a stepped grooving process is performed on the damage defect to form a multi-level stepped groove that rises from the bottom layer to the top layer; alloy powder is then fed to the damaged area using a coaxial powder feeding method; the axle is clamped in a CNC rotary fixture and rotates around its own axis; the laser cladding head is fed along the axial direction of the axle, so that the circumferential rotation of the axle and the axial feed of the laser cladding head are linked to form a spiral gradient scanning path; and a ring-shaped laser beam is used to perform high-speed laser cladding on the damaged area along the spiral gradient scanning path. The scanning path extends from the deepest point of the defect to the edge of the repair area in the coordinate system of the axle cylindrical surface. The axial feed per revolution increases along the extension direction. Finally, behind the laser cladding spot, a composite stress control of ultrasonic rolling and pulsed laser shock is performed simultaneously with the high-speed laser cladding. Compressive stress is introduced on the surface of the cladding layer by ultrasonic rolling, and residual stress inside the cladding layer is reduced by pulsed laser shock. Therefore, this repair method can achieve dense metallurgical bonding and deep repair of the damaged parts of the axle. At the same time as cladding, the stress of the surface and inside of the cladding layer is optimized, taking into account the repair depth, bonding strength, structural stability and repair efficiency, and meeting the long-term, high-strength and high-stability remanufacturing requirements of locomotive axles. Attached Figure Description
[0018] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the provided drawings without creative effort.
[0019] Figure 1 This is a schematic diagram of an embodiment of a high-speed laser repair method for locomotive axles provided by the present invention; Figure 2 This is a schematic diagram of the overall structure of the high-speed laser repair system for locomotive axles provided by the present invention; Figure 3 This is a schematic cross-sectional view of a stepped slotted structure. Detailed Implementation
[0020] The core of this invention is to provide a high-speed laser repair method for locomotive axles, which can achieve dense metallurgical bonding and deep repair of damaged axle parts, and optimize the stress of the surface and interior of the cladding layer while cladding, taking into account repair depth, bonding strength, structural stability and repair efficiency, thus meeting the long-term, high-strength and high-stability remanufacturing requirements of locomotive axles.
[0021] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0022] An example implementation of the high-speed laser repair method for locomotive axles provided by this invention. Figure 1 As shown, Figure 1 This is a schematic diagram of an embodiment of a high-speed laser repair method for locomotive axles provided by the present invention. The method may include the following steps: S1. Perform damage detection on the locomotive axle, determine the damaged area and remove the fatigue layer of the damaged area. When the depth of the damaged area reaches the preset depth, perform stepped grooving treatment on the damaged defects to form a multi-level stepped groove that rises step by step from the bottom layer to the top layer. Specifically, in step S1, a combination of ultrasonic testing and magnetic particle testing can be used to conduct non-destructive testing on the locomotive axle. This accurately locates various damage defects on the surface and near the surface, measures the depth, length, width, and distribution range of the defects, establishes a three-dimensional damage model, and clearly delineates the repair area and the non-repair isolation area. Subsequently, CNC precision turning is used to remove the fatigue layer, oxide scale, and impurities in the damaged area. After turning, the surface roughness is controlled between Ra1.6μm and Ra3.2μm. For damage defects with a depth of not less than 0.3mm, stepped grooving is implemented, with a 1:10 transition bevel on the groove wall to avoid stress concentration in the repair area. For shallow micro-damage with a depth of less than 0.3mm, stepped grooving is not required; after plasma activation, single-pass high-speed laser cladding can be directly applied. After the grooving is completed, the base surface is cleaned and repaired with anhydrous ethanol and ultrasonic cleaning to thoroughly remove oil, dust and other impurities. After drying at 80℃ to 100℃, the base surface is then subjected to plasma activation treatment to improve the wettability and interfacial bonding of the alloy powder on the base surface.
[0023] S2. Alloy powder is fed to the damaged area using a coaxial powder feeding method. The axle is clamped in a CNC rotary fixture and rotates around its own axis. The laser cladding head is fed along the axial direction of the axle, so that the circumferential rotation of the axle and the axial feed of the laser cladding head are linked to form a spiral gradient scanning path. The annular spot laser beam is used to perform high-speed laser cladding on the damaged area along the spiral gradient scanning path. The spiral gradient scanning path extends from the position corresponding to the deepest point of the defect in the coordinate system of the axle cylindrical surface to the edge of the repair area, and the axial feed per revolution increases along the extension direction. Specifically, in step S2, a coaxial powder-feeding high-speed laser cladding equipment can be used. This equipment is equipped with a molten pool condition monitoring module and an online stress monitoring module. The axle is clamped on a CNC rotary fixture to achieve coordinated operation of axial feed and circumferential rotation. The axial feed rate can be from 0.2 mm / r to 0.4 mm / r, and various process parameters such as laser, motion, powder feeding, and temperature control are optimized in a coordinated manner. (Reference) Figure 2 , Figure 2 This is a schematic diagram of the overall structure of the high-speed laser repair system for locomotive axles provided by the present invention. The overall structure may include an axle 1, a CNC rotary fixture 2, a tailstock 3, a multi-axis slide 4, a laser cladding head 5, a coaxial powder feeding nozzle 6, an annular spot 7, a cladding repair area 8, an ultrasonic rolling head 9, and a pulsed laser impact head 10. The diagram also shows the axle's rotation direction and axial feed direction. A fiber laser can be used for cladding, with the laser power set to 2.5kW to 4.5kW and the spot diameter to 1.2mm to 2.0mm. An annular spot mode is used to ensure uniform energy distribution and avoid local overheating. The scanning rate is controlled at 30m / min to 50m / min, the overlap rate is 45% to 55%, and the pitch of the spiral gradient scanning path varies from 0.20mm / r to 0.40mm / r. Adjacent paths use a 1 / 4 overlap method. The powder feeding rate can be set from 12g / min to 20g / min, and the powder feeding gas pressure can be from 0.3MPa to 0.5MPa. 99.99% high-purity argon is used as the protective gas, and the gas flow rate can be from 15L / min to 20L / min to isolate the molten pool from air and prevent oxidation. Through the coupling effect of high-speed scanning and low heat input, rapid solidification of the molten pool is achieved, forming a dense metallurgical bonding layer without pores, cracks, or inclusions. The bonding strength is not less than 450MPa, and the repair depth can reach more than 3mm. This breaks through the 0.5mm repair depth limitation of traditional molybdenum spraying processes.
[0024] S3. Behind the laser cladding spot, a composite stress control of ultrasonic rolling and pulsed laser shock is carried out simultaneously with high-speed laser cladding. Compressive stress is introduced on the surface of the cladding layer by ultrasonic rolling, and residual stress inside the cladding layer is reduced by pulsed laser shock.
[0025] Specifically, in step S3, an integrated mode of simultaneous cladding and stress control can be adopted. At a position 5mm to 10mm behind the laser cladding spot, combined stress control of ultrasonic rolling and pulsed laser impact is simultaneously implemented: the rolling head is 6mm behind the laser cladding spot, the impact head is 8mm behind the laser cladding spot, the ultrasonic rolling force can be controlled between 800N and 1200N, and the diameter of the ultrasonic rolling head can be 3mm to 5mm. This plastically strengthens the high-temperature cladding layer, introducing -500MPa pressure onto the surface of the cladding layer. The compressive stress is reduced to -300MPa to suppress the initiation of fatigue cracks. The pulsed laser shock energy is set to 1.5J to 3.0J, the pulse width is 5ns to 10ns, and the spot diameter is 0.8mm to 1.2mm. This targets and reduces the residual stress inside the cladding layer, ensuring that the internal residual stress does not exceed 50MPa. At the same time, it refines the surface grains, improves the density and fatigue strength of the cladding layer, and the entire process can be monitored in real time by stress sensors and the control parameters can be adjusted accordingly to ensure that the residual stress meets the standard and avoid thermal deformation of the axle.
[0026] As described above, in the embodiments of the high-speed laser repair method for locomotive axles provided by the present invention, damage detection of the locomotive axle is performed, the damaged area is determined, and the fatigue layer of the damaged area is removed. When the depth of the damaged area reaches a preset depth, a stepped grooving process is performed on the damage defect to form a multi-level stepped groove that rises from the bottom layer to the top layer. Then, alloy powder is fed to the damaged area using a coaxial powder feeding method. The axle is clamped in a CNC rotary fixture and rotates around its own axis. The laser cladding head is fed along the axial direction of the axle, so that the circumferential rotation of the axle and the axial feed of the laser cladding head are linked to form a spiral gradient scanning path. A ring-shaped laser beam is used to perform high-speed laser cladding on the damaged area along the spiral gradient scanning path. The spiral gradient scanning path extends from the deepest point of the defect to the edge of the repair area in the coordinate system of the axle cylindrical surface, with the axial feed per revolution increasing along the extension direction. Finally, behind the laser cladding spot, a composite stress control of ultrasonic rolling and pulsed laser shock is implemented simultaneously with high-speed laser cladding. Compressive stress is introduced on the surface of the cladding layer by ultrasonic rolling, and residual stress inside the cladding layer is reduced by pulsed laser shock. Therefore, this repair method can achieve dense metallurgical bonding and deep repair of the damaged parts of the axle, and optimize the stress on the surface and inside of the cladding layer at the same time as cladding. It takes into account the repair depth, bonding strength, structural stability and repair efficiency, and meets the long-term, high-strength and high-stability remanufacturing requirements of locomotive axles.
[0027] In a specific embodiment of the above-mentioned high-speed laser repair method for locomotive axles, in step S1, the number of steps N in the stepped grooving process can be determined by N=ceil(D1 / 0.5), where D1 is the depth value of the damage defect in mm, and ceil means rounding up; the depth of each step can be from 0.2mm to 0.7mm, and D1≥0.3mm.
[0028] Specifically, in the formula for calculating the number of steps N, 0.5mm is the safe thickness benchmark for a single layer of cladding. The depth of each step is distributed from the bottom to the top according to the following rules: the depth of the bottom step d1 is 0.30mm, and the depth of each intermediate step d... i Take 0.50mm (2≤i≤N-1), the depth d of the top step N =D1-Σd1 to d N-1 , and d N The depth should be no less than 0.20 mm to ensure balanced thermal stress across all cladding layers. For example, for a damage defect with a depth of 1.2 mm, the number of steps N = ceil(1.2 / 0.5) = 3, and the depth of each step can be distributed as follows: bottom layer 0.30 mm, middle layer 0.50 mm, and top layer 0.40 mm. A specific example is... Figure 3 As shown, Figure 3 This is a schematic cross-sectional view of a stepped slotted structure, where d1, d2, and d3 are the depths of the bottom, middle, and top steps, respectively; W1, W2, and W3 are the horizontal widths of the corresponding step surfaces; R1, R2, and R3 are the arc transition radii between the bottom of the step and the sidewall; D1 is the total depth of the damage / defect; and the slot wall has a 1:10 transition bevel.
[0029] Based on the above specific embodiments, further, the horizontal width W of each step surface... i =max[4×(d i +d i+1 ), 4.0mm], where d i Let d be the depth of the i-th step. i+1 Let d be the depth of the (i+1)th step. When i=N, let d N+1 =0; The bottom and sidewalls of each step are connected by a curved surface.
[0030] Specifically, the horizontal width of each step surface is determined according to the above rules, which ensures that the transition slope ratio between two adjacent steps is not less than 1:4, and that the cladding spot covers each step surface at least twice, thereby reducing the stress concentration factor K. t The radius R of the arc at the transition surface between the bottom and sidewall of each step should be kept below 1.35. i Based on the depth d of the current step i Adaptive value selection, i.e., R i=clamp(0.6×d i The formula (0.2mm, 2.0mm) is used, where the `clamp` function restricts the calculation result to a range between 0.2mm and 2.0mm. This rule ensures that the radius of the arc does not exceed the depth of the step, thus preserving the step shape. The lower limit of 0.2mm is sufficient to control the notch stress concentration factor within 1.5, while the upper limit of 2.0mm takes into account the versatility of the standard tool library. Each arc transition surface is precision turned in one pass using a CNC turning tool with rounded corners, resulting in a surface roughness Ra of no more than 1.6μm after forming.
[0031] In another specific embodiment of the above-mentioned high-speed laser repair method for locomotive axles, in step S1, atmospheric pressure dielectric barrier discharge plasma jet can be used to activate the surface of the stepped groove before cladding, and the working gas can be argon; the activation process is carried out under the protection of argon atmosphere and shares the same gas source as the argon protection gas path of high-speed laser cladding.
[0032] Specifically, after the substrate is dried, an atmospheric pressure dielectric barrier discharge (DBD) plasma jet generator can be used to perform plasma activation treatment on the stepped groove surface. The working gas can be high-purity argon, with a purity of not less than 99.999%. Under high-frequency, high-voltage (5kV to 15kV) excitation at 15kHz to 25kHz, an atmospheric pressure low-temperature plasma jet is generated in the discharge chamber and sprayed onto the substrate through a nozzle. Argon ions and high-energy active particles bombard the substrate, sputtering away residual oxide layers and adsorbed contaminants, while simultaneously breaking the metal atomic bonds on the substrate, forming numerous dangling active sites, thereby improving the surface energy of the substrate and the wettability of the alloy powder. Activation process parameters can be: discharge power of 1kW to 3kW, processing time of 5min to 10min, and distance from the nozzle outlet to the substrate of 5mm to 8mm. During the processing, the surface temperature of the axle does not rise by more than 50°C, and the original metallographic structure of the substrate, which has already undergone tempering treatment, remains unchanged. After activation, the substrate surface exhibits its natural metallic color, with a contact angle of no more than 10° and a surface energy of no less than 72 mN / m, meeting the wettability requirements of high-speed laser cladding. Furthermore, the plasma activation process is conducted entirely under an argon atmosphere with a flow rate of 5 L / min to 10 L / min, sharing the same gas source as the argon protective gas path used in subsequent high-speed laser cladding to prevent secondary oxidation of the activated substrate surface during transport.
[0033] In another specific embodiment of the above-mentioned high-speed laser repair method for locomotive axles, in step S2, the alloy powder is an Fe-based Ni-Cr-Mo pre-alloyed powder, which may include, by mass percentage: Ni: 10.5% to 16.0%, Cr: 17.5% to 20.0%, Mo: 2.0% to 4.5%, C: ≤0.10%, Ti: 0.10% to 0.30%, Nb: 0.05% to 0.20%, with the balance being Fe and unavoidable impurities; the absolute difference between the coefficient of thermal expansion of the alloy powder and the average coefficient of linear expansion of the axle matrix is ≤1.5×10⁻⁶. -6 / ℃.
[0034] Specifically, considering the matrix characteristics of commonly used alloy steels such as EA4T, EA1N, and 42CrMo in locomotive axles, the aforementioned alloy powder can be Fe-based Ni-Cr-Mo pre-alloyed powder. This powder can be prepared by gas atomization, with a particle size range of 50μm to 150μm, a loose packing density of 3.8g / cm³ to 4.2g / cm³, and a flowability of no more than 18s / 50g. The functions of each chemical component in the powder are as follows: Ni is used to ensure sufficient austenite content in the cladding layer and improve toughness, preferably 13.0%; Cr is used to form a dense passivation film, improving corrosion resistance and solid solution strengthening effect, preferably 18.5%; Mo is used for solid solution strengthening and improving high-temperature tempering stability, preferably 3.0%; C is strictly controlled to a low carbon content to avoid cracking of the cladding layer due to carbide networks, preferably 0.06%; Ti and Nb are grain refining elements, forming TiC and NbC respectively to pin grain boundaries and inhibit grain growth, preferably 0.20% for Ti and 0.10% for Nb. In addition, by mass percentage, the powder may also include Si: 0.12% to 1.0% (preferably 0.5%), for deoxidation and improving melt flowability; Mn: not more than 0.80% (preferably 0.4%), for deoxidation and desulfurization; B: 0 to 0.65% (preferably 0.3%), for lowering the melting point and improving wettability; P not more than 0.030%, and S not more than 0.030%, to strictly control impurity content. The powder composition design simultaneously meets the following constraints: the coefficient of thermal expansion is consistent with the EA4T matrix (the coefficient of thermal expansion is approximately 11 × 10⁻⁶). -6 / ℃ to 12×10 -6 The values ( / ℃) match, and the difference between the two is no greater than 1.5×10. -6 / ℃; the hardness of the cladding layer is 280HV to 320HV, with a smooth transition from the hardness of the substrate (280HV to 300HV), and there is no stress concentration caused by a sudden change in hardness.
[0035] In a preferred embodiment of the above-mentioned high-speed laser repair method for locomotive axles, the scanning rate of the high-speed laser cladding is 30 m / min to 50 m / min, and the scanning rate is the linear velocity of the laser spot relative to the axle surface; the annular spot is a hollow annular spot with an inner diameter of 0.30 to 0.40 times the outer diameter and an outer diameter of 1.2 mm to 2.0 mm; the spiral gradient scanning path extends from the deepest point of the defect to the edge in the coordinate system of the axle cylindrical surface, and the axle rotation speed n and the scanning rate V satisfy V=πD2n, where D2 is the actual diameter of the area to be repaired.
[0036] Specifically, the hollow annular laser spot can be achieved using a conical-annular double-mirror technique, with a duty cycle K preferably of 0.35. Its energy flux density exhibits a saddle-shaped distribution, with uniform energy in the annular region. This significantly improves the energy uniformity in the scanning width direction compared to traditional Gaussian distribution laser spots. Combined with coaxial powder feeding within the laser beam, it achieves encapsulated coupling heating of the powder. The pitch of the spiral gradient scanning path increases linearly from the center to the edge of the repair area along the axial direction, from 0.20 mm / r to 0.40 mm / r. The scan starts from the deepest point of the defect and expands outwards in a spiral pattern. This allows the heat source to diffuse symmetrically from the center outwards, avoiding unidirectional heat accumulation, improving the symmetry of the temperature field, and resulting in a more uniform distribution of residual stress. It should be noted that the 1 / 4 overlap between adjacent paths refers to the circumferential coverage ratio between adjacent spiral loops, which is a path topology parameter; while the overlap rate of 45% to 55% refers to the radial width overlap ratio between adjacent cladding passes, which is a cladding forming parameter. Both constrain the integrity of the cladding layer circumferentially and radially, respectively, and both conditions must be met simultaneously. Compared to the conventional zigzag reciprocating scanning path, the spiral gradient scanning path used here can reduce the residual stress of the cladding layer by more than 35%. This has been verified by ANSYS finite element simulation and XRD measurement. The simulated residual stress value has decreased from about 77 MPa to about 48 MPa, and the measured value has decreased from about 75 MPa to about 46 MPa. At the same time, compared with conventional laser cladding with a scanning rate of about 10 m / min, the repair efficiency of this method can be improved by more than 50%.
[0037] In another preferred embodiment of the above-mentioned high-speed laser repair method for locomotive axles, the journal diameter of the axle is 140mm to 260mm; in step S2, the cladding parameters are matched segmentally according to the actual diameter of the area to be repaired, and the larger the diameter, the higher the value of the scanning rate and laser power, and the lower the value of the axial feed per revolution; the axial feed per revolution is 0.20mm / r to 0.40mm / r, and is consistent with the pitch of the spiral gradient scanning path.
[0038] Specifically, due to the stepped diameter structure of the axle, the surface curvature of different diameter segments varies, resulting in differences in molten pool spreading behavior and heat dissipation conditions. Therefore, the cladding parameters need to be graded and matched according to the actual diameter of the area to be repaired. The matching of the axial feed rate f and the scanning rate V follows an inverse correlation constraint: for every 10 m / min increase in the scanning rate V, the axial feed rate f decreases by 0.05 mm / r to 0.08 mm / r to ensure that the overlap rate between adjacent helical paths remains stable at 45% to 55%. The specific matching relationship is as follows: when V is 30 m / min to 35 m / min (excluding 35 m / min), f is 0.35 mm / r to 0.40 mm / r; when V is 35 m / min to 42 m / min (excluding 42 m / min), f is 0.28 mm / r to 0.35 mm / r; when V is 42 m / min to 50 m / min, f is 0.20 mm / r to 0.28 mm / r. The parameter adjustment rules for different diameter ranges are as follows: For the large diameter range (200mm to 260mm), which has small curvature and good molten pool stability, a high parameter range is used, with V ranging from 40m / min to 50m / min, f from 0.25mm / r to 0.35mm / r, laser power P from 3.5kW to 4.5kW, and spot diameter from 1.8mm to 2.0mm; for the medium diameter range (160mm to 200mm, excluding 200mm), a medium parameter range is used, with V at 35m / min. For speeds up to 45 m / min, f is set to 0.28 mm / r to 0.38 mm / r, P to 3.0 kW to 4.0 kW, and the spot diameter to 1.5 mm to 1.8 mm. For smaller diameter segments (140 mm to 160 mm, excluding 160 mm), where curvature is high and the molten pool is prone to flow deviation, a lower parameter range is used: V is set to 30 m / min to 38 m / min, f to 0.32 mm / r to 0.40 mm / r, P to 2.5 kW to 3.5 kW, and the spot diameter to 1.2 mm to 1.5 mm. In actual operation, the actual diameter of the area to be repaired is automatically read by the CNC system. The process database matches and outputs the corresponding cladding parameter combination according to the above-mentioned grading rules, requiring no manual intervention. Simultaneously, the overlap rate and cladding layer forming quality are verified in real time through the molten pool status monitoring module. When the overlap rate deviates from the range of 45% to 55%, the system automatically fine-tunes the axial feed amount f (adjustment step size 0.01 mm / r) for compensation.
[0039] In another preferred embodiment of the above-mentioned high-speed laser repair method for locomotive axles, in step S2, the temperature of the molten pool is monitored in real time and the laser power is adjusted in a closed loop to control the temperature of the molten pool at 1600°C to 1800°C. At the same time, the substrate is preheated and interlayer insulation is performed to stabilize the substrate temperature at 180°C to 250°C.
[0040] Specifically, the molten pool temperature is acquired in real time through a molten pool condition monitoring module. This module uses a combination of multispectral imaging and high-speed infrared thermometry to acquire real-time molten pool size data and temperature distribution. The deviation thresholds for molten pool size are set to ±0.2 mm for width and ±0.1 mm for depth. The substrate temperature is monitored using online coaxial temperature measurement, with the measurement point positioned 5 mm from the edge of the repair area. By simultaneously performing preheating and interlayer insulation, the substrate temperature is stabilized between 180℃ and 250℃ with fluctuations not exceeding ±5℃ to avoid sudden temperature rises and falls. The linkage adjustment logic between temperature and laser power is as follows: when the molten pool temperature exceeds 1800℃, the laser power is reduced by 5% to 10%; when the molten pool temperature is below 1600℃, the laser power is increased by 3% to 5%, thereby controlling the heat-affected zone within 0.3 mm. Furthermore, the hardware layer of the molten pool condition monitoring module adopts a four-band multispectral imaging architecture: the visible light band (400nm to 700nm) is used for molten pool topography imaging, the near-infrared band (780nm to 1000nm) and short-wave infrared band (1000nm to 1700nm) are used for temperature field measurement in the high-temperature zone of the molten pool, and the mid-wave infrared band (3μm to 5μm) is used for substrate temperature monitoring. The four bands are simultaneously acquired by a single camera through a beam splitter prism group and a narrowband filter. Infrared temperature measurement can use a VPD type PbSe area array camera (64×64 pixels) with a maximum frame rate of 1000 frames / second, and substrate temperature monitoring uses an infrared pyrometer with a sampling frequency of 100Hz. At the algorithm level, a multi-band colorimetric temperature measurement model was established to address the emissivity differences of Fe-Ni-Cr-Mo alloys in the solid, liquid, and mushy regions. This model aims to eliminate the impact of emissivity uncertainty on temperature measurement accuracy. Furthermore, in conjunction with control logic that links temperature and laser power for adjustment and an algorithm for real-time extraction of molten pool size, the hardware, algorithm, CNC system, and laser control interface are integrated into a unified temperature control system.
[0041] Those skilled in the art will understand that in the above-mentioned high-speed laser repair method for locomotive axles, in step S3, both the ultrasonic rolling head and the pulsed laser impact head can be located 5mm to 10mm behind the laser cladding spot. The two are arranged at a circumferential angle of 45° to 60° in the cross section perpendicular to the axle axis. Along the axle axis, the ultrasonic rolling head is closer to the laser cladding spot than the pulsed laser impact head. During the continuous rotation of the axle, the same cladding layer area first introduces surface compressive stress through the ultrasonic rolling head, and then the internal residual stress is reduced through the pulsed laser impact head.
[0042] Specifically, the circumferential angle between the ultrasonic rolling head and the pulsed laser impact head is defined as: the angle α between the radial line connecting the axle center to the contact point between the ultrasonic rolling head and the cladding layer, and the radial line connecting the axle center to the center of the pulsed laser impact head spot. α can be between 45° and 60°. Along the axle axial direction, the ultrasonic rolling head is closer to the laser cladding spot, preferentially contacting the high-temperature cladding layer for plastic deformation. The pulsed laser impact head lags slightly in the axial direction, impacting the subsurface layer that has cooled to 200°C to 300°C. This circumferentially staggered arrangement has three functions: First, it ensures that the areas of action of the two energy fields do not overlap on the axle surface, avoiding interference between the mechanical vibration of ultrasonic rolling and the beam of pulsed laser impact. Second, during the continuous rotation of the axle, the same cladding layer area first undergoes surface compressive stress through the ultrasonic rolling head, and after a circumferential travel time delay corresponding to angle α (when α is expressed in radians, the time delay τ=α / (2πn), where n is the axle rotation speed), it then undergoes pulsed laser impact to eliminate internal tensile stress, achieving full-dimensional stress control of the surface and interior. Third, during one rotation of the axle, each of the two working heads completes one treatment of the entire circumference of the cladding layer, leaving no area untreated. In terms of installation structure, the laser cladding head, ultrasonic rolling head, and pulsed laser impact head are all fixedly mounted on the same multi-axis linkage slide base and arranged in series along the axle axis. The laser cladding head is located at the front, the ultrasonic rolling head is located in the middle (5mm to 10mm away from the cladding spot), and the pulsed laser impact head is located at the rear (5mm to 10mm away from the cladding spot). The three tool heads are fed synchronously along the axle axis with the slide. The two ends of the axle are clamped by CNC rotary fixtures to achieve circumferential rotation around the axis. The multi-axis linkage slide feeds along the axle axis and cooperates with the circumferential rotation of the axle to achieve the helical scanning path. The ultrasonic rolling head consists of an ultrasonic generator, a piezoelectric ceramic transducer, an amplitude transformer, and a WC-Co hard alloy rolling head (3mm to 5mm in diameter) connected in sequence. The axis of the rolling head coincides with the normal of the axle surface. A normal load of 800N to 1200N is applied by a spring or pneumatic loading mechanism. The output frequency of the ultrasonic generator is 20kHz to 40kHz, preferably 28kHz to 35kHz. The ultrasonic generator converts the vibration into mechanical vibration of the same frequency through the piezoelectric ceramic transducer, and then the amplitude is amplified by the amplitude transformer before being transmitted to the rolling head, which acts on the surface of the high-temperature cladding layer. The matching ratio between the rolling head rotation speed and the axle rotation speed is 1:1.2 to 1:1.5. The pulsed laser impact head uses an Nd:YAG solid-state laser with an output wavelength of 1064nm, a repetition frequency of 1Hz to 10Hz, a single pulse energy of 1.5J to 3.0J, a pulse width of 5ns to 10ns, and a spot diameter of 0.8mm to 1.2mm. The laser beam emitted from its focusing head coincides with the normal to the surface of the axle.For stress monitoring, a piezoelectric force sensor, an ultrasonic stress sensor, and a resistance strain gauge force sensor are used in synergistic monitoring: The piezoelectric force sensor (PVDF thin film type, sampling frequency 1MHz) is installed on the back of the lens at the end of the optical path inside the pulsed laser impact head, and indirectly characterizes the stability of the impact energy by monitoring the pressure amplitude when the laser shock wave reaches the mirror surface; the ultrasonic stress sensor (longitudinal wave probe, 5MHz, sampling frequency 100Hz) is placed on the substrate surface 3mm from the edge of the repair area, and detects the residual stress inside the cladding layer in real time by using the longitudinal wave acoustic time difference based on the acoustoelastic effect; the resistance strain gauge force sensor (range 0 to 2000N, sampling frequency 5kHz) is integrated between the amplitude transformer and the rolling head of the ultrasonic rolling head to monitor the rolling contact force in real time. The detection signals from the aforementioned sensors are input to the controller. The controller uses surface residual stress and internal residual stress as controlled variables, and ultrasonic rolling pressure, pulsed laser impact energy, and the axial distance between the two tool heads as manipulated variables. It employs a fuzzy PID composite control strategy for adjustment, that is, it adjusts the PID parameters online according to the real-time stress deviation, and outputs an execution signal to drive the pneumatic proportional valve, the laser Q-switching module, and the servo motor to complete the adjustment. The control accuracy of surface residual stress is ±25MPa, the control accuracy of internal residual stress is ±10MPa, the control accuracy of ultrasonic rolling pressure is ±20N, and the control accuracy of pulsed laser energy is ±0.1J.
[0043] This application also provides the following preferred embodiments. Based on the above embodiments, after step S3, a precision post-processing step may be included: after CNC precision grinding of the cladding repair area, flexible polishing is performed using a nylon bristle brush containing abrasive. The flexible polishing is performed in two steps: coarse polishing and fine polishing. The polishing pressure is provided by the centrifugal force of the brush body rotation and natural contact. Finally, a low-temperature aging treatment is performed.
[0044] Specifically, in the precision post-processing step, a high-precision cylindrical grinding machine is used to perform step-by-step CNC fine grinding on the cladding repair area. Rough grinding removes the machining allowance, and fine grinding controls the shaft diameter dimensional tolerance to within ±0.01mm, the roundness to no more than 0.005mm, the coaxiality to no more than 0.01mm, and the roughness to Ra0.4μm to Ra0.8μm, which meets the assembly accuracy requirements of locomotive axles. After CNC precision grinding achieves dimensional accuracy, flexible polishing is performed using abrasive nylon bristle brushes (flexible honing brushes). This polishing tool consists of a metal wire skeleton and nylon bristles with abrasive balls fixed at the top. Utilizing its flexible characteristics, it naturally conforms to the curved surface of the axle repair area under centrifugal force to remove trace amounts of material and perform surface finishing. Polishing is performed in two steps: rough polishing and fine polishing. Rough polishing uses abrasive brushes with grit sizes of 180# to 400# to quickly remove grinding marks. Fine polishing uses abrasive brushes with grit sizes of 600# to 1000# to reduce the surface roughness to Ra0.4μm to Ra0.6μm and eliminate residual marks. Polishing pressure is provided solely by the centrifugal force of the rotating brush and natural contact, eliminating the need for additional pressurization devices. The polishing speed is 800 r / min to 1000 r / min, and the radial feed rate is controlled at 0.01 mm / pass to 0.03 mm / pass. Uniform polishing is achieved through multiple micro-feeds, avoiding damage to the residual compressive stress state of the cladding layer surface or causing surface overheating due to excessive pressure. This flexible polishing method effectively preserves the residual compressive stress introduced by the preceding ultrasonic rolling while improving surface smoothness, without generating new grinding marks or work-hardened layers. Finally, a low-temperature aging treatment is performed at a temperature of 150℃ to 180℃, a heating rate of 5℃ / min to 10℃ / min, and a holding time of 2h to 3h. The axle is then cooled to room temperature in the furnace to stabilize the microstructure, eliminate residual stress, and ensure the dimensional stability of the axle. Furthermore, after the precision post-processing steps, the product inspection and acceptance steps can also be included: mechanical property testing of the repaired product, verifying that the hardness of the cladding layer is controlled within the range of 280HV to 320HV, and testing the bonding strength and impact toughness indicators; non-destructive re-inspection using a combination of magnetic particle testing and ultrasonic testing to ensure that the cladding layer is free of defects and cracks; full-dimensional measurement of the axle, verifying key parameters such as axle diameter, roundness, and coaxiality, and determining acceptance as qualified after all indicators meet the locomotive axle manufacturing standards. Among them, the mechanical performance testing shall be carried out in accordance with the methods specified in TB / T1027.2-2015 "Locomotive Axles Part 2: Axles"; the non-destructive testing shall be carried out in accordance with TB / T1618-2001 "Ultrasonic Testing of Locomotive and Rolling Stock Axles" to conduct 100% ultrasonic testing on the cladding layer and heat-affected zone, and magnetic particle testing shall be carried out in accordance with TB / T1619-2010 "Magnetic Particle Testing of Locomotive and Rolling Stock Axles"; all dimensions, geometric tolerances and surface roughness of the repaired axle shall comply with the provisions of TB / T 1027.2-2015.
[0045] The following example illustrates the high-speed laser repair method for locomotive axles provided by this invention, so that those skilled in the art can better understand the technical solution of this invention. However, the following example is only illustrative and should not be construed as limiting the scope of protection of this invention.
[0046] The object of repair in this example is an EA4T steel axle of a locomotive. The axle journal has a linear scratch with a depth of 1.2mm and a length of 80mm, and localized scoring occurred during axle removal. Conventional molybdenum spraying cannot repair this. The axle substrate hardness is 280HV to 300HV. The specific repair process and parameters are as follows: Step S1, Pre-treatment: A three-dimensional damage model is established by combining ultrasonic testing and magnetic particle testing. The fatigue layer is removed by CNC precision turning, and the surface roughness is Ra2.0μm. A stepped groove with a 1:10 transition bevel is made on the scratched area. After ultrasonic cleaning with anhydrous ethanol, it is dried at 80℃ and then activated by plasma at 2kW for 8min and 6mm.
[0047] Step S2, High-speed laser cladding: Fe-based Ni-Cr-Mo pre-alloyed powder with a particle size of 80μm to 120μm and a loose packing density of 4.0g / cm³ is selected. 3 The fluidity is 15s / 50g, and 0.2wt% of Ti and Nb composite grain refiner elements are added; the fiber laser power is 3.5kW, the annular spot diameter is 1.5mm, the scanning rate is 40m / min, the overlap rate is 50%, and the spiral gradient path pitch is 0.4mm / r; the powder feeding rate is 16g / min, the powder feeding gas pressure is 0.4MPa, and the argon protective gas flow rate is 18L / min; the molten pool temperature is controlled at 1700±50℃, the substrate temperature is stabilized at 200±5℃, the temperature measuring point is arranged 5mm from the edge of the repair area, and the laser power is adjusted by 8% when the temperature deviation exceeds the threshold.
[0048] Step S3, online stress control: Simultaneous composite stress control is implemented 8mm behind the cladding spot. The ultrasonic rolling pressure is 1000N, the rolling head diameter is 4mm, and the matching ratio between the rolling head speed and the axle rotation speed is 1:1.3. The pulsed laser impact energy is 2.0J, the pulse width is 8ns, the spot diameter is 1.0mm, and the circumferential angle between the ultrasonic rolling head and the pulsed laser impact head is 50°. Stress monitoring is carried out throughout the process, and the surface residual stress is controlled between -450MPa and -400MPa, and the internal residual stress does not exceed 40MPa.
[0049] Step S4, precision post-processing: CNC precision grinding to shaft diameter tolerance ±0.008mm, roundness not greater than 0.004mm, roughness Ra0.6μm; flexible polishing speed 900r / min; low temperature aging treatment temperature 160℃, heating rate 8℃ / min, holding for 2.5h, and furnace cooling to room temperature.
[0050] Testing revealed that the repaired axle cladding layer in this example was free of defects such as porosity, cracks, and slag inclusions, achieving a dense metallurgical bond with the substrate. The bond strength reached 480 MPa, and the heat-affected zone thickness was 0.25 mm. The surface residual compressive stress was -420 MPa, and the internal residual stress was 35 MPa, achieving comprehensive stress optimization. The repaired axle diameter tolerance was ±0.008 mm, the roundness was no greater than 0.004 mm, and the surface roughness Ra was 0.6 μm, meeting the requirements for high-precision assembly. The cladding layer hardness ranged from 290 HV to 310 HV, and both ultrasonic and magnetic particle testing showed no defects or cracks. The full-size measured axle diameter, roundness, and coaxiality all met the requirements of the "Technical Conditions for Locomotive Axle Manufacturing".
[0051] To verify the service reliability of the repaired axle, in accordance with EN 13261 "Railway applications—Wheelsets and bogies—Axles—Product requirements" and TSI's requirements for axle fatigue type testing, a full-scale physical fatigue test was conducted on the repaired axle on a rotating bending fatigue test bench. The test parameters were: cycle base 1×10 7 The axle body fatigue stress was 420 MPa, the stress ratio R = -1, and the loading frequency ranged from 10 Hz to 50 Hz. Each group consisted of 3 specimens. A control group was also set up: 3 newly manufactured EA4T axles and 3 EA4T axles repaired with molybdenum spraying. The test results showed that all 3 newly manufactured axles passed the 1×10⁻¹⁰ test. 7 The second cycle; only one axle passed the molybdenum spray repair, the rest were in the 6×10 cycle. 6 Next to 8×10 6 The first crack appeared; this invention repaired all three axles using a 1×10... 7 The loop continues, and the load is increased to 1.2 × 10⁻⁶. 7 No cracks appeared after this repair. This demonstrates that the fatigue performance of the axle repaired using this invention is no less than that of a newly manufactured axle, and significantly superior to that of an axle repaired with molybdenum spraying.
[0052] Furthermore, in accordance with GB / T2423.22 "Environmental Testing Part 2: Test Methods Test N: Temperature Change", Test Nb (temperature cycling, single-chamber method) was used to conduct 100 high and low temperature alternating tests on the repaired axles. The temperature range was -40℃ to +120℃, the heating and cooling rate was 3℃ / min to 5℃ / min, and the high and low temperature holding time was no less than 1 hour each. The control group consisted of 3 newly manufactured EA4T axles and 3 EA4T axles repaired with molybdenum spraying. After 100 thermal cycles: all 3 newly manufactured axles showed no abnormalities; 2 of the molybdenum sprayed axles showed coating peeling and flaking; all 3 axles repaired by this invention showed no peeling, cracking, or discoloration. Metallographic examination showed no microcracks at the interface between the cladding layer and the substrate, and the microstructure was stable. It can be seen that the cladding layer of this invention showed no peeling or cracking after 100 thermal cycles from -40℃ to 120℃, and its thermal cycling stability is significantly better than that of the molybdenum spraying process, fully meeting the long-term service requirements of Harmony locomotive axles.
[0053] To verify the synergistic effect of high-speed laser cladding combined with ultrasonic rolling and pulsed laser shock for stress control, four sets of comparative experiments were set up. The substrate material was EA4T, and the laser cladding parameters were identical, differing only in the stress control method: Group A only underwent cladding without stress control; Group B only underwent ultrasonic rolling during cladding; Group C only underwent pulsed laser shock during cladding; and Group D underwent combined control of ultrasonic rolling and pulsed laser shock during cladding. The experimental results are shown in Table 1 below, which presents the results of the four sets of comparative experiments.
[0054] Table 1
[0055] As shown in the table above, regarding surface stress, ultrasonic rolling is the dominant source of surface compressive stress, contributing approximately -425 MPa, while pulsed laser shock has a limited contribution of approximately -45 MPa. The two effects are essentially additive at the surface. Regarding internal stress, ultrasonic rolling has limited ability to eliminate internal tensile stress, reducing it by only about 15 MPa, while pulsed laser shock can significantly reduce internal tensile stress by about 45 MPa. If the two were simply superimposed, the theoretical value of internal stress should be +20 MPa. However, the measured internal residual stress in group D can be stably controlled below 40 MPa, and the improvement in fatigue life far exceeds the simple summation of each individual method. This indicates that the two control methods do not have a linear superposition effect on internal stress elimination. The compressive stress field established by ultrasonic rolling on the surface has a certain shielding effect on the release of internal tensile stress, while the pulsed laser shock wave can penetrate this shielding layer. The two form a gradient combination of surface compressive stress and low internal tensile stress in the depth domain, achieving stress optimization across the entire cross-section. Regarding fatigue life, the composite control increases the fatigue life from 0.6 × 10⁻⁶. 7 The next increase is 1.2×10 7After more than one cycle, the improvement was at least 100%, far exceeding the improvement of a single control method (Group B improved by 50%, Group C by 33%), proving that the composite stress control produced a significant synergistic effect. The above comparative experiments show that ultrasonic rolling and pulsed laser shock have a synergistic effect in both the spatial domain (surface and interior) and the temporal domain (rolling followed by shock).
[0056] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A high-speed laser repair method for locomotive axles, characterized in that, include: S1. Perform damage detection on the locomotive axle, determine the damaged area and remove the fatigue layer of the damaged area. When the depth of the damaged area reaches the preset depth, perform stepped grooving treatment on the damaged defects to form a multi-level stepped groove that rises step by step from the bottom layer to the top layer. S2. Alloy powder is fed to the damaged area using a coaxial powder feeding method. The axle is clamped in a CNC rotary fixture and rotates around its own axis. The laser cladding head is fed along the axial direction of the axle, so that the circumferential rotation of the axle and the axial feed of the laser cladding head are linked to form a spiral gradient scanning path. A ring-shaped laser beam is used to perform high-speed laser cladding on the damaged area along the spiral gradient scanning path. The spiral gradient scanning path extends from the position corresponding to the deepest point of the defect in the coordinate system of the axle cylindrical surface to the edge of the repair area, and the axial feed per revolution increases along the extension direction. S3. Behind the laser cladding spot, a composite stress control of ultrasonic rolling and pulsed laser shock is performed synchronously with the high-speed laser cladding. Compressive stress is introduced on the surface of the cladding layer by ultrasonic rolling, and residual stress inside the cladding layer is reduced by pulsed laser shock.
2. The high-speed laser repair method for locomotive axles according to claim 1, characterized in that, In step S1, the number of steps N in the stepped grooving process is determined by N=ceil(D1 / 0.5), where D1 is the depth of the damage defect in mm, and ceil means rounding up; the depth of each step is 0.2mm to 0.7mm, and D1≥0.3mm.
3. The high-speed laser repair method for locomotive axles according to claim 2, characterized in that, Horizontal width W of each step surface i = max [4 x (d i + d i+1 ), 4.0 mm], where d i is the depth of the i-th step; d i+1 is the depth of the i+1-th step, and when i = N, let d N+1 = 0; the bottom of each step is transitioned to the sidewall with a circular arc surface.
4. The high-speed laser repair method for locomotive axles according to claim 1, characterized in that, In step S1, the surface of the stepped groove is activated by an atmospheric pressure dielectric barrier discharge plasma jet before cladding, and the working gas is argon. The activation process is carried out under the protection of argon atmosphere and shares the same gas source as the argon protection gas path of the high-speed laser cladding.
5. The high-speed laser repair method for locomotive axles according to claim 1, characterized in that, In step S2, the alloy powder is a Fe-based Ni-Cr-Mo pre-alloy powder, including, in mass percentage: Ni: 10.5% to 16.0%, Cr: 17.5% to 20.0%, Mo: 2.0% to 4.5%, C: ≤0.10%, Ti: 0.10% to 0.30%, Nb: 0.05% to 0.20%, and the balance being Fe and inevitable impurities; and the absolute difference between the thermal expansion coefficient of the alloy powder and the average linear expansion coefficient of the axle body is ≤1.5×10 -6 / ℃. In step S2, the alloy powder is a Fe-based Ni-Cr-Mo pre-alloy powder, including, in mass percentage: Ni: 10.5% to 16.0%, Cr: 17.5% to 20.0%, Mo: 2.0% to 4.5%, C: ≤0.10%, Ti: 0.10% to 0.30%, Nb: 0.05% to 0.20%, and the balance being Fe and inevitable impurities; and the absolute difference between the thermal expansion coefficient of the alloy powder and the average linear expansion coefficient of the axle body is ≤1.5×10 -6 / ℃.
6. The high-speed laser repair method for locomotive axles according to claim 1, characterized in that, The scanning rate of the high-speed laser cladding is 30 m / min to 50 m / min, where the scanning rate is the linear velocity of the laser spot relative to the axle surface. The annular spot is a hollow annular spot with an inner diameter of 0.30 to 0.40 times the outer diameter and an outer diameter of 1.2 mm to 2.0 mm. The spiral gradient scanning path extends from the deepest point of the defect to the edge in the coordinate system of the axle cylindrical surface. The axle rotation speed n and the scanning rate V satisfy V = πD2n, where D2 is the actual diameter of the area to be repaired.
7. The high-speed laser repair method for locomotive axles according to claim 1, characterized in that, The journal diameter of the axle is 140mm to 260mm; in step S2, the cladding parameters are matched in segments according to the actual diameter of the area to be repaired, and the larger the diameter, the higher the value of the scanning rate and laser power, and the lower the value of the axial feed per revolution; the axial feed per revolution is 0.20mm / r to 0.40mm / r, and is consistent with the pitch of the spiral gradient scanning path.
8. The high-speed laser repair method for locomotive axles according to claim 1, characterized in that, In step S2, the molten pool temperature is monitored in real time and the laser power is adjusted in a closed loop to control the molten pool temperature between 1600℃ and 1800℃. At the same time, the substrate is preheated and interlayer insulation is performed to stabilize the substrate temperature between 180℃ and 250℃.
9. The high-speed laser repair method for locomotive axles according to claim 1, characterized in that, In step S3, both the ultrasonic rolling head and the pulsed laser impact head are located 5mm to 10mm behind the laser cladding spot. They are arranged at a circumferential angle of 45° to 60° in the cross section perpendicular to the axle axis. Along the axle axis, the ultrasonic rolling head is closer to the laser cladding spot than the pulsed laser impact head. During the continuous rotation of the axle, the same cladding layer area first receives surface compressive stress through the ultrasonic rolling head, and then the internal residual stress is reduced through the pulsed laser impact head.
10. The high-speed laser repair method for locomotive axles according to claim 1, characterized in that, After step S3, a precision post-processing step is also included: after CNC precision grinding of the cladding repair area, flexible polishing is performed using a nylon bristle brush containing abrasive. The flexible polishing is carried out in two steps: coarse polishing and fine polishing. The polishing pressure is provided by the centrifugal force of the brush body rotation and natural contact. Finally, a low-temperature aging treatment is performed.